A method for synthesizing ultra-pure battery-grade lithium carbonate from retired lithium batteries

By controlling impurity ion inclusions during the crystallization process through chemical purification and chelation, the problem of insufficient impurity content in battery-grade lithium carbonate prepared from recycled retired lithium batteries was solved, realizing the preparation of ultrapure battery-grade lithium carbonate, meeting the performance requirements of high-end lithium batteries and reducing costs.

CN116605893BActive Publication Date: 2024-10-29GANZHOU JIRUI NEW ENERGY TECH CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202310888227.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-19
Publication Date
2024-10-29
Estimated Expiration
2043-07-19

AI Technical Summary

Technical Problem

In existing technologies, the content of impurities such as Ni, Mn, Al, Cu, Fe, Na, K, and Ca in battery-grade lithium carbonate prepared from recycled retired lithium batteries cannot meet the performance requirements of high-end lithium batteries.

Method used

A chemical purification-chelation impurity control-controlled crystallization method was adopted. Most impurities were removed by adjusting the pH value with cement powder, impurity ions were chelated with chelating agents, and the difference between the nucleation rate and growth rate during the lithium carbonate crystallization process was controlled to reduce the crystallization rate of impurity carbonates.

Benefits of technology

Ultrapure battery-grade lithium carbonate with significantly lower levels of impurities such as Ni, Mn, Al, Cu, Fe, Na, K, and Ca than industry standards was obtained, meeting the performance requirements of high-end lithium batteries, reducing recycling costs, and improving the efficiency of the chemical purification process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116605893B_ABST
    Figure CN116605893B_ABST
Patent Text Reader

Abstract

The invention discloses a method for synthesizing ultra-pure battery-grade lithium carbonate from retired lithium batteries. The method comprises the steps of leaching, chemical purification, chelation control and controlled crystallization. By coupling chemical purification, chelation control and controlled crystallization, a method for synthesizing ultra-pure battery-grade lithium carbonate from retired lithium batteries is provided. The method removes most of the impurity ions by chemical purification. On this basis, the impurity ions are chelated by a chelating agent to achieve a significant reduction in the inclusion of impurity ions in the crystallization process. Furthermore, the difference in nucleation rate and growth rate between lithium carbonate and other impurity carbonates during crystallization of lithium carbonate is controlled to reduce the crystallization rate of the impurity carbonates, and finally ultra-pure battery-grade lithium carbonate is obtained. The problem that the impurity content in the battery-grade lithium carbonate prepared by recycling retired lithium batteries in the prior art cannot meet the requirements of high-end lithium batteries is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of retired lithium battery resource recovery, and in particular to a method for synthesizing ultra-pure battery-grade lithium carbonate from retired lithium batteries. Background Art

[0002] With the rapid development of new energy fields and energy storage system markets at home and abroad, the use of lithium batteries has also increased significantly. When the service life of lithium batteries ends, a large number of lithium batteries will be retired and urgently need to be recycled.

[0003] Retired lithium batteries contain a large amount of lithium and other metal elements with recycling value. At the same time, if the electrolyte and heavy metals in retired lithium batteries are not properly handled, they will cause harm to the natural environment. Therefore, from the perspective of recycling waste resources and environmental protection, the recycling process of retired lithium batteries is very urgent.

[0004] Currently, the main way to recycle retired lithium battery electrodes is through crushing, roasting, and then leaching to recover lithium and other raw materials. The lithium is generally re-prepared into battery-grade lithium carbonate that meets the industry standard "YST582-2013 Battery-grade lithium carbonate", and then continued to be used in the manufacture of lithium batteries.

[0005] However, the inventors of this application found that the above technology has at least the following technical problems in the process of implementing the technical solution of the invention in the embodiment of this application:

[0006] With the development and progress of the times and technology, the requirements for the performance of lithium batteries used are becoming more and more stringent. In addition, impurities such as Ni, Mn, Al, Cu, Fe, Na, K, and Ca have the characteristics of degrading the coulombic efficiency, cycle life, high and low temperature performance, calendar life and other performance of lithium batteries. Therefore, the content of impurities such as Ni, Mn, Al, Cu, Fe, Na, K, and Ca contained in the battery-grade lithium carbonate prepared by the traditional process method to recycle retired lithium batteries and meet the industry standard "YST582-2013 Battery-grade lithium carbonate" cannot meet the performance requirements of current high-end lithium batteries for battery-grade lithium carbonate. For this reason, it is very necessary to design and develop a method for synthesizing ultra-pure battery-grade lithium carbonate from retired lithium batteries. Summary of the invention

[0007] The embodiments of the present application provide a method for synthesizing ultra-pure battery-grade lithium carbonate from retired lithium batteries, thereby solving the problem in the prior art that the impurity content of battery-grade lithium carbonate prepared by recycling retired lithium batteries cannot meet the requirements of high-end lithium batteries. Ultra-pure battery-grade lithium carbonate with impurity contents such as Ni, Mn, Al, Cu, Fe, Na, K, and Ca significantly lower than the industry standard requirements is prepared using retired lithium batteries.

[0008] The present application provides a method for synthesizing ultrapure battery-grade lithium carbonate from retired lithium batteries, comprising the following steps:

[0009] 1) Leaching: Retired lithium batteries are crushed to obtain battery powder, which is then leached and enriched with acid to obtain a lithium solution containing impurities;

[0010] 2) Chemical purification: The impurities in the lithium solution are removed by a mixed solid of cement powder and sodium carbonate to obtain purified lithium solution after removing most of the impurities;

[0011] 3) Chelation control: Add a chelating agent that chelates Ni, Mn, Al, Cu, Fe, and Ca to the purified lithium solution to obtain a chelated lithium solution; reduce the inclusion of impurity metal ions during the crystallization of lithium carbonate through chelation;

[0012] 4) Controlled crystallization: wet lithium carbonate is obtained by controlling the directional crystallization of the chelated lithium solution. The wet lithium carbonate is washed and dried to obtain ultra-pure battery-grade lithium carbonate.

[0013] The chelating agent includes one or more of acetylacetone, salicylic acid and its sodium salt / ammonium salt, sulfosalicylic acid and its sodium salt / ammonium salt.

[0014] The controlled directional crystallization is to first subject the chelated lithium solution and the sodium carbonate solution to direct precipitation of crystal nuclei respectively, and then subject them to co-precipitation crystal growth to obtain ultra-pure battery-grade lithium carbonate.

[0015] Wherein, the crushing, acid leaching and enrichment methods described in step 1) are not particularly limited.

[0016] As some embodiments of the present application, in step 1) leaching, the lithium concentration in the impure lithium solution obtained after the retired batteries are crushed, leached and enriched is 15 g / L to 25 g / L.

[0017] As some embodiments of the present application, the chemical purification described in step 2) is to first heat the impure lithium solution to 30°C to 60°C, and then adjust the pH of the impure lithium solution to 8 to 12 by a mixture of cement powder and sodium carbonate, at which time, hydroxides and carbonate precipitates of Ni, Mn, Al, Cu, Fe, and Ca are formed, and the purified lithium solution is obtained after separating the metal slag;

[0018] Among them, the mass ratio of cement compound powder to sodium carbonate is 1:1. Cement compound powder refers to a mixture of cement and limestone, wherein the mass ratio of cement to limestone in cement compound powder is 1:3 to 1:10; cement compound powder is often used as a building material, and the cement composition is generally 3CaO·SiO2 (about 50%), 2CaO·SiO2 (about 20%), 2CaO·Al2O3 (about 15%), 4CaO·Al2O3·Fe2O3 (about 15%), and the main component of limestone is CaCO3, which has high cost performance, and is alkaline, not easy to produce colloidal precipitation, and has excellent slag-making performance. It can simultaneously achieve the functions of adjusting the pH of lithium solution containing impurities and quickly separating precipitation. Its action process is: cement undergoes hydration reaction when it meets water, that is:

[0019] 3CaO·SiO2+n H2O→xCaO·SiO2·yH2O+(3-x)Ca(OH)2

[0020] 2CaO·SiO2+n H2O→xCaO·SiO2·yH2O+(3-x)Ca(OH)2

[0021] 2CaO·Al2O3+n H2O→xCaO·Al2O3·yH2O+(3-x)Ca(OH)2

[0022] 4CaO·Al2O3·Fe2O3+n H2O→xCaO·Al2O3·Fe2O3·yH2O+(3-x)Ca(OH)2

[0023] The continuously generated Ca(OH)2, which is slightly soluble in water, consumes the H in the lithium-containing solution. + , continuously increasing the pH value, while generating OH - It reacts with Ni, Mn, Al, Cu, Fe, Ca and other ions to form hydroxide precipitates. Calcium carbonate, as a strong base and weak acid salt, continuously hydrolyzes to produce OH in water. - , and can also react with Ni, Mn, Al, Cu, Fe, Ca and other ions to form hydroxide precipitates.

[0024] Cement solidifies quickly when it comes into contact with water, causing the generated metal precipitation to form slag with larger particle size, avoiding the formation of colloidal precipitation and achieving rapid separation of precipitated materials.

[0025] It should be noted that during the pH adjustment process, cement powder reacts with acid to produce a small amount of soluble Ca impurities. In the present invention, the Ca impurities introduced by cement powder are removed in the form of calcium carbonate by using sodium carbonate solid.

[0026] As some embodiments of the present application, the amount of the chelating agent added in step 3) is 2 to 3 times the total molar amount of the impurity metal.

[0027] As some embodiments of the present application, the direct precipitation in step 4) refers to adding the sodium carbonate solution into the chelated lithium solution, and the co-precipitation refers to adding the chelated lithium solution and the sodium carbonate solution into the crystallization kettle in parallel.

[0028] As preferred in some embodiments of the present application, the concentration of the sodium carbonate solution in step 4) is 150 g / L to 250 g / L.

[0029] As some embodiments of the present application, the chelated lithium solution and the sodium carbonate solution are heated to 90°C~95°C and 80°C~90°C respectively before normal precipitation, the chelated lithium solution is pumped to 1 / 5 of the volume of the crystallization kettle, stirring is started, the stirring line speed is 5m / s~15m / s, and the sodium carbonate solution is added to the chelated lithium solution at an initial feed rate of 6L / h, and the rate is decreased at 0.4L / h~0.8L / h until the sodium carbonate addition rate reaches 4L / h, and the normal precipitation crystal nucleation stage is completed.

[0030] As some embodiments of the present application, during co-precipitation, the addition rates of the sodium carbonate solution and the chelated lithium solution are 3 L / h and 4 L / h respectively, and the reaction is carried out for 2 h to 5 h.

[0031] There are no particular limitations on the washing and drying of the wet lithium carbonate.

[0032] One or more technical solutions provided in the embodiments of the present application have at least the following technical effects or advantages:

[0033] By coupling chemical purification-chelation control-controlled crystallization, a method for synthesizing ultra-pure battery-grade lithium carbonate from retired lithium batteries is provided. The method removes most of the impurity ions through chemical purification. On this basis, the impurity ion inclusion in the crystallization process is greatly reduced by chelating the impurity ions through chelating agents. Furthermore, by controlling the difference in nucleation rate and growth rate of lithium carbonate and other impurity carbonates during the crystallization of lithium carbonate, the crystallization rate of impurity carbonates is reduced, and ultra-pure battery-grade lithium carbonate is finally obtained. The problem that the impurity content in the battery-grade lithium carbonate prepared by recycling retired lithium batteries in the prior art cannot meet the requirements of high-end lithium batteries is solved.

[0034] The cement compound powder used in the chemical purification process is cost-effective. It is alkaline, not prone to colloidal precipitation, and has excellent slag-making performance. It can simultaneously adjust the pH of the solution and quickly separate the precipitation, thereby reducing the cost of recycling retired lithium batteries and increasing the efficiency of the chemical purification process. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 The process flow chart of an embodiment of the present invention. DETAILED DESCRIPTION

[0036] The embodiment of the present application provides a method of coupled chemical purification-chelation control-controlled crystallization to solve the problem that the impurity content of battery-grade lithium carbonate prepared by recycling retired lithium batteries in the prior art cannot meet the requirements of high-end lithium batteries. The technical solution in the embodiment of the present application is to solve the problem of high impurity content, and the overall idea is as follows:

[0037] First, most of the impurity ions are removed through chemical purification. On this basis, the impurity ions are chelated by chelating agents to greatly reduce the inclusion of impurity ions in the crystallization process. Furthermore, by controlling the difference in nucleation rate and growth rate of lithium carbonate and other impurity carbonates during the crystallization process of lithium carbonate, the crystallization rate of impurity carbonates is reduced to obtain ultra-pure battery-grade lithium carbonate.

[0038] In order to better understand the above technical solution, the above technical solution will be described in detail below in conjunction with the accompanying drawings and specific implementation methods.

[0039] First embodiment:

[0040] like Figure 1 As shown, this embodiment is a method for synthesizing ultra-pure battery-grade lithium carbonate from retired lithium batteries, and the steps are as follows:

[0041] 1) Leaching: Retired lithium batteries are crushed to obtain battery powder, and the battery powder is leached and enriched by acid to obtain an impure lithium solution with a lithium concentration of 20 g / L; detected by ICP-OES of model PerkinElmer AVIO 200, the content of impurity elements is: Ni 0.45 g / L, Mn 0.23 g / L, Al 0.53 g / L, Cu 0.15 g / L, Fe 0.14 g / L, Na 7.57 g / L, K0.25 g / L, Ca 0.12 g / L.

[0042] 2) Chemical purification: first heat the impure lithium solution to 60°C, add a mixture of cement compound powder and sodium carbonate with a mass ratio of cement: limestone: sodium carbonate of 1:4:5 to the impure lithium solution, adjust the pH of the impure lithium solution to 10, separate the metal slag to obtain a preliminary impurity-removed lithium solution.

[0043] 3) Chelation control: Add acetylacetone, a chelating agent that chelates Ni, Mn, Al, Cu, Fe, and Ca, to the purified lithium solution. The amount of the chelating agent added is 3 times the total molar amount of the impurity metal to obtain a chelated lithium solution. The chelation effect significantly reduces the inclusion of impurity metal ions during the crystallization of lithium carbonate.

[0044] 4) Controlled crystallization: First, heat the sodium carbonate solution with a concentration of 200 g / L to 90°C and the chelated lithium solution with a lithium element concentration of 20 g / L to 95°C.

[0045] Next, the crystal nucleation was carried out, and the hot chelated lithium solution was pumped to 1 / 5 of the volume of the crystallization kettle, and stirring was started with a stirring linear speed of 8 m / s. Sodium carbonate solution was added to the chelated lithium solution at an initial feed rate of 6 L / h, and then decreased at a rate of 0.5 L / h until the sodium carbonate addition rate reached 4 L / h.

[0046] After the nucleation of the positive crystal is completed, co-precipitation crystal growth is carried out. The hot sodium carbonate solution and the chelated lithium solution are added to the reactor in parallel at a feed rate of 3L / h and 4L / h respectively. The reaction is carried out for 4 hours to obtain wet lithium carbonate. The wet lithium carbonate is washed and dried to obtain ultra-pure battery-grade lithium carbonate.

[0047] The elemental composition content of the ultrapure battery-grade lithium carbonate obtained in this example is shown in Table 1.

[0048] Second embodiment:

[0049] like Figure 1 As shown, this embodiment is a method for synthesizing ultra-pure battery-grade lithium carbonate from retired lithium batteries, and the steps are as follows:

[0050] 1) Leaching: Retired lithium batteries are crushed to obtain battery powder, and the battery powder is leached and enriched by acid to obtain an impure lithium solution with a lithium concentration of 15 g / L; detected by ICP-OES of model PerkinElmer AVIO 200, the content of impurity elements is: Ni 0.42 g / L, Mn 0.23 g / L, Al 0.52 g / L, Cu 0.13 g / L, Fe 0.12 g / L, Na 7.52 g / L, K 0.24 g / L, Ca 0.12 g / L.

[0051] 2) Chemical purification: first heat the impure lithium solution to 60°C, add a mixture of cement compound powder and sodium carbonate with a mass ratio of cement: limestone: sodium carbonate of 1:10:11 to the impure lithium solution, adjust the pH of the impure lithium solution to 8, and separate the metal slag to obtain purified lithium solution.

[0052] 3) Chelation control: Add acetylacetone, a chelating agent that chelates Ni, Mn, Al, Cu, Fe, and Ca, to the purified lithium solution. The amount of the chelating agent added is 3 times the total molar amount of the impurity metal to obtain a chelated lithium solution. The chelation effect significantly reduces the inclusion of impurity metal ions during the crystallization of lithium carbonate.

[0053] 4) Controlled crystallization: First, heat the sodium carbonate solution with a concentration of 250 g / L to 80°C and the chelated lithium solution with a lithium concentration of 15 g / L to 90°C.

[0054] Next, the crystal nucleation was carried out, and the hot chelated lithium solution was pumped to 1 / 5 of the volume of the crystallization kettle, and stirring was started with a stirring linear speed of 5 m / s. Sodium carbonate solution was added to the chelated lithium solution at an initial feed rate of 6 L / h, and then decreased at a rate of 0.8 L / h until the sodium carbonate addition rate reached 4 L / h.

[0055] After the nucleation of the positive crystal is completed, co-precipitation crystal growth is carried out. The hot sodium carbonate solution and the chelated lithium solution are added to the reactor in parallel at a feed rate of 3L / h and 4L / h, respectively. The reaction is carried out for 5 hours to obtain wet lithium carbonate. The wet lithium carbonate is washed and dried to obtain ultra-pure battery-grade lithium carbonate.

[0056] The elemental composition content of the ultrapure battery-grade lithium carbonate obtained in this example is shown in Table 1.

[0057] Third embodiment:

[0058] like Figure 1 As shown, this embodiment is a method for synthesizing ultra-pure battery-grade lithium carbonate from retired lithium batteries, and the steps are as follows:

[0059] 1) Leaching: Retired lithium batteries are crushed to obtain battery powder, and the battery powder is leached and enriched by acid to obtain an impure lithium solution with a lithium concentration of 20 g / L; detected by ICP-OES of model PerkinElmer AVIO 200, the content of impurity elements is: Ni 0.47 g / L, Mn 0.24 g / L, Al 0.54 g / L, Cu 0.16 g / L, Fe 0.13 g / L, Na 7.57 g / L, K 0.23 g / L, Ca 0.13 g / L.

[0060] 2) Chemical purification: first heat the impure lithium solution to 60°C, add a mixture of cement compound powder and sodium carbonate with a mass ratio of cement: limestone: sodium carbonate of 1:6:7 to the impure lithium solution, adjust the pH of the impure lithium solution to 10, separate the metal slag to obtain purified lithium solution.

[0061] 3) Chelation control: Add chelating agent ammonium sulfosalicylate, which has chelating effect on Ni, Mn, Al, Cu, Fe and Ca, to the purified lithium solution. The amount of chelating agent added is 3 times the total molar amount of impurity metal to obtain chelated lithium solution. The inclusion of impurity metal ions in the crystallization process of lithium carbonate is significantly reduced through chelation.

[0062] 4) Controlled crystallization: First, heat the sodium carbonate solution with a concentration of 200 g / L to 90°C and the chelated lithium solution with a lithium element concentration of 20 g / L to 95°C.

[0063] Next, the crystal nucleation was carried out, and the hot chelated lithium solution was pumped to 1 / 5 of the volume of the crystallization kettle, and stirring was started with a stirring linear speed of 8 m / s. Sodium carbonate solution was added to the chelated lithium solution at an initial feed rate of 6 L / h, and then decreased at a rate of 0.5 L / h until the sodium carbonate addition rate reached 4 L / h.

[0064] After the nucleation of the positive crystal is completed, co-precipitation crystal growth is carried out. The hot sodium carbonate solution and the chelated lithium solution are added to the reactor in parallel at a feed rate of 3L / h and 4L / h respectively. The reaction is carried out for 4 hours to obtain wet lithium carbonate. The wet lithium carbonate is washed and dried to obtain ultra-pure battery-grade lithium carbonate.

[0065] The elemental composition content of the ultrapure battery-grade lithium carbonate obtained in this example is shown in Table 1.

[0066] Fourth embodiment:

[0067] like Figure 1 As shown, this embodiment is a method for synthesizing ultra-pure battery-grade lithium carbonate from retired lithium batteries, and the steps are as follows:

[0068] 1) Leaching: Retired lithium batteries are crushed to obtain battery powder, and the battery powder is leached and enriched by acid to obtain an impure lithium solution with a lithium concentration of 22 g / L; detected by ICP-OES of model PerkinElmer AVIO 200, the content of impurity elements is: Ni 0.44 g / L, Mn 0.26 g / L, Al 0.57 g / L, Cu 0.17 g / L, Fe 0.15 g / L, Na 7.16 g / L, K 0.25 g / L, Ca 0.13 g / L.

[0069] 2) Chemical purification: first heat the impure lithium solution to 60°C, add a mixture of cement compound powder and sodium carbonate with a mass ratio of cement: limestone: sodium carbonate of 1:8:9 to the impure lithium solution, adjust the pH of the impure lithium solution to 10, separate the metal slag to obtain purified lithium solution.

[0070] 3) Chelation control: Add chelating agent ammonium sulfosalicylate, which has chelating effect on Ni, Mn, Al, Cu, Fe and Ca, to the purified lithium solution. The amount of chelating agent added is 3 times the total molar amount of impurity metal to obtain chelated lithium solution. The inclusion of impurity metal ions in the crystallization process of lithium carbonate is significantly reduced through chelation.

[0071] 4) Controlled crystallization: First, heat the sodium carbonate solution with a concentration of 200 g / L to 90°C and the chelated lithium solution with a lithium concentration of 22 g / L to 95°C.

[0072] Next, the crystal nucleation was carried out, and the hot chelated lithium solution was pumped to 1 / 5 of the volume of the crystallization kettle, and stirring was started with a stirring linear speed of 9 m / s. Sodium carbonate solution was added to the chelated lithium solution at an initial feed rate of 6 L / h, and then decreased at a rate of 0.4 L / h until the sodium carbonate addition rate reached 4 L / h.

[0073] After the nucleation of the positive crystal is completed, co-precipitation crystal growth is carried out. The hot sodium carbonate solution and the chelated lithium solution are added to the reactor in parallel at a feed rate of 3L / h and 4L / h, respectively. The reaction is carried out for 5 hours to obtain wet lithium carbonate. The wet lithium carbonate is washed and dried to obtain ultra-pure battery-grade lithium carbonate.

[0074] The elemental composition content of the ultrapure battery-grade lithium carbonate obtained in this example is shown in Table 1.

[0075] Fifth embodiment:

[0076] like Figure 1 As shown, this embodiment is a method for synthesizing ultra-pure battery-grade lithium carbonate from retired lithium batteries, and the steps are as follows:

[0077] 1) Leaching: Retired lithium batteries are crushed to obtain battery powder, and the battery powder is leached and enriched by acid to obtain an impure lithium solution with a lithium concentration of 18 g / L; detected by ICP-OES of model PerkinElmer AVIO 200, the content of impurity elements is: Ni 0.49 g / L, Mn 0.26 g / L, Al 0.58 g / L, Cu 0.19 g / L, Fe 0.17 g / L, Na 7.53 g / L, K 0.24 g / L, Ca 0.16 g / L.

[0078] 2) Chemical purification: first heat the impure lithium solution to 60°C, add a mixture of cement compound powder and sodium carbonate with a mass ratio of cement: limestone: sodium carbonate of 1:7:8 to the impure lithium solution, adjust the pH of the impure lithium solution to 9, separate the metal slag to obtain purified lithium solution.

[0079] 3) Chelation control: Add sodium salicylate, a chelating agent that chelates Ni, Mn, Al, Cu, Fe, and Ca, to the purified lithium solution. The amount of chelating agent added is twice the total molar amount of the impurity metal to obtain a chelated lithium solution. The chelation effect significantly reduces the inclusion of impurity metal ions during the crystallization of lithium carbonate.

[0080] 4) Controlled crystallization: First, heat the sodium carbonate solution with a concentration of 220 g / L to 90°C and the chelated lithium solution with a lithium element concentration of 18 g / L to 90°C.

[0081] Next, the crystal nucleation was carried out, and the hot chelated lithium solution was pumped to 1 / 5 of the volume of the crystallization kettle, and stirring was started with a stirring linear speed of 8 m / s. Sodium carbonate solution was added to the chelated lithium solution at an initial feed rate of 6 L / h, and then decreased at a rate of 0.6 L / h until the sodium carbonate addition rate reached 4 L / h.

[0082] After the nucleation of the positive crystal is completed, co-precipitation crystal growth is carried out. The hot sodium carbonate solution and the chelated lithium solution are added to the reactor in parallel at a feed rate of 3L / h and 4L / h respectively. The reaction is carried out for 4 hours to obtain wet lithium carbonate. The wet lithium carbonate is washed and dried to obtain ultra-pure battery-grade lithium carbonate.

[0083] The elemental composition content of the ultrapure battery-grade lithium carbonate obtained in this example is shown in Table 1.

[0084] The first comparison:

[0085] This comparative example is based on Example 5, and the addition of the chelating agent in the chelating step is reduced, and the steps are as follows:

[0086] 1) Leaching: Retired lithium batteries are crushed to obtain battery powder, and the battery powder is leached and enriched by acid to obtain an impure lithium solution with a lithium concentration of 18 g / L; detected by ICP-OES of model PerkinElmer AVIO 200, the content of impurity elements is: Ni 0.49 g / L, Mn 0.26 g / L, Al 0.58 g / L, Cu 0.19 g / L, Fe 0.17 g / L, Na 7.53 g / L, K 0.24 g / L, Ca 0.16 g / L.

[0087] 2) Chemical purification: first heat the impure lithium solution to 60°C, add a mixture of cement compound powder and sodium carbonate with a mass ratio of cement: limestone: sodium carbonate of 1:7:8 to the impure lithium solution, adjust the pH of the impure lithium solution to 9, separate the metal slag to obtain purified lithium solution.

[0088] 3) Controlled crystallization: First, heat the sodium carbonate solution with a concentration of 220 g / L to 90°C and the purified lithium solution with a lithium element concentration of 18 g / L to 90°C.

[0089] Next, the crystal nucleation was carried out, and the hot purified lithium solution was pumped to 1 / 5 of the volume of the crystallization kettle, and stirring was started with a stirring linear speed of 8 m / s. Sodium carbonate solution was added to the purified lithium solution at an initial feed rate of 6 L / h, and then decreased at a rate of 0.6 L / h until the sodium carbonate addition rate reached 4 L / h.

[0090] After the nucleation of the positive crystal is completed, co-precipitation crystal growth is carried out. The hot sodium carbonate solution and the purified lithium solution are added to the reactor in parallel at a feed rate of 3L / h and 4L / h, respectively. The reaction is carried out for 4 hours to obtain wet lithium carbonate, which is washed and dried to obtain lithium carbonate.

[0091] The elemental composition content of lithium carbonate obtained in this comparative example is shown in Table 1.

[0092] Second comparison:

[0093] This comparative example is based on Example 5, except that the cement powder in the chemical purification step is replaced by caustic soda flakes, and the steps are as follows:

[0094] 1) Leaching: Retired lithium batteries are crushed to obtain battery powder, and the battery powder is leached and enriched by acid to obtain an impure lithium solution with a lithium concentration of 18 g / L; detected by ICP-OES of model PerkinElmer AVIO 200, the content of impurity elements is: Ni 0.49 g / L, Mn 0.26 g / L, Al 0.58 g / L, Cu 0.19 g / L, Fe 0.17 g / L, Na 7.53 g / L, K 0.24 g / L, Ca 0.16 g / L.

[0095] 2) Chemical purification: first heat the impure lithium solution to 60°C, add caustic soda flakes to the impure lithium solution, adjust the pH of the impure lithium solution to 9, separate the metal slag to obtain purified lithium solution.

[0096] 3) Chelation control: Add sodium salicylate, a chelating agent that chelates Ni, Mn, Al, Cu, Fe, and Ca, to the purified lithium solution. The amount of chelating agent added is twice the total molar amount of the impurity metal to obtain a chelated lithium solution. The chelation effect significantly reduces the inclusion of impurity metal ions during the crystallization of lithium carbonate.

[0097] 4) Controlled crystallization: First, heat the sodium carbonate solution with a concentration of 220 g / L to 90°C and the chelated lithium solution with a lithium element concentration of 18 g / L to 90°C.

[0098] Next, the crystal nucleation was carried out, and the hot chelated lithium solution was pumped to 1 / 5 of the volume of the crystallization kettle, and stirring was started with a stirring linear speed of 8 m / s. Sodium carbonate solution was added to the chelated lithium solution at an initial feed rate of 6 L / h, and then decreased at a rate of 0.6 L / h until the sodium carbonate addition rate reached 4 L / h.

[0099] After the nucleation of the normal precipitated crystals is completed, co-precipitated crystal growth is carried out. The hot sodium carbonate solution and the chelated lithium solution are added to the reactor in parallel at feed rates of 3L / h and 4L / h, respectively. The reaction is carried out for 4 hours to obtain wet lithium carbonate, which is then washed and dried to obtain lithium carbonate.

[0100] The elemental composition content of lithium carbonate obtained in this comparative example is shown in Table 1.

[0101] The third comparison ratio:

[0102] This comparative example is based on Example 5, in which the crystallization step is not divided into two stages: the normal precipitation crystal nucleation and the co-precipitation crystal growth, and the crystallization is directly carried out, and the steps are as follows:

[0103] 1) Leaching: Retired lithium batteries are crushed to obtain battery powder, and the battery powder is leached and enriched by acid to obtain an impure lithium solution with a lithium concentration of 18 g / L; detected by ICP-OES of model PerkinElmer AVIO 200, the content of impurity elements is: Ni 0.49 g / L, Mn 0.26 g / L, Al 0.58 g / L, Cu 0.19 g / L, Fe 0.17 g / L, Na 7.53 g / L, K 0.24 g / L, Ca 0.16 g / L.

[0104] 2) Chemical purification: first heat the impure lithium solution to 60°C, add a mixture of cement compound powder and sodium carbonate with a mass ratio of cement: limestone: sodium carbonate of 1:7:8 to the impure lithium solution, adjust the pH of the impure lithium solution to 9, separate the metal slag to obtain purified lithium solution.

[0105] 3) Chelation control: Add sodium salicylate, a chelating agent that has a chelating effect on Ni, Mn, Al, Cu, Fe, and Ca, to the purified lithium solution. The amount of the chelating agent added is twice the total molar amount of the impurity metals to obtain a chelated lithium solution.

[0106] 4) Crystallization: First, heat the sodium carbonate solution with a concentration of 220g / L to 90°C and the chelated lithium solution with a lithium concentration of 18g / L to 90°C.

[0107] Next, crystallization is performed, and the hot chelated lithium solution is pumped to 1 / 5 of the volume of the crystallization kettle, and stirring is started, and the stirring linear speed is 8 m / s. The hot sodium carbonate solution and the chelated lithium solution are added to the reactor in a parallel flow manner at a feed rate of 3 L / h and 4 L / h, respectively, and the reaction is carried out for 4 hours to obtain wet lithium carbonate, which is washed and dried to obtain lithium carbonate.

[0108] The element content of lithium carbonate obtained in this comparative example is shown in Table 1 after detection by ICP-OES of model PerkinElmer AVIO 200.

[0109] The elemental composition of the lithium carbonate synthesized by the first to fifth embodiments and the first to third comparative examples is shown in Table 1.

[0110] Table 1 Element content

[0111] Ni Mn Al Cu Fe K Ca Na Industry Standards ≤0.001% ≤0.0003% ≤0.001% ≤0.0003% ≤0.001% ≤0.001% ≤0.0003% ≤0.025% First embodiment 0.00025% 0.00005% 0.000063% 0.00006% 0.00076% 0.00009% 0.00019% 0.0085% Second embodiment 0.00035% 0.00009% 0.000072% 0.00008% 0.00083% 0.00015% 0.00025% 0.0091% Third embodiment 0.00018% 0.00007% 0.000056% 0.00004% 0.00081% 0.00007% 0.00021% 0.0083% Fourth embodiment 0.00012% 0.00008% 0.000051% 0.00002% 0.00073% 0.00008% 0.00017% 0.0078% Fifth embodiment 0.00001% 0.00001% 0.000048% 0.00001% 0.00067% 0.00001% 0.00017% 0.0075% The first comparison 0.0015% 0.00032% 0.0013% 0.00036% 0.0012% 0.0015% 0.00032% 0.029% The second comparison 0.0019% 0.00034% 0.0016% 0.00042% 0.0016% 0.0018% 0.00035% 0.026% The third comparison 0.0012% 0.00031% 0.0011% 0.00032% 0.0011% 0.0013% 0.00031% 0.027%

[0112] As can be seen from Table 1, the impurity content of lithium carbonate synthesized by the method of the present application is significantly lower than the requirements of the industry standard "YST582-2013 Battery Grade Lithium Carbonate", and can meet the needs of high-end lithium battery preparation.

[0113] Although the preferred embodiments of the present invention have been described, those skilled in the art may make other changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.

[0114] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. A method for synthesizing ultrapure battery-grade lithium carbonate from retired lithium batteries, characterized in that: The steps include: 1) Leaching: Retired lithium batteries are crushed to obtain battery powder, which is then leached and enriched with acid to obtain a lithium solution containing impurities; 2) Chemical purification: The impurity-containing lithium solution is purified by a mixed solid of cement powder and sodium carbonate to obtain purified lithium liquid after removing most of the impurities; the cement powder is a mixture of cement and limestone; 3) Chelating and controlling impurities: adding a chelating agent having a chelating effect on Ni, Mn, Al, Cu, Fe and Ca to the purified lithium solution to obtain a chelated lithium solution; the chelating agent includes one or more of acetylacetone, salicylic acid and its sodium salt / ammonium salt, sulfosalicylic acid and its sodium salt / ammonium salt; 4) Controlled crystallization: wet lithium carbonate is obtained by controlling the directional crystallization of the chelated lithium solution, and the wet lithium carbonate is washed and dried to obtain ultra-pure battery-grade lithium carbonate; the controlled directional crystallization is to first subject the chelated lithium solution and the sodium carbonate solution to normal precipitation crystal nucleation, and then co-precipitate crystal growth to obtain ultra-pure battery-grade lithium carbonate; Step 4) The direct precipitation refers to adding the sodium carbonate solution into the chelated lithium solution, and the co-precipitation refers to adding the chelated lithium solution and the sodium carbonate solution into the crystallization kettle in parallel.

2. The method for synthesizing ultrapure battery-grade lithium carbonate from retired lithium batteries according to claim 1, characterized in that: In step 1) leaching, the retired batteries are crushed, acid-leached, and enriched to obtain an impure lithium solution with a lithium concentration of 15 g / L to 25 g / L.

3. The method for synthesizing ultrapure battery-grade lithium carbonate from retired lithium batteries according to claim 1, characterized in that: The chemical purification in step 2) is to first heat the lithium solution containing impurities to 30°C to 60°C, and then adjust the pH of the lithium solution containing impurities to 8 to 12 using a mixed solid of cement powder and sodium carbonate.

4. The method for synthesizing ultrapure battery-grade lithium carbonate from retired lithium batteries according to claim 1, characterized in that: The mass ratio of the cement compound powder to the sodium carbonate solid is 1:1, and the mass ratio of cement to limestone in the cement compound powder is 1:3-1:

10.

5. The method for synthesizing ultrapure battery-grade lithium carbonate from retired lithium batteries according to claim 1, characterized in that: The amount of the chelating agent added in step 3) is 2 to 3 times the total molar amount of the impurity metal.

6. The method for synthesizing ultrapure battery-grade lithium carbonate from retired lithium batteries according to claim 1, characterized in that: In step 4), the concentration of the sodium carbonate solution is 150 g / L to 250 g / L.

7. The method for synthesizing ultrapure battery-grade lithium carbonate from retired lithium batteries according to claim 1, characterized in that: Before precipitation, the chelated lithium solution and the sodium carbonate solution are heated to 90°C to 95°C and 80°C to 90°C respectively.

8. The method for synthesizing ultrapure battery-grade lithium carbonate from retired lithium batteries according to claim 7, characterized in that: After the heating of the chelated lithium solution and the sodium carbonate solution is completed, the chelated lithium solution is pumped to 1 / 5 of the volume of the crystallization kettle, stirring is started, the stirring linear speed is 5m / s~15m / s, and the sodium carbonate solution is added to the chelated lithium solution at an initial feed rate of 6L / h, and the rate is decreased at 0.4L / h~0.8L / h until the sodium carbonate addition rate reaches 4L / h, and the nucleation stage of the positive precipitation crystal is completed.

9. The method for synthesizing ultrapure battery-grade lithium carbonate from retired lithium batteries according to claim 1, characterized in that: During co-precipitation, the addition rates of sodium carbonate solution and chelated lithium solution are 3 L / h and 4 L / h respectively, and the reaction takes 2h to 5h.

Citation Information

Patent Citations

  • Method for recovering lithium from lithium iron phosphate waste materials for preparing cell-level lithium carbonate