A high-selectivity and high-stability carbon dioxide to methanol catalyst and preparation method thereof
By using a combination of copper-based metal oxide and silica coating in the carbon dioxide hydrogenation catalyst, the problem of catalyst deactivation under long-term reaction conditions is solved, high selectivity and stability are achieved, and carbon dioxide conversion is improved. rate and methanol selectivity, suitable for industrial applications.
Patent Information
- Application Number
- CN202210139341.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-02-15
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-02-15
Smart Images

Figure CN116637624B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of hydrogenation catalysts, and in particular to a high-selectivity and high-stability carbon dioxide to methanol catalyst and a preparation method thereof. Background Art
[0002] In the context of vigorously developing renewable energy such as solar energy and wind energy, we use renewable energy to generate electricity and electrolyze water to produce hydrogen, namely "green hydrogen", and convert carbon dioxide into basic chemical methanol by hydrogenation. Methanol is an important basic chemical raw material that can be used as an alternative fuel. It can also be used to synthesize dimethyl ether, olefins, aromatics, acetic acid, esters and other chemicals. At present, my country's methanol production mainly adopts the coal chemical route, that is, coal-based synthesis gas is used as raw material to directly synthesize methanol. There are three main catalyst systems reported for the catalytic hydrogenation of carbon dioxide to methanol: Cu-based catalysts, In-based catalysts and metal oxide catalysts.
[0003] Cu-based catalysts, such as Cu / ZnO, Cu / ZrO2, Cu / ZnO / Al2O3, etc., have good catalytic conversion activity for carbon dioxide and are considered to be the catalysts with the most promising industrial applications. However, Cu-based catalysts are prone to sintering and oxidation in the reaction atmosphere, which can lead to catalyst deactivation. In addition, the selectivity of by-products such as CO and alkanes is relatively high. In-based catalysts are mainly divided into two categories: supported and bulk catalysts, such as In2O3-Pd, In2O3-ZrO2, etc. The oxygen vacancies in In2O3 can effectively activate carbon dioxide and inhibit the formation of carbon monoxide while generating methanol. However, the active components of this type of catalyst are easily lost and deactivated at high temperatures, and In is expensive, making it unsuitable for large-scale applications. Metal oxide catalysts, such as ZnZrO X 、GaZrO X The strong synergistic effect of the two metal components enhances the heterolytic dissociation of H2, resulting in high activity and high methanol selectivity. This type of catalyst has a low conversion rate at low temperatures and requires a certain activity at higher temperatures, but it is easy to generate CO by-products at high temperatures, affecting carbon utilization efficiency.
[0004] In summary, the current methanol catalyst is mainly based on Cu-based catalysts, but under long-term reaction conditions, Cu-based catalysts are prone to sintering and deactivation, which makes it difficult to simultaneously improve their catalytic performance, especially carbon dioxide conversion rate and methanol selectivity, which will limit their industrial application. Therefore, it is of great significance to develop a carbon dioxide hydrogenation catalyst with low reverse water gas shift activity and high stability. Summary of the invention
[0005] The object of the present invention is to solve the above problems in the prior art and to provide a catalyst for producing methanol from carbon dioxide hydrogenation having low reverse water vapor shift activity and high stability and a preparation method thereof.
[0006] In order to achieve the above object, the present invention adopts the following technical scheme:
[0007] A high-selectivity and high-stability carbon dioxide to methanol catalyst comprises a copper-based metal oxide and a silicon dioxide coating layer, wherein the silicon dioxide coating layer comprises an inorganic silicon compound and an organic silane hydrophobic agent; based on the total mass of the catalyst, the mass fraction of the copper-based metal oxide is 50% to 70%, and the remainder is the silicon dioxide coating layer; in the silicon dioxide coating layer, the mass fraction of the inorganic silicon compound is 40% to 70%, and the mass fraction of the organic silane hydrophobic agent is 30% to 60%.
[0008] The inorganic silicon compound includes at least one of white carbon black, silica sol, and silicate, and the organic silane hydrophobic agent includes at least one of trimethylchlorosilane, tert-butyldimethylchlorosilane, triisopropylchlorosilane, and di-tert-butyldichlorosilane.
[0009] The copper-based metal oxide includes at least one of copper zinc, copper zinc aluminum, copper zinc zirconium, copper zinc aluminum zirconium, copper zinc yttrium, copper zinc cerium, copper gallium zirconium, copper gallium aluminum, and copper gallium cerium.
[0010] The method for preparing a high-selectivity and high-stability carbon dioxide to methanol catalyst comprises the following steps:
[0011] 1) adding copper-based metal oxide to anhydrous ethanol for dispersion, then adding inorganic silicon compound, stirring, then adding ammonia water, continuing stirring, and finally centrifugation washing to obtain a filter cake;
[0012] 2) drying and calcining the filter cake obtained in step 1) to obtain a solid sample of copper-based metal oxide coated with inorganic silicon;
[0013] 3) adding the inorganic silicon-coated copper-based metal oxide solid sample obtained in step 2) into n-hexane, stirring, then adding an organosilane hydrophobic agent, continuing to stir, and then ultrasonicating to obtain a suspension;
[0014] 4) The suspension obtained in step 3) is centrifuged, washed, dried, and reduced to obtain a catalyst for hydrogenating carbon dioxide to methanol.
[0015] In step 1), the copper-based metal oxide is prepared by a coprecipitation method, a sol-gel method or a hydrothermal method.
[0016] In step 1), the mass ratio of the anhydrous ethanol to the copper-based metal oxide is (100-200):1; the mass ratio of the ammonia water to the inorganic silicon compound is (10-20):1, and the concentration of the ammonia water is 25%-28%; in step 2), the mass ratio of the n-hexane to the inorganic silicon compound is (50-100):1.
[0017] In step 1), the stirring speed is 200-1000 r / min, the stirring temperature is 20-60° C., and the stirring time is 2-8 h; in step 3), the stirring speed is 200-1000 r / min, the stirring temperature is 20-60° C., the stirring time is 0.5-1.5 h, and the ultrasonic time is 1-4 h.
[0018] In step 2), the drying step is: drying in an oven at 100-120°C for 2-10 hours, taking out the dried solid product to cool it down, and then transferring it to a vacuum oven at 130-160°C for drying for 5-12 hours; the calcining step is: calcining at 300-600°C in an air atmosphere for 2-12 hours.
[0019] In step 4), the reduction conditions are: reduction at a temperature of 200-500° C. for 0.5-10 h in an atmosphere of H2 / N2 or H2 / Ar or pure H2 with a H2 concentration of 5%-50%.
[0020] The high-selectivity and high-stability carbon dioxide to methanol catalyst is applied to the carbon dioxide hydrogenation to methanol reaction, and the reaction conditions are: carbon dioxide hydrogenation reaction pressure 5-150 bar, reaction temperature 180-320 ° C, H2 to CO2 volume ratio 1:9-9:1, reaction gas space velocity 1000-50000 mL h -1 g -1 .
[0021] Compared with the prior art, the technical solution of the present invention has the following beneficial effects:
[0022] 1. The catalyst of the present invention shows excellent low reverse water vapor shift activity and stability for selective hydrogenation of carbon dioxide to methanol, with a carbon dioxide conversion rate of more than 18% and a methanol selectivity of more than 87%;
[0023] 2. The silicon dioxide surface coating layer added during the preparation of the catalyst of the present invention can inhibit the generated water from entering the catalyst surface and contacting the copper-based catalyst, thereby protecting the copper-based catalyst from being oxidized by the water generated during the methanol synthesis process. At the same time, it can inhibit the migration of ZnO, thereby inhibiting the generation of CO by the reverse water gas shift reaction, and significantly inhibiting the deactivation of the catalyst;
[0024] 3. The catalyst preparation process of the present invention is simple, has good repeatability, and is easy to scale up for production;
[0025] 4. The catalyst of the present invention is non-precious metal, cheap, has low industrial production cost, and has good application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 The stability evaluation results of the catalyst prepared in Example 1;
[0027] Figure 2 The stability evaluation results of the catalyst prepared in Comparative Example 2 are shown. DETAILED DESCRIPTION
[0028] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present invention clearer and more understandable, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments.
[0029] The invention discloses a high-selectivity and high-stability carbon dioxide to methanol catalyst, comprising a copper-based metal oxide and a silicon dioxide coating layer, wherein the silicon dioxide coating layer comprises an inorganic silicon compound and an organic silane hydrophobic agent; based on the total mass of the catalyst, the mass fraction of the copper-based metal oxide is 50% to 70%, and the remainder is the silicon dioxide coating layer; in the silicon dioxide coating layer, the mass fraction of the inorganic silicon compound is 40% to 70%, and the mass fraction of the organic silane hydrophobic agent is 30% to 60%.
[0030] Specifically, the inorganic silicon compound includes at least one of white carbon black, silica sol, and silicate, and the organosilane hydrophobic agent includes at least one of trimethylchlorosilane, tert-butyldimethylchlorosilane, triisopropylchlorosilane, and di-tert-butyldichlorosilane.
[0031] Specifically, the copper-based metal oxide includes at least one of copper zinc, copper zinc aluminum, copper zinc zirconium, copper zinc aluminum zirconium, copper zinc yttrium, copper zinc cerium, copper gallium zirconium, copper gallium aluminum, and copper gallium cerium, and is prepared by co-precipitation, sol-gel or hydrothermal method.
[0032] The highly selective and stable carbon dioxide to methanol catalyst of the present invention has the following specific preparation steps:
[0033] (1) taking a measured amount of copper-based metal oxide, grinding it into powder in a mortar, and sieving it through a 100-200 mesh sieve to obtain a uniform powder;
[0034] (2) Weigh the powder obtained in the above step, add it into a measured amount of anhydrous ethanol, and ultrasonicate it at 20 to 60° C. for 0.5 to 2.0 h to uniformly disperse the powder sample;
[0035] (3) adding a measured amount of an inorganic silicon compound to the mixed solution obtained in the above step (2), stirring at 200 to 1000 r / min and at 20 to 60° C. for 2 to 8 hours; then adding a measured amount of ammonia water (25 to 28%), maintaining the same speed and reaction temperature, and continuing to stir for 2 to 8 hours, and then centrifuging the mixed solution and washing with anhydrous ethanol to obtain a filter cake;
[0036] (4) The obtained filter cake was transferred to an oven at 100-120° C. and dried for 2-10 h. The dried solid product was taken out and cooled to 30° C., and then transferred to a vacuum oven at 130-160° C. and dried for 5-12 h. The solid product was cooled to 30° C. to obtain a solid sample.
[0037] (5) placing the solid sample in a muffle furnace and calcining it at 300-600° C. in an air atmosphere for 2-12 hours to obtain a copper-based metal oxide solid sample coated with inorganic silicon;
[0038] (6) adding the solid sample of the copper-based metal oxide coated with inorganic silicon to a measured amount of n-hexane, stirring at a speed of 200-1000 r / min at 20-60° C. for 0.5-1.5 h; then adding a measured amount of an organic silane hydrophobic agent, maintaining the same speed and reaction temperature, continuing to stir for 0.5-1.5 h, and ultrasonicating for 1-4 h to obtain a suspension;
[0039] (7) The suspension obtained above was centrifuged and washed with n-hexane, then transferred to a vacuum oven at 70-100° C. and dried for 5-12 h. The dried solid product was taken out and cooled to 30° C., ground into powder in a mortar, and sieved through 100-200 mesh to obtain a uniform powder. The pellet was pressed using a pressure of 30-60 KN to screen the catalyst precursor with 30-60 mesh particles.
[0040] (8) The catalyst precursor is loaded into a reactor, and reduced at a temperature of 1°C / min to 200-500°C for 0.5-10h in an atmosphere of H2 / N2 or H2 / Ar or pure H2 with a H2 concentration of 5-50%, to obtain a catalyst for hydrogenation of carbon dioxide to methanol.
[0041] The solid-liquid ratio of the anhydrous ethanol to the copper-based metal oxide is (100-200):1; the solid-liquid ratio of the ammonia water (25-28%) to the inorganic silicon compound is (10-20):1; the solid-liquid ratio of the n-hexane to the inorganic silicon compound is (50-100):1.
[0042] The high-selectivity and high-stability carbon dioxide to methanol catalyst of the present invention is used for the carbon dioxide hydrogenation to methanol reaction. The specific reaction conditions are: carbon dioxide hydrogenation reaction pressure 5-150 bar, reaction temperature 180-320 ° C, H2 to CO2 volume ratio 1:9-9:1, reaction gas space velocity 1000-50000 mL h -1 g -1 .
[0043] Example 1
[0044] Take 10 small cylindrical Cu-Zn-Zr metal oxides, crush them in a mortar and grind them into powder, sieve through 120 mesh to obtain uniform powder. Weigh 2.0g of powder in a beaker, add 300mL of anhydrous ethanol to it, ultrasonicate at 40℃ for 1h, add 1.0mL of silica sol to the mixture, place it on a stirring table, stir at 40℃ for 4h at a speed of 450r / min, then add 25mL of ammonia water (25%~28%), continue stirring for 4h at the same speed and reaction temperature, and then the mixture is centrifuged and washed with anhydrous ethanol to obtain a filter cake, which is transferred to a 100~120℃ oven and dried for 10h. The dried solid product is taken out and cooled to 30℃, and then transferred to a 150℃ vacuum oven and dried for 11h, cooled to 30℃ to obtain a solid sample, and air-dried at 400℃ The solid sample of copper-based metal oxide coated with inorganic silicon was obtained by calcining for 4 hours at room temperature to obtain a solid sample of copper-based metal oxide coated with inorganic silicon. The solid sample was added to 150 mL of n-hexane, placed on a stirring platform, stirred at 40°C for 0.5 hours at a speed of 450 r / min, and then 0.8 mL of trimethylchlorosilane was added. At the same speed and reaction temperature, stirring was continued for 0.5 hours, and ultrasonic was performed for 3 hours to obtain a suspension. After centrifugal washing with n-hexane, it was transferred to an 80°C vacuum oven for drying for 11 hours. The dried solid product was taken out and cooled to 30°C, placed in a mortar and ground to powder, sieved through 120 mesh, and uniform powder was obtained. The tablet was pressed with a pressure of 30KN, and 30 to 60 mesh particles were screened to obtain a catalyst precursor. The catalyst precursor was loaded into a reactor, heated to 300°C at 1°C / min and reduced for 2 hours under a 10% H2 / N2 atmosphere at normal pressure to obtain a Cu-Zn-Zr / silica sol-TMSCl catalyst.
[0045] The catalyst was used for the evaluation of carbon dioxide hydrogenation reaction. The specific operation was as follows: a fixed bed reactor was used, the catalyst loading was 0.5 g, the carbon dioxide hydrogenation reaction pressure was adjusted to 60 bar, the reaction temperature was 230 °C, the volume ratio of H2 to CO2 was 3:1, and the reaction gas space velocity was 9000 mL h -1 g -1 The performance evaluation results of the catalyst are shown in Table 1. Figure 1 The results of catalyst stability evaluation show that during the 100h reaction time, there was no significant change in carbon dioxide conversion and methanol selectivity on the Cu-Zn-Zr / silica sol-TMSCl catalyst, showing good stability.
[0046] Example 2
[0047] Take 10 small cylindrical Cu-Zn-Zr metal oxides, crush them in a mortar and grind them into powder, sieve through 120 mesh to obtain uniform powder. Weigh 2.0g of powder in a beaker, add 300mL of anhydrous ethanol to it, ultrasonicate at 40℃ for 1h, add 1.0mL of silica sol to the mixture, place it on a stirring table, stir at 40℃ for 4h at a speed of 450r / min, then add 25mL of ammonia water (25%~28%), continue stirring for 4h at the same speed and reaction temperature, and then the mixture is washed by centrifugation with anhydrous ethanol to obtain a filter cake, which is transferred to a 100~120℃ oven and dried for 10h. The dried solid product is taken out and cooled to 30℃, and then transferred to a 150℃ vacuum oven and dried for 11h, cooled to 30℃ to obtain a solid sample, and baked at 400℃ in air. After calcination for 4 hours, a solid sample of copper-based metal oxide coated with inorganic silicon was obtained. The solid sample was added to 150 mL of n-hexane, placed on a stirring table, stirred at 40°C for 0.5 hours at a speed of 450 r / min, and then 0.8 mL of tert-butyldimethylchlorosilane was added. At the same speed and reaction temperature, stirring was continued for 0.5 hours, and ultrasonication was performed for 3 hours to obtain a suspension. After centrifugal washing with n-hexane, it was transferred to an 80°C vacuum oven for drying for 11 hours. The dried solid product was taken out and cooled to 30°C, placed in a mortar and ground to powder, sieved through 120 mesh, and uniform powder was obtained. The tablet was pressed with a pressure of 30KN, and 30 to 60 mesh particles were screened to obtain a catalyst precursor. The catalyst precursor was loaded into a reactor, heated to 300°C at 1°C / min and reduced for 2 hours under a 10% H2 / N2 atmosphere at normal pressure to obtain a Cu-Zn-Zr / silica sol-TBSCl catalyst.
[0048] The catalyst was used for the evaluation of carbon dioxide hydrogenation reaction. The specific operation was as follows: a fixed bed reactor was used, the catalyst loading was 0.5 g, the carbon dioxide hydrogenation reaction pressure was adjusted to 60 bar, the reaction temperature was 230 °C, the volume ratio of H2 to CO2 was 3:1, and the reaction gas space velocity was 9000 mL h -1 g -1 The performance evaluation results of the catalyst are shown in Table 1.
[0049] Example 3
[0050] Take 10 small cylindrical Cu-Zn-Zr metal oxides, crush them in a mortar and grind them into powder, sieve through 120 mesh to obtain uniform powder. Weigh 2.0g of powder in a beaker, add 300mL of anhydrous ethanol to it, ultrasonicate at 40℃ for 1h, add 1.0mL of silica sol to the mixture, place it on a stirring table, stir at 40℃ for 4h at a speed of 450r / min, then add 25mL of ammonia water (25%~28%), continue stirring for 4h at the same speed and reaction temperature, and then the mixture is centrifuged and washed with anhydrous ethanol to obtain a filter cake, which is transferred to a 100~120℃ oven and dried for 10h. The dried solid product is taken out and cooled to 30℃, and then transferred to a 150℃ vacuum oven and dried for 11h, cooled to 30℃ to obtain a solid sample, and then dried at 400℃ in air. After calcination for 4 hours, a solid sample of copper-based metal oxide coated with inorganic silicon was obtained. The solid sample was added to 150 mL of n-hexane, placed on a stirring table, stirred at 40°C for 0.5 hours at a speed of 450 r / min, and then 0.8 mL of triisopropylsilyl chloride was added. At the same speed and reaction temperature, stirring was continued for 0.5 hours, and ultrasonic was performed for 3 hours to obtain a suspension. After centrifugal washing with n-hexane, it was transferred to an 80°C vacuum oven for drying for 11 hours. The dried solid product was taken out and cooled to 30°C, placed in a mortar and ground to powder, sieved through 120 mesh, and uniform powder was obtained. The tablet was pressed with a pressure of 30KN, and 30 to 60 mesh particles were screened to obtain a catalyst precursor. The catalyst precursor was loaded into a reactor, heated to 300°C at 1°C / min and reduced for 2 hours under a 10% H2 / N2 atmosphere at normal pressure to obtain a Cu-Zn-Zr / silica sol-TIPSCl catalyst.
[0051] The catalyst was used for the evaluation of carbon dioxide hydrogenation reaction. The specific operation was as follows: a fixed bed reactor was used, the catalyst loading was 0.5 g, the carbon dioxide hydrogenation reaction pressure was adjusted to 60 bar, the reaction temperature was 230 °C, the volume ratio of H2 to CO2 was 3:1, and the reaction gas space velocity was 9000 mL h -1 g -1 The performance evaluation results of the catalyst are shown in Table 1.
[0052] Example 4
[0053] Take 10 small cylindrical Cu-Zn-Zr metal oxides, crush them in a mortar and grind them into powder, sieve through 120 mesh to obtain uniform powder. Weigh 2.0g of powder in a beaker, add 300mL of anhydrous ethanol to it, ultrasonicate at 40℃ for 1h, add 1.0mL of silica sol to the mixture, place it on a stirring table, stir at 40℃ for 4h at a speed of 450r / min, then add 25mL of ammonia water (25%~28%), continue stirring for 4h at the same speed and reaction temperature, and then the mixture is centrifuged and washed with anhydrous ethanol to obtain a filter cake, which is transferred to a 100~120℃ oven and dried for 10h. The dried solid product is taken out and cooled to 30℃, and then transferred to a 150℃ vacuum oven and dried for 11h, cooled to 30℃ to obtain a solid sample, and then dried at 400℃ in air. After calcination for 4 hours, a solid sample of copper-based metal oxide coated with inorganic silicon was obtained. The solid sample was added to 150 mL of n-hexane, placed on a stirring table, stirred at 40°C for 0.5 hours at a speed of 450 r / min, and then 0.8 mL of di-tert-butyldichlorosilane was added. At the same speed and reaction temperature, stirring was continued for 0.5 hours, and ultrasonic was performed for 3 hours to obtain a suspension. After centrifugal washing with n-hexane, it was transferred to an 80°C vacuum oven for drying for 11 hours. The dried solid product was taken out and cooled to 30°C, placed in a mortar and ground to powder, sieved through 120 mesh, and uniform powder was obtained. The tablet was pressed with a pressure of 30KN, and 30 to 60 mesh particles were screened to obtain a catalyst precursor. The catalyst precursor was loaded into a reactor, heated to 300°C at 1°C / min and reduced for 2 hours under a 10% H2 / N2 atmosphere at normal pressure to obtain a Cu-Zn-Zr / silica sol-DTBSCl2 catalyst.
[0054] The catalyst was used for the evaluation of carbon dioxide hydrogenation reaction. The specific operation was as follows: a fixed bed reactor was used, the catalyst loading was 0.5 g, the carbon dioxide hydrogenation reaction pressure was adjusted to 60 bar, the reaction temperature was 230 °C, the volume ratio of H2 to CO2 was 3:1, and the reaction gas space velocity was 9000 mL h -1 g -1 The performance evaluation results of the catalyst are shown in Table 1.
[0055] Example 5
[0056] Take 10 small cylindrical Cu-Zn-Al metal oxides, crush them in a mortar and grind them into powder, sieve through 120 mesh to obtain uniform powder. Weigh 2.0g of powder in a beaker, add 300mL of anhydrous ethanol to it, ultrasonicate at 40℃ for 1h, add 1.0mL of silica sol to the mixture, place it on a stirring table, stir at 40℃ for 4h at a speed of 450r / min, then add 25mL of ammonia water (25%~28%), continue stirring for 4h at the same speed and reaction temperature, and then the mixture is centrifuged and washed with anhydrous ethanol to obtain a filter cake, which is transferred to a 100~120℃ oven and dried for 10h. The dried solid product is taken out and cooled to 30℃, and then transferred to a 150℃ vacuum oven and dried for 11h, cooled to 30℃ to obtain a solid sample, and air-dried at 400℃ The solid sample of copper-based metal oxide coated with inorganic silicon was obtained by calcining for 4 hours at room temperature to obtain a solid sample of copper-based metal oxide coated with inorganic silicon. The solid sample was added to 150 mL of n-hexane, placed on a stirring platform, stirred at 40°C for 0.5 hours at a speed of 450 r / min, and then 0.8 mL of trimethylchlorosilane was added. At the same speed and reaction temperature, stirring was continued for 0.5 hours, and ultrasonication was performed for 3 hours to obtain a suspension. After centrifugal washing with n-hexane, it was transferred to an 80°C vacuum oven for drying for 11 hours. The dried solid product was taken out and cooled to 30°C, placed in a mortar and ground to powder, sieved through 120 mesh, and uniform powder was obtained. The catalyst precursor was screened with a pressure of 30KN to obtain a catalyst precursor by screening 30 to 60 mesh particles. The catalyst precursor was loaded into a reactor, heated to 300°C at 1°C / min and reduced for 2 hours under a 10% H2 / N2 atmosphere at normal pressure to obtain a Cu-Zn-Al / silica sol-TMSCl catalyst.
[0057] The catalyst was used for the evaluation of carbon dioxide hydrogenation reaction. The specific operation was as follows: a fixed bed reactor was used, the catalyst loading was 0.5 g, the carbon dioxide hydrogenation reaction pressure was adjusted to 60 bar, the reaction temperature was 230 °C, the volume ratio of H2 to CO2 was 3:1, and the reaction gas space velocity was 9000 mL h -1 g -1 The performance evaluation results of the catalyst are shown in Table 1.
[0058] Example 6
[0059] Take 10 small cylindrical Cu-Zn-Zr metal oxides, crush them in a mortar and grind them into powder, sieve through 120 mesh to obtain uniform powder. Weigh 2.0g of powder in a beaker, add 300mL of anhydrous ethanol to it, ultrasonicate at 40℃ for 1h, add 0.5mL of sodium silicate to the mixture, place it on a stirring table, stir at 40℃ for 4h at a speed of 450r / min, then add 25mL of ammonia water (25%~28%), continue stirring for 4h at the same speed and reaction temperature, and then the mixture is centrifuged and washed with anhydrous ethanol to obtain a filter cake, which is transferred to a 100~120℃ oven and dried for 10h. The dried solid product is taken out and cooled to 30℃, and then transferred to a 150℃ vacuum oven and dried for 11h, cooled to 30℃ to obtain a solid sample, and then placed in an air conditioner at 400℃ The solid sample of copper-based metal oxide coated with inorganic silicon was obtained by calcining for 4 hours at room temperature to obtain a solid sample of copper-based metal oxide coated with inorganic silicon. The solid sample was added to 150 mL of n-hexane, placed on a stirring platform, stirred at 40°C for 0.5 hours at a speed of 450 r / min, and then 0.8 mL of trimethylchlorosilane was added. At the same speed and reaction temperature, stirring was continued for 0.5 hours, and ultrasonication was performed for 3 hours to obtain a suspension. After centrifugal washing with n-hexane, it was transferred to an 80°C vacuum oven for drying for 11 hours. The dried solid product was taken out and cooled to 30°C, placed in a mortar and ground to powder, sieved through 120 mesh, and uniform powder was obtained. The catalyst precursor was screened with a pressure of 30KN to obtain a catalyst precursor by screening 30 to 60 mesh particles. The catalyst precursor was loaded into a reactor, heated to 300°C at 1°C / min and reduced for 2 hours under a 10% H2 / N2 atmosphere at normal pressure to obtain a Cu-Zn-Zr / sodium silicate-TMSCl catalyst.
[0060] The catalyst was used for the evaluation of carbon dioxide hydrogenation reaction. The specific operation was as follows: a fixed bed reactor was used, the catalyst loading was 0.5 g, the carbon dioxide hydrogenation reaction pressure was adjusted to 60 bar, the reaction temperature was 230 °C, the volume ratio of H2 to CO2 was 3:1, and the reaction gas space velocity was 9000 mL h -1 g -1 The performance evaluation results of the catalyst are shown in Table 1.
[0061] Example 7
[0062] Take 10 small cylindrical Cu-Zn-Al metal oxides, crush them in a mortar and grind them into powder, sieve through 120 mesh to obtain uniform powder. Weigh 2.0g of powder in a beaker, add 300mL of anhydrous ethanol to it, ultrasonicate at 40℃ for 1h, add 0.5mL of sodium silicate to the mixture, place it on a stirring table, stir at 40℃ for 4h at a speed of 450r / min, then add 25mL of ammonia water (25%~28%), continue stirring for 4h at the same speed and reaction temperature, and then the mixture is centrifuged and washed with anhydrous ethanol to obtain a filter cake, which is transferred to a 100~120℃ oven and dried for 10h. The dried solid product is taken out and cooled to 30℃, and then transferred to a 150℃ vacuum oven and dried for 11h, cooled to 30℃ to obtain a solid sample, and air-dried at 400℃ The solid sample of copper-based metal oxide coated with inorganic silicon was obtained by calcining for 4 hours at room temperature to obtain a solid sample of copper-based metal oxide coated with inorganic silicon. The solid sample was added to 150 mL of n-hexane, placed on a stirring table, stirred at 40°C for 0.5 hours at a speed of 450 r / min, and then 0.8 mL of trimethylchlorosilane was added. At the same speed and reaction temperature, stirring was continued for 0.5 hours, and ultrasonication was performed for 3 hours to obtain a suspension. After centrifugal washing with n-hexane, it was transferred to an 80°C vacuum oven for drying for 11 hours. The dried solid product was taken out and cooled to 30°C, placed in a mortar and ground to powder, sieved through 120 mesh, and uniform powder was obtained. The catalyst precursor was screened with a pressure of 30KN to obtain a catalyst precursor by screening 30 to 60 mesh particles. The catalyst precursor was loaded into a reactor, heated to 300°C at 1°C / min and reduced for 2 hours under a 10% H2 / N2 atmosphere at normal pressure to obtain a Cu-Zn-Al / sodium silicate-TMSCl catalyst.
[0063] The catalyst was used for the evaluation of carbon dioxide hydrogenation reaction. The specific operation was as follows: a fixed bed reactor was used, the catalyst loading was 0.5 g, the carbon dioxide hydrogenation reaction pressure was adjusted to 60 bar, the reaction temperature was 230 °C, the volume ratio of H2 to CO2 was 3:1, and the reaction gas space velocity was 9000 mL h -1 g -1 The performance evaluation results of the catalyst are shown in Table 1.
[0064] Comparative Example 1
[0065] Take 10 small cylindrical Cu-Zn-Al industrial methanol catalysts, crush them in a mortar and grind them into powder, sieve 120 mesh to obtain uniform powder, use 30KN pressure to press tablets, and screen 30 to 60 mesh particles to obtain catalyst precursors. The catalyst precursor is loaded into a reactor, and the temperature is increased to 300℃ at 1℃ / min under normal pressure and 10% H2 / N2 atmosphere for 2h to obtain a Cu-Zn-Al catalyst, which is recorded as Cu-Zn-Al.
[0066] The catalyst was used for the evaluation of carbon dioxide hydrogenation reaction. The specific operation was as follows: a fixed bed reactor was used, the catalyst loading was 0.5 g, the carbon dioxide hydrogenation reaction pressure was adjusted to 60 bar, the reaction temperature was 230 °C, the volume ratio of H2 to CO2 was 3:1, and the reaction gas space velocity was 12000 mL h -1 g -1 The performance evaluation results of the catalyst are shown in Table 1.
[0067] Comparative Example 2
[0068] Take 10 small cylindrical Cu-Zn-Zr industrial methanol catalysts, crush them in a mortar and grind them into powder, sieve 120 mesh to obtain uniform powder, use 30KN pressure to press tablets, and screen 30 to 60 mesh particles to obtain catalyst precursors. The catalyst precursor is loaded into a reactor, and the temperature is increased to 300℃ at 1℃ / min under normal pressure and 10% H2 / N2 atmosphere for 2h to obtain a Cu-Zn-Zr catalyst, which is recorded as Cu-Zn-Zr.
[0069] The catalyst was used for the evaluation of carbon dioxide hydrogenation reaction. The specific operation was as follows: a fixed bed reactor was used, the catalyst loading was 0.5 g, the carbon dioxide hydrogenation reaction pressure was adjusted to 60 bar, the reaction temperature was 230 °C, the volume ratio of H2 to CO2 was 3:1, and the reaction gas space velocity was 12000 mL h -1 g -1 The performance evaluation results of the catalyst are shown in Table 1. Figure 2 The results of catalyst stability evaluation are shown in the figure. As can be seen from the figure, with the extension of reaction time, the carbon dioxide conversion rate on the Cu-Zn-Zr catalyst decreases, the methanol selectivity decreases significantly, and the byproduct carbon monoxide selectivity increases sharply, that is, the catalyst is deactivated.
[0070] Table 1
[0071]
[0072] The catalyst of the invention is suitable for carbon dioxide hydrogenation reaction, with a carbon dioxide conversion rate exceeding 18%, a methanol selectivity exceeding 87%, and good stability. The catalyst preparation method is simple, the price is low, the performance is excellent, and it has broad industrial application prospects.
Claims
1. A high selectivity and high stability carbon dioxide to methanol catalyst, characterized in that: It comprises a copper-based metal oxide and a silicon dioxide coating layer, wherein the silicon dioxide coating layer comprises an inorganic silicon compound and an organic silane hydrophobic agent; based on the total mass of the catalyst, the mass fraction of the copper-based metal oxide is 50% to 70%, and the remainder is the silicon dioxide coating layer; in the silicon dioxide coating layer, the mass fraction of the inorganic silicon compound is 40% to 70%, and the mass fraction of the organic silane hydrophobic agent is 30% to 60%; The inorganic silicon compound includes at least one of white carbon black, silica sol, and silicate, and the organosilane hydrophobic agent includes at least one of trimethylchlorosilane, tert-butyldimethylchlorosilane, triisopropylchlorosilane, and di-tert-butyldichlorosilane; The copper-based metal oxide is at least one of copper-zinc-aluminum and copper-zinc-zirconium.
2. The method for preparing a high-selectivity and high-stability carbon dioxide to methanol catalyst according to claim 1, characterized in that The following steps are involved: 1) Add copper-based metal oxide to anhydrous ethanol for dispersion, then add inorganic silicon compound, stir, then add ammonia water, continue stirring, and finally centrifuge and wash to obtain a filter cake; 2) drying and calcining the filter cake obtained in step 1) to obtain a copper-based metal oxide solid sample coated with inorganic silicon; 3) adding the inorganic silicon-coated copper-based metal oxide solid sample obtained in step 2) into n-hexane, stirring, then adding an organic silane hydrophobic agent, continuing to stir, and then ultrasonicating to obtain a suspension; 4) The suspension obtained in step 3) is centrifuged, washed, dried, and reduced to obtain a catalyst for hydrogenating carbon dioxide to methanol.
3. The preparation method according to claim 2, characterized in that: In step 1), the copper-based metal oxide is prepared by a co-precipitation method, a sol-gel method or a hydrothermal method.
4. The preparation method according to claim 2, characterized in that: In step 1), the mass ratio of the anhydrous ethanol to the copper-based metal oxide is (100-200):1; the mass ratio of the ammonia water to the inorganic silicon compound is (10-20):1, and the concentration of the ammonia water is 25%-28%; in step 3), the mass ratio of the n-hexane to the inorganic silicon compound is (50-100):
1.
5. The preparation method according to claim 2, characterized in that: In step 1), the stirring speed is 200~1000 r / min, the stirring temperature is 20~60 ℃, and the stirring time is 2~8 h; in step 3), the stirring speed is 200~1000 r / min, the stirring temperature is 20~60 ℃, the stirring time is 0.5~1.5 h, and the ultrasonic time is 1~4 h.
6. The preparation method according to claim 2, characterized in that: In step 2), the drying step is: drying in an oven at 100-120°C for 2-10 h, taking out the dried solid product and cooling it, and then transferring it to a vacuum oven at 130-160°C for drying for 5-12 h; the calcining step is: calcining at 300-600°C in an air atmosphere for 2-12 h.
7. The preparation method according to claim 2, characterized in that: In step 4), the reduction conditions are: reduction at a temperature of 200-500 °C for 0.5-10 h in an atmosphere of H2 / N2 or H2 / Ar or pure H2 with a H2 concentration of 5%-50%.
8. The high-selectivity and high-stability carbon dioxide to methanol catalyst of claim 1 and the catalyst prepared by the preparation method of any one of claims 2 to 7 are used in the carbon dioxide hydrogenation to methanol reaction, and the reaction conditions are: using a fixed bed reactor, the catalyst loading amount is 0.5 g, the carbon dioxide hydrogenation reaction pressure is adjusted to 60 bar, the reaction temperature is 230 ° C, the volume ratio of H2 to CO2 is 3:1, and the reaction gas space velocity is 9000 mL h -1 g -1 .