Intercalated hydrotalcite-stabilized AKD emulsion and preparation method thereof

The method of stabilizing AKD emulsion by inserting hydrotalcites has solved the problem of stability and low glue application efficiency in preparing AKD emulsions with starch emulsifiers and polymer emulsifiers, and achieved high stability and efficient glue application effects, which are suitable for papermaking fields. .

CN116641256BActive Publication Date: 2024-11-26SHANGHAI DONGSHENG NEW MATERIALS
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202310837455.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-10
Publication Date
2024-11-26
Estimated Expiration
2043-07-10

AI Technical Summary

Technical Problem

In the prior art, the AKD emulsion prepared by starch emulsifier has poor stability and the AKD emulsifier has low glue application efficiency.

Method used

Using the method of stabilizing AKD emulsion by intercalating hydrotalcite, the hydrotalcite aqueous solution, zirconium oxychloride and iron-free aluminum sulfate aqueous solution are used to stabilize the AKD emulsion by constituting AKD wax powder, intercalating hydrotalcite aqueous solution, and using the hydrophilic and lipophilic interface mask and adsorption of intercalating hydrotalcite. Effects to improve the stability of AKD emulsion.

Benefits of technology

It improves the stability and glue application efficiency of AKD emulsion, reduces costs, and is suitable for promotion and application in the field of papermaking.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004329373070000071
    Figure BDA0004329373070000071
  • Figure BDA0004329373070000081
    Figure BDA0004329373070000081
Patent Text Reader

Abstract

The invention provides an intercalated hydrotalcite-stabilized AKD emulsion, which is composed of AKD wax powder, an intercalated hydrotalcite aqueous solution, zirconium oxychloride and an iron-free aluminum sulfate aqueous solution, wherein the mass ratio of AKD wax powder to intercalated hydrotalcite is 10-20:1, the mass ratio of AKD wax powder to zirconium oxychloride is 50-65:1, the mass ratio of AKD wax powder to iron-free aluminum sulfate is 10-30:1, and the intercalated hydrotalcite is selected from sodium lignin sulfonate intercalated hydrotalcite or sodium dinaphthylmethane disulfonate intercalated hydrotalcite. The preparation method of the intercalated hydrotalcite-stabilized AKD emulsion comprises adding zirconium oxychloride and molten AKD to an intercalated hydrotalcite aqueous solution, mixing, high-pressure homogenizing, adding an iron-free aluminum sulfate solution, mixing evenly, and then sieving to remove impurities. The invention provides a method for preparing AKD emulsion by using intercalated hydrotalcite, which solves the problem that the traditional hydrotalcite alone has poor effect in emulsifying AKD, and the amount of intercalated hydrotalcite is small, the prepared emulsion has high stability and high sizing efficiency, and is suitable for promotion and application in the field of papermaking.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of papermaking sizing agents, and in particular to a method for preparing AKD emulsion by using intercalated hydrotalcite. Background Art

[0002] At present, the major changes in neutral papermaking technology have caused the world's papermaking to begin to change from acidic to alkaline. Although most domestic paper mills still use acidic papermaking technology, the many benefits of neutral papermaking and environmental protection requirements have prompted many manufacturers to begin to adopt neutral papermaking. The so-called neutral papermaking refers to a papermaking method in which the pH of the pulp is always controlled above 7 during the entire papermaking process. One of the key links in neutral papermaking is the selection of neutral sizing agents or neutral sizing systems.

[0003] Alkyl Ketene dimers, referred to as AKD, are a commonly used synthetic sizing agent for neutral sizing. The melting point of solid AKD is about 50°C, and it is insoluble in water. It can only obtain sizing performance by being made into an emulsion. The commonly used emulsifier is cationic starch, but cationic starch has a low charge density, a large molecular weight, and a low bonding strength with AKD particles, so the emulsion stability is poor. At present, the technology of preparing AKD emulsions using high-charge-density polymers is becoming more and more mature. These polymers mainly include polydiallyldimethylammonium chloride and polyethyleneimine, but the cost of polymer emulsifiers is high and the emulsion sizing efficiency is not high. Using solid particles as emulsifiers to prepare emulsions instead of traditional emulsions to prepare stable multiphase systems is the future development direction of AKD emulsions, which is not only cheaper but also more environmentally friendly. In Chinese patent CN114960279A, titanium dioxide is modified by dopamine and then mixed with a composite cationic starch emulsifier to prepare an AKD emulsion, which proves the possibility of solid particle emulsified AKD, but the preparation method is relatively complicated.

[0004] Hydrotalcite is a new type of inorganic functional material with a layered structure. The controllability of the composition and structure of hydrotalcite can be used to adjust the type of interlayer anions to synthesize different types of hydrotalcite and give them different properties. In Chinese patent CN103774498A, a modified hydrotalcite-stabilized AKD emulsion sizing agent is disclosed, which is composed of amino acid in-situ intercalated hydrotalcite, a water phase composed of polyethyleneimine and deionized water, and AKD. The preparation method is also relatively complicated, and polyethyleneimine is still required for joint stabilization. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide an intercalated hydrotalcite-stabilized AKD emulsion and a preparation method of the intercalated hydrotalcite-stabilized AKD emulsion, so as to solve the shortcomings of the prior art that the AKD emulsion prepared by starch emulsifier has poor stability and the AKD emulsion prepared by polymer emulsifier has low sizing efficiency.

[0006] The present invention is achieved by adopting the following technical solutions:

[0007] An intercalated hydrotalcite-stabilized AKD emulsion consists of AKD wax powder, an intercalated hydrotalcite aqueous solution, zirconium oxychloride and an iron-free aluminum sulfate aqueous solution, wherein the mass ratio of AKD wax powder to intercalated hydrotalcite is 10-20:1, the mass ratio of AKD wax powder to zirconium oxychloride is 50-65:1, the mass ratio of AKD wax powder to iron-free aluminum sulfate is 10-30:1, and the intercalated hydrotalcite is selected from sodium lignin sulfonate intercalated hydrotalcite or sodium dinaphthyl methane disulfonate intercalated hydrotalcite.

[0008] The intercalated hydrotalcite stabilized AKD emulsion can use various commonly used alkyl ketene dimers as the AKD wax powder, preferably one of tetradecyl ketene dimer and hexadecyl ketene dimer.

[0009] The intercalated hydrotalcite is obtained by adding a crude hydrotalcite product obtained by treating magnesium salt and aluminum salt under alkaline conditions to an intercalated aqueous solution, wherein the solute of the intercalated aqueous solution is sodium lignin sulfonate or sodium dinaphthylmethane disulfonate. The intercalated hydrotalcite is generally prepared into an aqueous solution with a mass fraction of 2-10% by adding water.

[0010] Preferably, the mass ratio of the solute in the intercalation aqueous solution to the crude hydrotalcite product is 1-1.5:1.

[0011] Preferably, the intercalated hydrotalcite has Mg 2+ / Al 3+ The molar ratio is 2-4:1.

[0012] The preferred mass fraction of the iron-free aluminum sulfate aqueous solution is 15-25%, more preferably 18-22%, and most preferably 20%.

[0013] As a further preferred technical solution, the intercalated hydrotalcite is prepared by the following method: magnesium nitrate and aluminum nitrate are dissolved into an aqueous solution with deionized water and heated to 60-70°C, an ammonia solution is added dropwise under stirring, the pH value is adjusted to 9.5-10.5, and the obtained suspension is transferred to a reactor after sufficient reaction, and reacted at 120-140°C for 10-12h to obtain a crude hydrotalcite product, the crude hydrotalcite product is added to the intercalated aqueous solution, heated to 85-90°C, stirred for 1.5-2h, and then filtered, dried, aged, and ground to obtain the intercalated hydrotalcite.

[0014] The present invention further provides a method for preparing the intercalated hydrotalcite-stabilized AKD emulsion, comprising the following steps:

[0015] S1. Dissolve the intercalated hydrotalcite in deionized water to form an aqueous solution with a mass fraction of 2-10% and preheat to 70-75° C. for later use;

[0016] S2, heating and melting the AKD wax powder;

[0017] S3, sequentially adding zirconium oxychloride and molten AKD into the intercalated hydrotalcite aqueous solution, stirring and mixing at 75-80°C;

[0018] S4, transferring the mixed material of step S3 into a high-pressure homogenizer for homogenization, then cooling the material to below 25° C., adding an iron-free aluminum sulfate solution, mixing evenly, and then sieving to remove impurities to obtain an AKD emulsion.

[0019] Preferably, in step S3, the zirconium oxychloride, molten AKD and intercalated hydrotalcite are preferably mixed under high-speed stirring, and the rotation speed is preferably 2000-2500 r / min.

[0020] Preferably, in step S4, the homogenization temperature is 75-80°C, and the homogenization is performed twice under high pressure, with the pressure of the first pass being 20-25 MPa and the pressure of the second pass being 30-35 MPa.

[0021] The present invention performs intercalation treatment on the hydrotalcite to make it both hydrophilic and lipophilic, and forms a tightly arranged interface film on the surface of the AKD emulsion droplets. The steric hindrance of the interface film weakens the collision and aggregation between the AKD emulsion droplets. At the same time, the intercalated hydrotalcite is adsorbed on the surface of the AKD droplets to make the surface charges of the droplets the same, thereby increasing the electrostatic repulsion between the emulsion droplets. These two effects jointly improve the stability of the AKD emulsion.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] (1) The present invention provides a method for preparing AKD emulsion using intercalated hydrotalcite, which solves the problem that the traditional hydrotalcite alone has poor effect in emulsifying AKD, and the amount of intercalated hydrotalcite used is small, and the obtained emulsion has high stability.

[0024] (2) The present invention provides a method for preparing AKD emulsion by using intercalated hydrotalcite. The process conditions are simple and the emulsion sizing efficiency is high, which is suitable for promotion and application in the field of papermaking. DETAILED DESCRIPTION

[0025] The following description is used to disclose the present invention so that those skilled in the art can implement the present invention. The preferred embodiments described below are only used as examples, but are not used to limit the scope of the present invention. Those skilled in the art can think of other obvious variations. The basic principles of the present invention defined in the following description can be applied to other embodiments, variations, improvements, equivalent solutions, and other technical solutions that do not deviate from the spirit and scope of the present invention.

[0026] The instruments or raw materials in the present invention without indicating the manufacturer are all conventional commercial instruments or raw materials.

[0027] Unless otherwise mentioned, the detection indicators involved in the embodiments of the present invention are detected by conventional detection methods in the art.

[0028] Example 1

[0029] (1) Add 100g magnesium nitrate, 90g aluminum nitrate and 500g deionized water to a reaction flask to dissolve into an aqueous solution and heat to 65°C. Add 25% ammonia solution dropwise under stirring, adjust the pH value to 10, continue stirring for 20-30min, transfer the obtained suspension to a reactor, react at 130°C for 10-12h, cool to room temperature after the reaction, filter and dry the product to obtain a crude hydrotalcite product. Add 50g of the crude hydrotalcite product to 250g of 20% sodium lignin sulfonate aqueous solution and heat to 85-90°C, stir for 1.5-2h, then filter, dry, age and grind to obtain intercalated hydrotalcite. Dissolve 20g of intercalated hydrotalcite in deionized water to form an aqueous solution with a mass fraction of 5% and preheat to 70-75°C for use.

[0030] (2) Heat 200 g of AKD wax powder to 75-80°C to melt.

[0031] (3) 3.5 g of zirconium oxychloride and 200 g of molten AKD wax powder were added to the intercalated hydrotalcite aqueous solution in sequence, and stirred at 2000-2500 r / min at 75-80° C. for 10 min.

[0032] (4) The material after high-speed stirring is quickly transferred to a high-pressure homogenizer, the homogenization temperature is 75-80°C, and the homogenization is performed twice under high pressure, the pressure of the first pass is 20-25MPa, and the pressure of the second pass is 30-35MPa. After homogenization, the material is quickly cooled to below 25°C, 50g of 20% iron-free aluminum sulfate solution is added, mixed evenly, and then sieved, and an appropriate amount of deionized water is added to adjust the solid content to 15%-16%, thereby obtaining AKD emulsion.

[0033] Example 2

[0034] (1) Add 100g magnesium nitrate, 50g aluminum nitrate and 500g deionized water to a reaction flask to dissolve into an aqueous solution and heat to 65°C. Add 25% ammonia solution dropwise under stirring, adjust the pH value to 10, continue stirring for 20-30min, transfer the obtained suspension to a reactor, react at 130°C for 10-12h, cool to room temperature after the reaction, filter and dry the product to obtain a crude hydrotalcite product. Add 50g of the crude hydrotalcite product to 375g of 20% sodium lignin sulfonate aqueous solution and heat to 85-90°C, stir for 1.5-2h, then filter, dry, age and grind to obtain intercalated hydrotalcite. Dissolve 15g of intercalated hydrotalcite in deionized water to a 5% aqueous solution and preheat to 70-75°C for use.

[0035] (2) Heat 200 g of AKD wax powder to 75-80°C to melt.

[0036] (3) 3.5 g of zirconium oxychloride and 200 g of molten AKD wax powder were added to the intercalated hydrotalcite aqueous solution in sequence, and stirred at 2000-2500 r / min at 75-80° C. for 10 min.

[0037] (4) The material after high-speed stirring is quickly transferred to a high-pressure homogenizer, the homogenization temperature is 75-80°C, and the homogenization is performed twice under high pressure, the pressure of the first pass is 20-25MPa, and the pressure of the second pass is 30-35MPa. After homogenization, the material is quickly cooled to below 25°C, 75g of 20% iron-free aluminum sulfate solution is added, mixed evenly, and then sieved, and an appropriate amount of deionized water is added to adjust the solid content to 15%-16%, thereby obtaining AKD emulsion.

[0038] Example 3

[0039] (1) Add 100g of magnesium nitrate, 75g of aluminum nitrate and 500g of deionized water to a reaction flask to dissolve into an aqueous solution and heat to 65°C. Add a 25% ammonia aqueous solution dropwise under stirring, adjust the pH value to 10, continue stirring for 20-30min, transfer the obtained suspension to a reactor, react at 130°C for 10-12h, cool to room temperature after the reaction, filter and dry the product to obtain a crude hydrotalcite product. Add 50g of the crude hydrotalcite product to 300g of a 20% sodium dinaphthylmethane disulfonate aqueous solution and heat to 85-90°C, stir for 1.5-2h, then filter, dry, age and grind to obtain an intercalated hydrotalcite. Dissolve 10g of the intercalated hydrotalcite in deionized water to obtain an aqueous solution with a mass fraction of 5% and preheat to 70-75°C for use.

[0040] (2) Heat 200 g of AKD wax powder to 75-80°C to melt.

[0041] (3) 4 g of zirconium oxychloride and 200 g of molten AKD wax powder were added to the intercalated hydrotalcite aqueous solution in sequence, and stirred at 2000-2500 r / min at 75-80° C. for 10 min.

[0042] (4) The material after high-speed stirring is quickly transferred to a high-pressure homogenizer, the homogenization temperature is 75-80°C, and the homogenization is performed twice under high pressure, the pressure of the first pass is 20-25MPa, and the pressure of the second pass is 30-35MPa. After homogenization, the material is quickly cooled to below 25°C, 35g of 20% iron-free aluminum sulfate solution is added, mixed evenly, and then sieved, and an appropriate amount of deionized water is added to adjust the solid content to 15%-16%, thereby obtaining AKD emulsion.

[0043] Example 4

[0044] (1) Add 100g magnesium nitrate, 60g aluminum nitrate and 500g deionized water to a reaction flask to dissolve into an aqueous solution and heat to 65°C. Add 25% ammonia solution dropwise under stirring, adjust the pH value to 10, continue stirring for 20-30min, transfer the obtained suspension to a reactor, react at 130°C for 10-12h, cool to room temperature after the reaction, filter and dry the product to obtain a crude hydrotalcite product. Add 50g of the crude hydrotalcite product to 275g of 20% sodium dinaphthylmethane disulfonate aqueous solution and heat to 85-90°C, stir for 1.5-2h, then filter, dry, age and grind to obtain intercalated hydrotalcite. Dissolve 20g of intercalated hydrotalcite in deionized water to obtain a 5% aqueous solution and preheat to 70-75°C for use.

[0045] (2) Heat 200 g of AKD wax powder to 75-80°C to melt.

[0046] (3) 3.7 g of zirconium oxychloride and 200 g of molten AKD wax powder were added to the intercalated hydrotalcite aqueous solution in sequence, and stirred at 2000-2500 r / min at 75-80° C. for 10 min.

[0047] (4) The material after high-speed stirring is quickly transferred to a high-pressure homogenizer, the homogenization temperature is 75-80°C, and the homogenization is performed twice under high pressure, the pressure of the first pass is 20-25MPa, and the pressure of the second pass is 30-35MPa. After homogenization, the material is quickly cooled to below 25°C, 100g of 20% iron-free aluminum sulfate solution is added, mixed evenly, and then sieved, and an appropriate amount of deionized water is added to adjust the solid content to 15%-16%, thereby obtaining AKD emulsion.

[0048] Comparative Example 1

[0049] Only hydrotalcite is used to prepare AKD emulsion, and the preparation method comprises the following steps:

[0050] (1) Add 100 g of magnesium nitrate, 60 g of aluminum nitrate and 500 g of deionized water to a reaction bottle to dissolve into an aqueous solution and heat to 65° C., add a 25% by mass ammonia solution dropwise under stirring, adjust the pH value to 10, continue stirring for 20-30 min, transfer the obtained suspension to a reactor, react at 130° C. for 10-12 h, cool to room temperature after the reaction, filter the product, dry, age and grind to obtain a hydrotalcite product, dissolve 20 g of hydrotalcite in deionized water to form an aqueous solution with a mass fraction of 5% and preheat to 70-75° C. for standby use.

[0051] (2) Heat 200 g of AKD wax powder to 75-80°C to melt.

[0052] (3) 3.7 g of zirconium oxychloride and 200 g of molten AKD wax powder were added to the hydrotalcite aqueous solution in sequence, and stirred at 2000-2500 r / min at 75-80° C. for 10 min.

[0053] (4) The material after high-speed stirring is quickly transferred to a high-pressure homogenizer, the homogenization temperature is 75-80°C, and the homogenization is performed twice under high pressure, the pressure of the first pass is 20-25MPa, and the pressure of the second pass is 30-35MPa. After homogenization, the material is quickly cooled to below 25°C, 100g of 20% iron-free aluminum sulfate solution is added, mixed evenly, and then sieved, and an appropriate amount of deionized water is added to adjust the solid content to 15%-16%. If it is found that the filter residue is added too much, an appropriate amount of deionized water is added to adjust the solid content to 15%-16%, and AKD emulsion is obtained.

[0054] Comparative Example 2

[0055] Only hydrotalcite is used to prepare AKD emulsion, and the preparation method comprises the following steps:

[0056] (1) Add 100 g of magnesium nitrate, 80 g of aluminum nitrate and 500 g of deionized water to a reaction bottle to dissolve into an aqueous solution and heat to 65° C., add a 25% by mass ammonia solution dropwise under stirring, adjust the pH value to 10, continue stirring for 20-30 min, transfer the obtained suspension to a reactor, react at 130° C. for 10-12 h, cool to room temperature after the reaction, filter the product, dry, age and grind to obtain a hydrotalcite product, dissolve 20 g of hydrotalcite in deionized water to form an aqueous solution with a mass fraction of 5% and preheat to 70-75° C. for standby use.

[0057] (2) Heat 200 g of AKD wax powder to 75-80°C to melt.

[0058] (3) 3.5 g of zirconium oxychloride and 200 g of molten AKD wax powder were added to the hydrotalcite aqueous solution in sequence, and stirred at 2000-2500 r / min at 75-80° C. for 10 min.

[0059] (4) The material after high-speed stirring is quickly transferred to a high-pressure homogenizer, the homogenization temperature is 75-80°C, and the homogenization is performed twice under high pressure, the pressure of the first pass is 20-25MPa, and the pressure of the second pass is 30-35MPa. After homogenization, the material is quickly cooled to below 25°C, 80g of 20% iron-free aluminum sulfate solution is added, mixed evenly, and then sieved. If there is a lot of filter residue, add an appropriate amount of deionized water to adjust the solid content to 15%-16%, and AKD emulsion is obtained.

[0060] The particle size and stability of the AKD emulsions prepared in the examples and comparative examples were tested, and the results are shown in Table 1.

[0061] Table 1 Different AKD emulsion particle size and stability results

[0062]

[0063]

[0064] From the above test results, it can be seen that the AKD emulsion prepared using only hydrotalcite has more filter residue and poor stability, and cannot be stored stably for a long time. The AKD emulsion prepared using intercalated hydrotalcite has a smaller particle size, is more stable, and can be stored for a long time.

[0065] Application Examples

[0066] The AKD emulsions of Examples 1-4 and Comparative Examples 1-2 were sized under the following conditions:

[0067] Pulp: coniferous pulp / broadleaf pulp / chemical mechanical pulp = 20:40:40

[0068] Beating degree: 35-40°SR

[0069] Paper weight: 80g / m 2

[0070] Sizing agent addition amount: 10kg / t paper

[0071] Cationic polyacrylamide dosage: 200ppm

[0072] Process: Weigh the pulp, then add AKD emulsion, stir for 1 minute, add mixed calcium (35%) and cationic polyacrylamide in turn, stir for 1 minute each, then take out the prepared pulp, use a semi-automatic paper sheet former to make sheets, and press with a standard paper sheet press, dry with a glazing machine for 10 minutes, then test the paper sample and age it in an oven at 105℃ for 10 minutes, and measure the water absorption value of the paper sample for 1 minute. The test results are shown in Table 2.

[0073] Table 2 Test results of water absorption properties of paper samples prepared from different samples

[0074] sample <![CDATA[Water absorption value g / m 2 > Example 1 22.3 Example 2 25.6 Example 3 20.5 Example 4 23.7 Comparative Example 1 99.8 Comparative Example 2 103.4

[0075] It can be seen from the above application results that the sizing effect of AKD emulsion prepared by using intercalated hydrotalcite is better than that of using only hydrotalcite.

[0076] It should be understood by those skilled in the art that the above embodiments are only examples and do not limit the present invention. The purpose of the present invention has been fully and effectively achieved. The functional and structural principles of the present invention have been demonstrated and explained in the embodiments, and the embodiments of the present invention may be deformed or modified in any way without departing from the principles.

Claims

1. An intercalated hydrotalcite-stabilized AKD emulsion, characterized in that: The invention comprises AKD wax powder, an intercalated hydrotalcite aqueous solution, zirconium oxychloride and an iron-free aluminum sulfate aqueous solution, wherein the mass ratio of AKD wax powder to intercalated hydrotalcite is 10-20:1, the mass ratio of AKD wax powder to zirconium oxychloride is 50-65:1, the mass ratio of AKD wax powder to iron-free aluminum sulfate is 10-30:1, the intercalated hydrotalcite is selected from sodium lignin sulfonate intercalated hydrotalcite or sodium dinaphthyl methane disulfonate intercalated hydrotalcite; the intercalated hydrotalcite is obtained by adding a crude hydrotalcite product obtained by preparing magnesium salt and aluminum salt under alkaline conditions, the solute of the intercalated aqueous solution is sodium lignin sulfonate or sodium dinaphthyl methane disulfonate, and the mass ratio of the solute of the intercalated aqueous solution to the crude hydrotalcite product is 1-1.5:

1.

2. The intercalated hydrotalcite-stabilized AKD emulsion according to claim 1, characterized in that: The Mg in the intercalated hydrotalcite 2+ / Al 3+ The molar ratio is 2-4:

1.

3. The intercalated hydrotalcite-stabilized AKD emulsion according to claim 1, characterized in that: The intercalated hydrotalcite is prepared by the following method: magnesium nitrate and aluminum nitrate are dissolved into an aqueous solution with deionized water and heated to 60-70°C, an ammonia solution is added dropwise under stirring, the pH value is adjusted to 9.5-10.5, and the obtained suspension is transferred to a reactor after sufficient reaction, and reacted at 120-140°C for 10-12h to obtain a crude hydrotalcite product, the crude hydrotalcite product is added to the intercalated aqueous solution, heated to 85-90°C, stirred for 1.5-2h, and then filtered, dried, aged, and ground to obtain the intercalated hydrotalcite.

4. The intercalated hydrotalcite-stabilized AKD emulsion according to claim 1, characterized in that: The AKD wax powder is selected from one of tetradecyl ketene dimer and hexadecyl ketene dimer.

5. The intercalated hydrotalcite-stabilized AKD emulsion according to claim 1, characterized in that: The intercalated hydrotalcite is added with water to prepare an aqueous solution with a mass fraction of 2-10%.

6. The method for preparing the intercalated hydrotalcite-stabilized AKD emulsion according to any one of claims 1 to 5, characterized in that: The steps include: S1. Dissolve the intercalated hydrotalcite in deionized water to form an aqueous solution with a mass fraction of 2-10% and preheat to 70-75° C. for later use; S2, heating and melting the AKD wax powder; S3, sequentially adding zirconium oxychloride and molten AKD into the intercalated hydrotalcite aqueous solution, stirring and mixing at 75-80°C; S4, transferring the mixed material of step S3 into a high-pressure homogenizer for homogenization, then cooling the material to below 25° C., adding an iron-free aluminum sulfate solution, mixing evenly, and then sieving to remove impurities to obtain an AKD emulsion.

7. The method according to claim 6, characterized in that Step S3 is to mix zirconium oxychloride, molten AKD and intercalated hydrotalcite under high-speed stirring at a speed of 2000-2500 r / min.

8. The method according to claim 6, characterized in that In step S4, the homogenization temperature is 75-80°C, and the homogenization is performed twice under high pressure, with the pressure of the first pass being 20-25 MPa and the pressure of the second pass being 30-35 MPa.

Citation Information

Patent Citations

  • Modified hydrotalcite stabilized AKD (Alkyl Ketene Dimer) emulsion sizing agent and preparation method thereof

    CN103774498A

  • AKD (alkyl ketene dimer) production process based on dopamine modified titanium dioxide

    CN114960279A

  • Preparation method of stable AKD (Alkyl Ketene Dimer) emulsion sizing agent for modified hydrotalcite

    CN103774496A

  • Application of ligninsulfonate-intercalated hydrotalcite

    CN105664866A

  • Method for preparing alkyl ketene dimer emulsion without surfactants

    CN105908567A