A method for preparing eucommia gum with high efficiency and high yield

Through the phased reaction between pretreatment solvent and Eucommia ulmoide resource and petroleum ether extraction method, the problems of time, high cost and environmental pollution during the extraction process of Eucommia ulmoide gel are solved, and efficient and high-yield preparation of Eucommia ulmoide gel and the green solvent are achieved. Recycling improves the extraction efficiency and purification effect of the glue.

CN116655941BActive Publication Date: 2024-11-19BEIJING FORESTRY UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310864124.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-14
Publication Date
2024-11-19
Estimated Expiration
2043-07-14

AI Technical Summary

Technical Problem

In the prior art, the extraction method of Eucommia ulmoides is long, costly and low efficiency, and consumes a lot of alkali, acid and organic solvents, resulting in serious environmental pollution, making it difficult to achieve efficient and high-yield preparation of Eucommia ulmoides and Green recovery of solvent.

Method used

Pretreatment solvents (choline chloride or betaine and ethylene glycol, formic acid, ethanolamine and other mixtures) are used to react with the biomass materials of Eucommia resources in stages, combined with the use of petroleum ether, solid Eucommia gel is obtained by separation and refrigeration. , and recover the solvent through acidic aqueous solution to achieve reusing solvent.

Benefits of technology

It improves the extraction efficiency and yield of Eucommia ulmoides, reduces solvent consumption and environmental pollution, and is easy to prepare, low-priced, and biodegradable, effectively breaks the barriers between lignin and cell walls, and improves the purification effect of the glue.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116655941B_ABST
    Figure CN116655941B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing eucommia gum with high efficiency and high yield, which belongs to the technical field of natural product extraction, and comprises the following steps: pre-preparing choline chloride or betaine with ethylene glycol, formic acid, ethanolamine or isopropanol by mixing and heating or pre-preparing without heating to obtain a pre-prepared solvent; mixing the pre-prepared solvent with eucommia resource biomass to carry out a first-stage reaction, and then adding petroleum ether to carry out a second-stage reaction. The liquid component a and the solid residue in the product obtained after the reaction are separated; the petroleum ether layer rich in eucommia gum in the liquid component a is refrigerated at low temperature, and then centrifuged to obtain solid eucommia gum and petroleum ether. The core of the eucommia gum preparation method of the invention is not to directly extract eucommia gum with common solvents, but to extract natural eucommia gum with a method of pretreatment combined with organic solvent extraction.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of natural product extraction, and more specifically relates to a method for preparing eucommia gum with high efficiency and high yield. Background Art

[0002] Eucommia gum is a strategic natural polymer material with a structure of trans-1,4-polyisoprene, which is an isomer of cis-1,4-polyisoprene of natural rubber and can be used as a potential rubber resource. Its molecular structure is as follows:

[0003]

[0004] As a new type of natural rubber, it is one of the most promising high-quality natural rubber resources in the world besides Hevea brasiliensis. my country's Eucommia resources account for more than 95% of the world's total resource area, with the unique advantage of independent and controllable resources. In recent years, my country has actively promoted the application and development of Eucommia gum, focusing on the development of this unique biopolymer resource in my country.

[0005] Eucommia gum exists in the plant body and is surrounded by cell walls composed of a variety of complex non-glue components, forming a natural barrier for the separation of Eucommia gum, which seriously hinders the extraction of Eucommia gum. The extraction of Eucommia gum is essentially to break the above-mentioned cell wall barrier, extract the Eucommia gum in the glue-containing cells, and further separate and purify it to obtain a white solid. Therefore, the extraction of Eucommia gum is not as simple as the direct tapping of Hevea brasiliensis, and physical, chemical, biological and other methods are required. At present, the extraction methods of Eucommia gum in industry include mechanical method, alkali leaching method, fermentation method, organic solvent extraction method, comprehensive method, etc. Since Eucommia gum is surrounded by a variety of natural macromolecules, and natural macromolecules such as lignin and cellulose are insoluble in organic solvents, it is usually necessary to use mechanical method or appropriate alkali solution and acid solution pretreatment before extracting Eucommia gum. However, this method consumes a large amount of alkali solution, acid solution organic solvent and energy consumption in the production process, the cost is too high, and the environmental pollution is serious.

[0006] Commonly used extraction solvents include benzene, toluene, petroleum ether and chloroform. Among them, eucommia gum has the highest solubility in chloroform, but it is difficult to precipitate after dissolution. The gum obtained by distillation to remove chloroform is dense and difficult to purify. Petroleum ether is also the most common extraction solvent. However, the preparation process of organic solvent extraction method is time-consuming and requires repeated extraction, and the yield of eucommia gum is low.

[0007] In addition, the existing biological, mechanical and comprehensive methods are relatively complex, costly and inefficient. In the preparation of eucommia gum, they cannot achieve the separation and conversion of the main components of the cell wall of eucommia industrial resources.

[0008] Therefore, how to develop a method for preparing eucommia gum with high efficiency and high yield is a technical problem that technical personnel in this field urgently need to solve. Summary of the invention

[0009] The main purpose of the present invention is to provide a method for preparing eucommia gum with high efficiency and high yield. The problem to be solved is how to achieve efficient and high yield preparation of eucommia gum and realize green recovery of solvent at the same time.

[0010] In order to achieve the above object, the present invention adopts the following technical solution:

[0011] A method for preparing eucommia gum with high efficiency and high yield comprises the following steps:

[0012] (1) mixing choline chloride or betaine with ethylene glycol, formic acid, ethanolamine or isopropanol in a molar ratio of (0-10):(1-10) and heating or pre-heating without heating, the heating temperature is 80° C., the heating time is 30 minutes, to obtain a pre-made solvent;

[0013] (2) Mixing the Eucommia biomass raw material with the pre-made solvent in a ratio of 1:(5-20) to carry out a first stage reaction at a reaction temperature of 80-100° C. for a reaction time of 1-3 h.

[0014] (3) adding petroleum ether to the reactants obtained in step (2) and mixing them, wherein the mass ratio of petroleum ether to the Eucommia biomass raw material is (1-10):1, and performing a second stage reaction at a reaction temperature of 70-90° C. and a reaction time of 1-3 hours;

[0015] (4) separating the liquid component a and the solid residue in the product obtained after the reaction in step (3);

[0016] (5) allowing the liquid component a in step (4) to stand for stratification to obtain a petroleum ether layer rich in eucommia gum, refrigerating the petroleum ether layer rich in eucommia gum at low temperature, and then centrifuging to obtain solid eucommia gum and petroleum ether, and collecting the petroleum ether for reuse;

[0017] (6) adding 5 times the volume of pH=2 acidic aqueous solution to obtain liquid b after removing the petroleum ether layer rich in eucommia gum from the liquid component a in step (5), and then performing solid-liquid separation. After rotary evaporation and concentration, the obtained liquid component c is again obtained to obtain the pre-made solvent for repeated use.

[0018] Furthermore, in step (1), the eucommia resource biomass is one or more of eucommia bark, eucommia leaves or eucommia wing fruits.

[0019] Furthermore, in the above step (1), the pre-made solution is ready for use, and in the step (3), the boiling range of petroleum ether is 60-90°C.

[0020] Furthermore, in the above step (5), the mixture is refrigerated at a low temperature of -20 to -60°C for 0.5 to 2 hours.

[0021] Beneficial effects of the present invention:

[0022] The preformed solvent synthesized by the present invention has the advantages of being easy to prepare, low in price, biodegradable and environmentally friendly, and has great advantages in removing lignin and cell wall anti-degradation barriers, which is beneficial to the removal of lignin in eucommia gum resources, and the staged reactions involved are beneficial to the penetration of organic solvents, thereby improving the extraction efficiency and yield of eucommia gum. Therefore, the core of the eucommia gum preparation method of the present invention is not to use common solvents to extract eucommia gum, but to use a method of pretreatment combined with organic solvent extraction to extract natural eucommia gum. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is a physical picture of the solid eucommia gum of Example 1;

[0024] Figure 2 For the solid eucommia gum of Example 1 1 H-NMR spectrum;

[0025] Figure 3 For the solid eucommia gum of Example 1 13 C-NMR spectrum;

[0026] Figure 4 This is the 2D-HSQC NMR graph of the solid eucommia gum of Example 1. DETAILED DESCRIPTION

[0027] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] In the following examples, the boiling range of petroleum ether is 60-90°C.

[0029] Example 1

[0030] The method for preparing eucommia gum with high efficiency and high yield comprises the following steps:

[0031] (1) mixing choline chloride and ethylene glycol in a molar ratio of 1:10 and heating them at a heating temperature of 80° C. for 30 minutes to obtain a preformed solvent;

[0032] (2) mixing the bark of Eucommia ulmoides with the pre-made solvent in a mass ratio of 1:20, the reaction temperature being 100° C., and the reaction time being 3 hours;

[0033] (3) adding petroleum ether to the reactants obtained in step (2) and mixing them, wherein the mass ratio of petroleum ether to Eucommia bark is 10:1, and performing a second stage reaction at a reaction temperature of 80° C. and a reaction time of 2 hours;

[0034] (4) separating the liquid component a and the solid residue in the product obtained after the reaction in step (3);

[0035] (5) allowing the liquid component a in step (4) to stand and separate into layers to obtain a petroleum ether layer rich in eucommia gum, refrigerating the petroleum ether layer rich in eucommia gum at -20°C for half an hour, and then centrifuging to obtain solid eucommia gum and petroleum ether, and collecting the petroleum ether for reuse;

[0036] (6) Add 5 times the volume of hydrochloric acid with a pH of 2 to obtain liquid b obtained by removing the petroleum ether layer rich in eucommia gum from the liquid component a in step (5), and then perform solid-liquid separation. The obtained liquid component c is concentrated by rotary evaporation to obtain the pre-made solvent for repeated use.

[0037] Example 2

[0038] The method for preparing eucommia gum with high efficiency and high yield comprises the following steps:

[0039] (1) mixing choline chloride and ethanolamine in a molar ratio of 1:1 and heating them at a temperature of 80° C. for 30 minutes to obtain a preformed solvent;

[0040] Steps (2) to (6) are the same as in Example 1.

[0041] Example 3

[0042] The method for preparing eucommia gum with high efficiency and high yield comprises the following steps:

[0043] (1) taking formic acid as the pre-made solvent;

[0044] Steps (2) to (6) are the same as in Example 1.

[0045] Example 4

[0046] The method for preparing eucommia gum with high efficiency and high yield comprises the following steps:

[0047] Step (1) is the same as in Example 1;

[0048] (2) mixing the bark of Eucommia ulmoides with the pre-made solvent in a mass ratio of 1:5, the reaction temperature is 100° C., and the reaction time is 1 hour;

[0049] Steps (3) to (6) are the same as in Example 1.

[0050] Example 5

[0051] The method for preparing eucommia gum with high efficiency and high yield comprises the following steps:

[0052] Step (1) is the same as in Example 1;

[0053] (2) mixing the Eucommia bark with the pre-made solvent in a mass ratio of 1:20, the reaction temperature is 80° C., and the reaction time is 1 hour;

[0054] Steps (3) to (6) are the same as in Example 1.

[0055] Example 6

[0056] The method for preparing eucommia gum with high efficiency and high yield comprises the following steps:

[0057] Step (1) is the same as in Example 1;

[0058] (2) mixing the bark of Eucommia ulmoides with the pre-made solvent in a mass ratio of 1:20, reacting at a reaction temperature of 80° C. for 3 hours;

[0059] Steps (3) to (6) are the same as in Example 1.

[0060] Example 7

[0061] The method for preparing eucommia gum with high efficiency and high yield comprises the following steps:

[0062] Steps (1)-(2) are the same as in Example 1;

[0063] (3) adding petroleum ether to the reactants obtained in step (2) and mixing them, wherein the mass ratio of petroleum ether to Eucommia bark is 5:1, and performing a second stage reaction at a reaction temperature of 70° C. and a reaction time of 3 hours;

[0064] Steps (4) to (6) are the same as in Example 1.

[0065] Example 8

[0066] The method for preparing eucommia gum with high efficiency and high yield comprises the following steps:

[0067] Steps (1)-(2) are the same as in Example 1;

[0068] (3) Then, petroleum ether was mixed with Eucommia bark in a mass ratio of 10:1, and then the second stage reaction was continued at a reaction temperature of 80° C. and a reaction time of 1 hour;

[0069] Steps (4) to (6) are the same as in Example 1.

[0070] Example 9

[0071] The method for preparing eucommia gum with high efficiency and high yield comprises the following steps:

[0072] Step (1) is the same as in Example 1;

[0073] (2) mixing the Eucommia ulmoides leaves with the pre-prepared solvent in a mass ratio of 1:20, the reaction temperature was 100° C., and the reaction time was 3 hours;

[0074] Steps (3) to (6) are the same as in Example 1.

[0075] Example 10

[0076] The method for preparing eucommia gum with high efficiency and high yield comprises the following steps:

[0077] Step (1) is the same as in Example 1;

[0078] (2) mixing the Eucommia ulmoides fruit with the pre-made solvent in a mass ratio of 1:20, the reaction temperature is 100° C., and the reaction time is 3 hours;

[0079] Steps (3) to (6) are the same as in Example 1.

[0080] Comparative Example 1

[0081] (1) mixing Eucommia bark and petroleum ether in a mass ratio of 1:20 for reaction at a reaction temperature of 80° C. for a reaction time of 5 hours;

[0082] (2) The liquid component petroleum ether (rich in eucommia gum) in step (1) is refrigerated at -20°C for half an hour, and then centrifuged to obtain solid eucommia gum and petroleum ether, and the petroleum ether is collected for reuse.

[0083] Comparative Example 2

[0084] (1) mixing Eucommia bark and petroleum ether in a mass ratio of 1:40, reacting at a reaction temperature of 80° C. for 5 hours;

[0085] (2) The liquid component petroleum ether (rich in eucommia gum) in step (1) is refrigerated at -20°C for half an hour, and then centrifuged to obtain solid eucommia gum and petroleum ether, and the petroleum ether is collected for reuse.

[0086] Comparative Example 3

[0087] (1) Step (1) is the same as in Example 1;

[0088] (2) mixing the Eucommia bark with the pre-made solvent at a mass ratio of 1:20 and with petroleum ether at a mass ratio of 1:10;

[0089] (3) reacting the mixture of step (2) at a reaction temperature of 80° C. for 8 hours;

[0090] (4) separating the liquid component a and the solid residue in the product obtained after the reaction in step (3);

[0091] (5) The liquid component a in step (4) is allowed to stand for stratification to obtain a petroleum ether layer rich in eucommia gum, the petroleum ether layer rich in eucommia gum is refrigerated at -20°C for half an hour, and then centrifuged to obtain solid eucommia gum.

[0092] Table 1 Comparison of the yield of Eucommia gum obtained in the examples and comparative examples

[0093] sample Solid eucommia gum yield Example 1 96.2% Example 2 92.4% Example 3 94.0% Example 4 91.6% Example 5 85.7% Example 6 92.1% Example 7 90.2% Example 8 92.4% Example 9 94.5% Example 10 94.7% Comparative Example 1 50.2% Comparative Example 2 64.3% Comparative Example 3 72.7%

[0094] The disclosed embodiments are described to enable one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A method for preparing eucommia gum with high efficiency and high yield, characterized in that: The steps include: (1) mixing choline chloride with ethylene glycol, formic acid or ethanolamine in a molar ratio of 1:10 and heating them at a heating temperature of 80° C. for 30 minutes to obtain a preformed solvent; (2) mixing the Eucommia biomass raw material with the pre-made solvent in a ratio of 1:20 to carry out a first-stage reaction at a reaction temperature of 100° C. for a reaction time of 3 h; (3) adding petroleum ether to the reactants obtained in step (2) and mixing them, wherein the mass ratio of petroleum ether to the Eucommia biomass raw material is 10:1, and performing a second stage reaction at a reaction temperature of 80° C. and a reaction time of 2 hours; (4) separating the liquid component a and the solid residue in the product obtained after the reaction in step (3); (5) allowing the liquid component a in step (4) to stand for stratification to obtain a petroleum ether layer rich in eucommia gum, refrigerating the petroleum ether layer rich in eucommia gum at low temperature, and then centrifuging to obtain solid eucommia gum and petroleum ether, and collecting the petroleum ether for reuse; (6) adding 5 times the volume of pH=2 acidic aqueous solution to obtain liquid b after removing the petroleum ether layer rich in eucommia gum from the liquid component a in step (5), and then performing solid-liquid separation. After rotary evaporation and concentration, the obtained liquid component c is again obtained to obtain the pre-made solvent for repeated use.

2. The method for preparing eucommia gum with high efficiency and high yield according to claim 1, characterized in that: The Eucommia ulmoides biomass in step (1) is one or more of Eucommia ulmoides bark, Eucommia ulmoides leaves or Eucommia ulmoides winged fruit.

3. The method for preparing eucommia gum with high efficiency and high yield according to claim 1, characterized in that: In the step (1), the pre-made solution is ready for use, and in the step (3), the boiling range of petroleum ether is 60-90°C.

4. The method for preparing eucommia gum with high efficiency and high yield according to claim 1, characterized in that: In the step (5), the mixture is refrigerated at a low temperature of -20 to -60°C for 0.5 to 2 hours.