Can for foaming beverage and method for producing the same

By forming a specific concave structure and resin layer on the inner surface of the foamable beverage can, the problem of insufficient foaming when opening the can in the prior art is solved, and higher foaming properties and larger foaming volume are achieved, satisfying the satisfaction of User requirements.

CN116670038BActive Publication Date: 2024-11-05ASAHI GRP HLDG LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180087872.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-11-16
Filing Date
2021-12-27
Publication Date
2024-11-05
Estimated Expiration
2041-12-27

AI Technical Summary

Technical Problem

The existing cans for foaming beverages have insufficient foaming properties when opening the can, making it difficult to meet the user's demand for appropriate foaming.

Method used

A specific structure is formed on the inner surface of the tank, including a first recess with a diameter of 5 μm or more and 20 μm or less and a second recess with a diameter of 0.5 μm or more and less than 5 μm. A resin layer is applied thereon, and a wax is made by heating treatment The recess is formed by disengaging, thereby improving foaming properties.

Benefits of technology

It significantly improves the degassing and coverage of foamed beverages, ensuring that users can enjoy a larger amount of foam and liquid when opening the can, and at the same time improves the design of the can lid to facilitate the enjoyment of foam and liquid at one time.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116670038B_ABST
    Figure CN116670038B_ABST
Patent Text Reader

Abstract

The can for a foaming beverage comprises: a surface, a lower surface and a main body, wherein a plurality of first recesses having a diameter of 5 μm or more are provided on the inner surface of the main body, and the number of the plurality of first recesses is 1 mm 2 The number of pcs is between 200 and 2000.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a can for a foaming beverage and a method for producing the same. Background Art

[0002] Sparkling beverages such as beer are sometimes provided in a sealed container. One of the important characteristics of sparkling beverages is the foaming property. Various studies have been conducted to obtain an appropriate amount of foam when drinking.

[0003] In order to improve the foaming property, it is also known to work on the structure of the container. For example, Patent Document 1 (Japanese Patent No. 4758693) discloses a technology for the purpose of providing a can for a foaming beverage that has no adverse effect on the filling property and can well improve the foaming property when the can is opened. Patent Document 1 records the following aspects: in the can for a foaming beverage, an organic resin coating layer is provided on the inner surface of the can; an organic resin coating material mixed with a specified large-diameter particle in a specified amount accounts for more than 20% and less than 60% of the inner surface area of ​​the aforementioned can, and an organic resin coating material mixed with a specified small-diameter particle in a specified amount accounts for the remainder of the inner surface area of ​​the aforementioned can; and a concave portion or convex portion caused by the detachment of at least a part of the large-diameter particle, and a concave portion caused by the detachment of the small-diameter particle are formed in the organic resin coating layer.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent No. 4758693 Summary of the invention

[0007] The present inventors have considered that the foaming property needs to be further improved. Therefore, an object of the present invention is to provide a can for a sparkling beverage and a method for producing the can, which can further improve the foaming property.

[0008] The inventors of the present invention have found that the above-mentioned problems can be solved by forming a predetermined structure on the inner surface of a tank, and have arrived at the present invention. That is, the present invention is achieved by the following means.

[0009] [1] A can for a foaming beverage, comprising: an upper surface, a lower surface, and a main body;

[0010] A plurality of first recesses having a diameter of 5 μm or more and 20 μm or less are provided on the inner surface of the main body.

[0011] The number of the plurality of first recesses is 1 mm 2 The number of pcs is between 200 and 2000.

[0012] [2] The foaming beverage can according to [1], wherein a plurality of second recesses having a diameter of not less than 0.5 μm and less than 5 μm are provided on the inner surface of the main body.

[0013] The number of the plurality of second recesses is 1 mm 2 The number of pcs in the middle ranges from 5,000 to 20,000.

[0014] [3] The can for a sparkling drink according to [1] or [2], wherein a resin layer is provided on the inner surface of the body.

[0015] The first recessed portion is formed in the resin layer.

[0016] [4] The can for a sparkling beverage according to any one of [1] to [3], wherein the upper surface is formed by a can lid configured to be opened in a fully open state.

[0017] [5] A method for manufacturing a can for a sparkling beverage, the can having an upper surface, a lower surface, and a body, the method comprising the following steps:

[0018] The step of applying a coating containing resin and wax to the inner surface of the main body or a predetermined area to be the inner surface of the main body; and

[0019] The step of heating the applied coating to form a resin layer and remove the wax.

[0020] The average particle size of the wax in the coating is 1 μm or more.

[0021] The content of the wax is 7 to 40 parts by mass based on 100 parts by mass of the nonvolatile components (excluding the wax) in the coating material.

[0022] [6] The production method according to [5], wherein the wax comprises polyethylene wax.

[0023] [7] The production method according to [5] or [6], wherein the coating material comprises at least one resin selected from the group consisting of epoxy resins, acrylic resins, polyester resins, and polyurethane resins.

[0024] [8] A foaming beverage comprising:

[0025] The beverage can according to any one of [1] to [4], and

[0026] A foamable drinkable liquid filled into the beverage can.

[0027] According to the present invention, there are provided a can for a sparkling beverage having further improved foaming properties and a method for producing the same. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 The figure is a cross-sectional view schematically showing a pit-like structure.

[0029] Figure 2 It is a cross-sectional view schematically showing a method of forming a pit-like structure.

[0030] Figure 3A This is a microscopic photograph showing the inner surface of the main body portion of the control area.

[0031] Figure 3B This is a microscope photograph showing the inner surface of the main body of the test area 1.

[0032] Figure 3C This is a microscope photograph showing the inner surface of the main body of the test area 2.

[0033] Figure 4A It is a figure which shows the 3D image of the inner surface of the main body part of a control area.

[0034] Figure 4B This is a diagram showing a 3D image of the inner surface of the main body of the test area 1 .

[0035] Figure 4C This is a diagram showing a 3D image of the inner surface of the main body of the test area 2.

[0036] Figure 5A It is a diagram showing the measurement positions of the profile of the surface of the test area 2.

[0037] Figure 5B 3 is a diagram showing the measurement results of the surface profile of the test area 2. DETAILED DESCRIPTION

[0038] Hereinafter, embodiments of the present invention will be described in detail.

[0039] The can for foaming beverages of this embodiment has an upper surface, a main body and a lower surface. The main body and the lower surface are in an integrated or joined state and have a bottomed cylindrical shape, and the upper opening is closed in a manner that can be opened from the upper surface.

[0040] A plurality of first recesses are provided on the inner surface of the main body.

[0041] It should be noted that in this specification, a "concave portion" refers to a structure having a depth of 1 μm or more.

[0042] The first recessed portion has a substantially circular shape when viewed from the front. The first recessed portion has a diameter of 5 μm or more and 20 μm or less.

[0043] Number of first concave parts per 1 mm 2The number of the plurality of nanoparticles is 200 to 2000, preferably 300 to 1500, more preferably 400 to 1200.

[0044] The average depth of the plurality of first recessed portions is, for example, 1 to 5 μm, or preferably 2 to 4 μm.

[0045] It should be noted that the number and average depth of the first recessed portions can be obtained using, for example, a laser microscope.

[0046] The first recessed portion is preferably a pit-shaped structure. Figure 1 FIG. 2 is a cross-sectional view schematically showing a pit-like structure. Figure 1 As shown, the pit-like structure refers to a structure in which the edge portion of the concave portion is raised inversely.

[0047] In this embodiment, preferably, a plurality of second recesses are further provided on the inner surface of the main body. The second recesses are recesses having a diameter of 0.5 μm or more and less than 5 μm.

[0048] The number of the second recessed portions per 1 mm 2 The number of the plurality of nanoparticles is 5,000 to 20,000, preferably 7,000 to 15,000.

[0049] The average depth of the plurality of second recessed portions is, for example, 1 to 5 μm, or preferably 2 to 4 μm.

[0050] The number and average depth of the second recesses can be determined by the same method as that of the first recesses.

[0051] Similar to the first recessed portion, the second recessed portion is also preferably a pit-shaped structure.

[0052] The can for a sparkling beverage of the present embodiment is preferably made of metal. In addition, a resin layer obtained by applying and drying a paint on a metal layer is preferably provided on the inner surface of the main body, and the first and second recesses are formed in the resin layer.

[0053] The thickness of the resin layer is, for example, 1 to 10 μm, or preferably 3 to 8 μm.

[0054] In the present invention, the "resin layer" refers to a layer obtained after the applied paint is dried, and should be distinguished from the layer of the paint before drying.

[0055] The can lid of the can for a foaming beverage of the present embodiment is preferably a fully open end. A fully open end refers to a type of lid in which 30% or more of the area of ​​the top surface of the can lid is open. The open area is preferably 50% or more of the top surface of the can lid, more preferably 90% or more, and even more preferably the entire top surface of the can lid.

[0056] A preferred embodiment is, for example, a type of lid in which the entire circumference of the top surface of the circular can lid is scored (cut), and the entire top surface of the lid is separated from the can body and opened. On the other hand, a part of the lid may remain on the can body without the lid being completely separated. Compared with a conventional can lid, the fully open end can visually capture the foaming from the can body, thus causing a reminder of beer poured into a large beer glass. In addition, the amount of liquid flowing into the mouth at the same angle is greater than that of a conventional can lid, so that both the foam and the liquid can be enjoyed at once.

[0057] The capacity of the can for a sparkling beverage (the amount of the beverage liquid filled) is, for example, 135 to 1000 ml, and preferably 320 to 500 ml.

[0058] When the lid is circular, the diameter of the can for a sparkling drink is, for example, 200 to 211 dia., preferably 202 to 206 dia.

[0059] Next, an example of a method for producing the above-mentioned sparkling drink can will be described.

[0060] The manufacturing method of this embodiment includes the following steps: a step of applying a coating containing resin and wax on the inner surface of the main body (or a predetermined area of ​​the inner surface of the main body); and, then, a step of heating the applied coating to form a resin layer on the inner surface to remove the wax (hereinafter also referred to as a sintering step).

[0061] According to this method, the wax is released, thereby forming the recessed portion in the resin layer.

[0062] It should be noted that wax is generally used for the purpose of preventing scratches on the coating film in the canning process, but in this specification, wax refers to a component in the form of solid particles at room temperature.

[0063] As a method for forming a can body having a resin layer on the inner surface, for example, a method can be mentioned in which a can body having a bottomed cylindrical shape is formed in advance by deep drawing and ironing, and then the coating of the present invention is applied by spray coating and sintered to form a resin layer (the obtained can is called a two-piece can). Alternatively, a method can be used in which a metal plate having a predetermined area to become an inner surface is prepared, and the coating is applied to the predetermined area to become the inner surface and sintered to form a resin layer, and then the metal plate having the resin layer is formed into a cylindrical shape and rolled up to form a can bottom of the lower surface to obtain a can body having a bottomed cylindrical shape (the obtained can is called a three-piece can).

[0064] Hereinafter, the coating and baking steps of the paint will be described in detail.

[0065] First, a coating comprising resin and wax is prepared.

[0066] As the paint, for example, a water-based paint can be used.

[0067] As the resin contained in the coating material, for example, epoxy resin, acrylic resin, polyester resin, polyurethane resin or the like is used.

[0068] The wax in the coating is a wax having an average particle size of 1 μm or more. The average particle size here refers to the particle size (D50) at which the frequency accumulation is 50% in terms of volume conversion, and is a value obtained by measuring an aqueous dispersion containing about 20% by mass of wax diluted 500 times with water using a dynamic light scattering particle size distribution measuring device ("Microtrac S3500" manufactured by Nikkiso Co., Ltd.).

[0069] The average particle size of the wax is preferably 1 to 15 μm, more preferably 2 to 10 μm, and further preferably 3 to 8 μm.

[0070] The content of the wax in the coating is, for example, 7 to 40 parts by mass, preferably 10 to 40 parts by mass, and more preferably 12 to 30 parts by mass, relative to 100 parts by mass of the nonvolatile components (excluding wax) in the coating. It should be noted that the nonvolatile components (excluding wax) referred to herein are components that remain on the adherend to form a resin layer after the coating is applied and sintered, excluding the wax.

[0071] In addition, a plurality of waxes having different average particle sizes may be used in combination. By combining a plurality of waxes having such different average particle sizes, it becomes easy to control the size and number of the recessed portions.

[0072] As the wax, for example, a wax having a softening point of 90 to 160°C, preferably 110 to 140°C is used.

[0073] As the wax, carnauba wax, polyethylene wax, and the like can be used.

[0074] As the form of the wax, those in the form of powder / paste / water or solvent dispersion can be suitably used. From the viewpoint of dispersion stability in the coating material, those in the form of water or solvent dispersion are preferably used.

[0075] The coating method of the coating material in the present embodiment is preferably spray coating such as air spray, airless spray, electrostatic spray, roll coater coating, dip coating, electrodeposition coating, etc., and more preferably spray coating.

[0076] In order to dry the coating material and form a uniform resin layer, it is preferred to perform a calcination treatment promptly after coating.

[0077] The conditions in the sintering step can be appropriately selected so as to dry the coating and form the resin layer, but preferably the sintering step is performed at 150 to 280° C. for 10 seconds to 30 minutes. In addition, the sintering step is performed at 180 to 280° C. for 1 minute to 30 minutes because the wax melts during sintering to cause separation from the coating film. The thickness of the resin layer after sintering is, for example, 1 to 10 μm, preferably 3 to 8 μm.

[0078] Figure 2 FIG. 2 is a cross-sectional view schematically showing a method for forming a pit-like structure. Figure 2 As shown, by applying and drying the coating, water and solvent are first volatilized to form the resin layer 1. Here, the wax 2 is temporarily embedded in the resin layer 1. In addition, the upper part of the wax 2 is exposed on the surface of the resin layer 1. Then, during sintering, the wax 2 melts and is separated from the resin layer 1. As a result, a concave portion of a pit-like structure is formed in the resin layer 1.

[0079] Thereafter, a beverage can is manufactured in the same manner as a method generally used in the art, and the can is filled with a drinkable liquid and sealed.

[0080] The filling of the drinkable liquid is preferably performed at a low temperature (eg, 1 to 20° C.).

[0081] According to the above method, by using a coating material containing a wax having a specific average particle size in a specific amount, recesses of a specific size are formed on the inner surface of the main body at a specific density. Furthermore, by using such a special structure, the can for a foaming beverage formed on the main body at a specific density can exhibit extremely high foaming properties.

[0082] In addition, the drinking liquid filled in the can for sparkling beverages of this embodiment is not particularly limited as long as it is a sparkling liquid.

[0083] The drinking liquid to be filled is preferably a beer-like sparkling beverage. "Beer-like sparkling beverage" refers to a sparkling beverage that has a flavor / taste and texture that is equal to or similar to beer, and has a high thirst-quenching feeling / easy drinkability (the property of not feeling overly full even if you continue to drink multiple cups), regardless of whether the alcohol content, malt and hops are used, or whether fermentation is performed. The beer-like sparkling beverage can be an alcoholic beverage, or a so-called non-alcoholic beverage or low-alcohol beverage with an alcohol content of less than 1% by volume. In addition, it can be a beverage using malt as a raw material, a beverage not using malt as a raw material, a fermented beverage manufactured through a fermentation process, or a non-fermented beverage manufactured without a fermentation process.

[0084] Specific examples of beer-like sparkling beverages include beer, sparkling liquor made from malt, sparkling alcoholic beverages not using malt, low-alcohol sparkling beverages, non-alcoholic beer, etc. In addition, liqueurs obtained by mixing a beverage made from malt as a raw material and through a fermentation process with an alcohol-containing distillate may also be used.

[0085] More preferably, the drinking liquid filled is beer. When the can for a sparkling beverage of the present embodiment is filled with beer, bubbles are generated from the inner surface of the can when the tap is opened, and the bubbles and the beer can be drunk at the same time.

[0086] However, when a beverage other than beer is filled, the aroma component also evaporates along with the foaming, so the flavor of the content can be strongly felt.

[0087] Preferably, the gas pressure of the foaming beverage is 2 to 4 gas volumes.

[0088] Example

[0089] Hereinafter, the present invention will be described in more detail, and thus examples performed by the present inventors will be described.

[0090] (Control Area)

[0091] An aluminum container (350 ml volume) having a lower surface and a main body was prepared. In addition, a water-based epoxy acrylic paint containing 1 mass part of carnauba wax with an average particle size of 0.3 μm relative to 100 mass parts of non-volatile components (excluding wax) in the paint was prepared. The prepared paint was applied to the entire inner surface of the main body of the container by spray coating, and then heated at 200° C. for 2 minutes to obtain a beverage can in the control area. The thickness of the main body resin layer was 5 μm on average.

[0092] (Test Area 1)

[0093] As the wax, 7.5 parts by mass of wax with an average particle size of 6 μm was used with respect to 100 parts by mass of the nonvolatile components (excluding wax) in the coating material. In the same manner as in the control group, a beverage can of Example 1 was obtained.

[0094] (Test Area 2)

[0095] The waxes used were a wax having an average particle size of 6 μm (first wax) and a wax having an average particle size of 4 μm (second wax). The amount of the first wax was 7.5 parts by mass relative to 100 parts by mass of the nonvolatile components (excluding the wax) in the coating. The amount of the second wax was 7.5 parts by mass relative to 100 parts by mass of the nonvolatile components (excluding the wax) in the coating.

[0096] Beverage cans for the test group 2 were obtained in the same manner as in the control group in other respects.

[0097] (Determination of degassing amount)

[0098] 350 ml of beer was quietly poured into each prepared beverage can and the mass was measured. After that, the mass was measured again after standing for 5 minutes. The difference between the mass before and after standing for 5 minutes was calculated as the "degassing amount". For each beverage can, every 5 cans were measured. The upper limit and lower limit of the degassing amount measured value of each beverage can are shown in the following Table 1.

[0099] [Table 1]

[0100] Control area Test Area 1 Test Area 2 Degassing volume (g) 0.01~0.02 0.21~0.26 0.29~0.34

[0101] As shown in Table 1, the degassing amount of test area 1 and test area 2 is significantly greater than that of the control area. In addition, the degassing amount of test area 2 is further greater than that of test area 1. The degassing amount indicates the amount of gas removed (the size of the bubbles), that is, the larger the value, the higher the foaming property (the larger the bubbles).

[0102] (Coverage Evaluation)

[0103] Each prepared beverage can was filled with beer, and the upper surface was sealed with a fully opened can lid. After filling, the beverage can was left to stand at 4°C for 24 hours. Then, the coverage time (the time from opening the can stopper, bubbles appearing in the beverage can, and the time from the top of the beverage can being hidden by the bubbles) was set to 10 seconds, and the coverage was evaluated. For each beverage can, 10 cans were tested, and the number of cans with a coverage time of less than 10 seconds was counted. The results are shown in Table 2.

[0104] [Table 2]

[0105]

[0106] As shown in Table 2, the coverage was also greater in the order of test plot 2, test plot 1, and control plot. The evaluation results of the coverage also showed that test plots 1 and 2 were superior to the control plot, and test plot 2 was particularly superior.

[0107] (Measurement of surface conditions)

[0108] The surface condition of the inner surface of the main body of each beverage can obtained was observed. Specifically, an image of the inner surface of the main body was obtained using a laser microscope VK-X3000 (manufactured by KEYENCE CORPORATION) equipped with a white interferometer. Figure 3A to Figure 3C The images obtained for the control area, test area 1, and test area 2 are shown in FIG. Figure 4A to Figure 4C 3D images of the images obtained for the control area, test area 1, and test area 2 are shown in FIG.

[0109] In addition, for test area 2, the profile of the surface was measured. Figure 5A is a diagram showing the measurement position of the surface profile. Figure 5A The line segments shown measure the surface profile. Figure 5B is a diagram showing the measurement results of the surface profile. Figure 5B The horizontal axis represents the position, and the vertical axis represents the height (depth) from the baseline.

[0110] Furthermore, based on the obtained image, the number of concave portions with a diameter of 5 μm or more (first concave portion) and the number of concave portions with a diameter of 1 μm or more and less than 5 μm (second concave portion) were counted using a laser microscope VK-X3000 (manufactured by KEYENCE CORPORATION) equipped with a white interferometer, and the number of concave portions with a diameter of 1 μm or more and less than 5 μm (second concave portion) was calculated. 2 The number of in .

[0111] When counting the number of recessed portions, the number of recessed portions having a depth of 1 μm or more from the base line was counted.

[0112] The results are shown in the following Table 3. The maximum diameter of the structure counted as the first recessed portion was 8.8 μm.

[0113] [Table 3]

[0114]

[0115] (About the summary of the results)

[0116] The first concave part is 1 mm 2 Compared with the control area where no first concave portion was found, the test area 1 and the test area 2, which had 200 to 2000 concave portions, showed a large degassing amount and coverage, and a high foaming property. 2 The foaming property of the test area 2 with a molecular weight of 7,000 to 15,000 was higher.

[0117] Description of Reference Numerals

[0118] 1 Resin layer

[0119] 2 Wax

Claims

1. A can for a foaming beverage, comprising: an upper surface, a lower surface and a main body, A first recess and a second recess are provided on the inner surface of the main body. The diameter of the first recess is 5 μm or more and 20 μm or less, and the number of the first recesses is 1 mm. 2 200 to 1200 in China. The diameter of the second recess is 0.5 μm or more and less than 5 μm, and the number of the second recesses is 1 mm. 2 The number is between 7,000 and 15,000.

2. The can for a foaming beverage according to claim 1, wherein: The number of the first recessed portions is 1 mm 2 256 to 768 in The number of the second recessed portions is 1 mm 2 The number of digits in the middle ranges from 7000 to 9552.

3. The can for a foaming beverage according to claim 1, wherein: The diameter of the first recess is not less than 5 μm and not more than 8.8 μm.

4. The can for a foaming beverage according to claim 1, wherein: A resin layer is provided on the inner surface of the main body. The first recessed portion and the second recessed portion are formed in the resin layer.

5. The can for a sparkling drink according to any one of claims 1 to 4, wherein The upper surface is formed by a can lid configured to be opened in a fully open configuration.

6. A sparkling beverage comprising: the sparkling beverage can according to claim 5, and a drinkable liquid filled in the sparkling beverage can, By opening the stopper, the drinkable liquid is foamed so that the upper end of the can for sparkling beverage is hidden.

7. The foaming beverage according to claim 6, wherein The drinkable liquid is a beer flavored beverage.