Preparation method of copper nanoparticle / flaky fullerol nanocomposite material and its antibacterial application

Copper nanoparticle/sheet-shaped fullerol composite material was prepared by liquid-liquid interface precipitation method and light reduction method, which solved the problems of fullerene derivatives being easily agglomerated and highly hydrophobic, and achieved efficient inhibition of bacteria, especially The antibacterial effect is significantly improved under light conditions.

CN116672362BActive Publication Date: 2024-11-05JIANGNAN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310615028.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-26
Publication Date
2024-11-05
Estimated Expiration
2043-05-26

AI Technical Summary

Technical Problem

The existing fullerene derivatives are prone to agglomeration and have strong hydrophobicity, which limits their application in the field of biomedicine and is difficult to control their morphology to improve antibacterial properties.

Method used

Flat-shaped fullerol was prepared by liquid-liquid interface precipitation method, and copper nanoparticles were uniformly grown on its surface by light reduction method to form copper nanoparticles/flat-shaped fullerol composite material.

Benefits of technology

By controlling the morphology of fullerol and the uniform growth of copper nanoparticles, the antibacterial properties of the composite material are improved, and bacterial growth can be effectively inhibited, especially the production of superoxide and hydroxyl radicals under light conditions, which significantly improves the gold resistance Inhibition rate of Staphylococcus aureus and E. coli.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116672362B_ABST
    Figure CN116672362B_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a copper nanoparticle / flaky fullerol nanocomposite material and its antibacterial application, belonging to the technical field of nanomaterials. The invention uses fullerene as a matrix, performs hydroxylation modification on fullerene to obtain fullerol, regulates the morphology of fullerol to obtain a flake fullerol cluster, reduces copper ions in copper chloride to copper nanoparticles by laser photoreduction and stably loads them on the surface of the flake fullerol cluster, and prepares a copper nanoparticle / fullerol composite material. The method of the invention is simple and efficient, and the obtained copper nanoparticle / flaky fullerol composite material has a small particle size and uniform distribution, and exhibits good antibacterial activity against Staphylococcus aureus and Escherichia coli, solves the problem that the antibacterial performance of a single fullerene derivative is not strong, and has good application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a preparation method of a copper nanoparticle / flaky fullerol nanocomposite material and its antibacterial application, belonging to the technical field of nanomaterials. Background Art

[0002] In recent years, bacterial infections have posed a severe challenge to public health and imposed a heavy burden on patients. Due to the long-term abuse of antibiotics, bacteria have evolved complex resistance mechanisms to avoid being killed by antimicrobial molecules, and some bacteria are even able to use a series of resistance mechanisms to inhibit the effects of antibiotics. Therefore, there is an urgent need to find new bactericides and develop antibiotic-free synergistic antibacterial methods.

[0003] Fullerene is a sp 2 Hollow clusters of carbon atoms with hybrid structures usually contain 60 completely equivalent carbon atoms arranged in 20 six-membered rings and 12 five-membered rings, which have good photoactivity and excellent chemical reactivity. Since fullerene itself is non-cytotoxic and can produce 1 O2 kills bacteria, so its application in the biomedical field has been widely explored. The antibacterial activity of fullerene and its derivatives can be attributed to two aspects. On the one hand, the interaction between fullerene and biological molecules causes the cell membrane / wall to rupture to inhibit its respiratory chain and prevent bacterial growth; on the other hand, fullerene produces superoxide and hydroxyl free radicals or 1 O2, these reactive oxygen species (ROS) can cause more than 99.9% of bacterial and fungal cell death. However, fullerenes are easy to aggregate and have strong hydrophobicity. They are only soluble in limited organic solvents (such as toluene, carbon tetrachloride, etc.), which limits their application in the biomedical field. Although we have enhanced its solubility by grafting hydrophilic groups, it is still very easy to aggregate. The surface morphology can affect its performance in generating ROS to a certain extent. Therefore, we want to improve the antibacterial properties of fullerene derivatives by controlling the specific morphology of fullerene derivatives.

[0004] Copper nanoparticles (CuNPs) have become one of the most commonly used antibacterial agents due to their high redox potential, relatively low production cost, and broad-spectrum antibacterial activity. Based on the above advantages, we thought of anchoring CuNPs on the surface of fullerene derivatives with controlled morphology to form a new composite antibacterial material. Therefore, how to control the morphology and size of fullerene derivatives through a simple and effective method and load copper nanoparticles on the surface of derivatives with specific morphology is a key issue to further achieve the synergistic antibacterial effect of the two. Summary of the invention

[0005] In order to solve the above problems, the present invention first provides a method for preparing a copper nanoparticle / flaky fullerol composite material. First, the morphology of fullerol is controlled by a liquid-liquid interface precipitation method (LLIP), and then the copper nanoparticles are uniformly grown on the surface of the flake fullerol by a light reduction method. The prepared composite material can be applied to the antibacterial field.

[0006] A method for preparing a copper nanoparticle / flaky fullerol composite material, the method comprising the following steps:

[0007] (1) dispersing fullerene in an organic solvent to prepare a fullerene dispersion, then adding peroxide and tetrabutylammonium hydroxide to carry out a solvothermal reaction, and after the reaction is completed, standing and stratifying, collecting the lower liquid phase, and then adding a precipitant to separate the solid and liquid, collecting the solid, and drying to obtain a fullerol powder;

[0008] (2) dispersing fullerol powder in a good solvent with good solubility, adding a poor solvent with relatively poor solubility for fullerol to the fullerol dispersion at a constant rate, and then sealing and incubating at room temperature for a period of time to obtain a flake fullerol dispersion;

[0009] (3) mixing the divalent copper salt with the flake fullerol dispersion obtained in step (2) to obtain a mixed solution, which is then placed under laser irradiation. After the irradiation, the solid-liquid separation is performed, and the solid is collected and dried to obtain a copper nanoparticle / flake fullerol composite material.

[0010] In one embodiment of the present invention, the organic solvent in step (1) is toluene.

[0011] In one embodiment of the present invention, the mass volume ratio of fullerene to organic solvent in step (1) is (1.5-3): 1 (mg / mL);

[0012] In one embodiment of the present invention, the peroxide in step (1) comprises any one or more of the following: 30% hydrogen peroxide, tert-butyl hydroperoxide, dibenzoyl peroxide, and potassium permanganate.

[0013] In one embodiment of the present invention, the volume ratio of the organic solvent, peroxide and tetrabutylammonium hydroxide in step (1) is 100:20:1 (mL).

[0014] In one embodiment of the present invention, the temperature range of the solvent thermal reaction in step (1) is 50°C-80°C; and the time is 12h-20h.

[0015] In one embodiment of the present invention, the stratification in step (1) is an upper transparent liquid phase and a lower dark yellow liquid phase.

[0016] In one embodiment of the present invention, the precipitant in step (1) comprises any one or more of isopropanol, anhydrous ether, and n-hexane. When the three are mixed, the volume ratio of isopropanol, anhydrous ether, and n-hexane is 7:5:5.

[0017] In one embodiment of the present invention, the solid-liquid separation in step (1) further comprises: after adding a precipitant for separation, adding a detergent to continue separation, and finally collecting a solid product.

[0018] In one embodiment of the present invention, step (1) further comprises washing the solid after collection, and the washing agent is anhydrous ether.

[0019] In one embodiment of the present invention, the centrifugal speed in step (1) is 8000 rpm and the centrifugal time is 8 min.

[0020] In one embodiment of the present invention, the drying in step (1) is performed using a vacuum oven with a vacuum degree of -1 MPa and a drying temperature of 25°C.

[0021] In one embodiment of the present invention, the good solvent in step (2) is dimethyl sulfoxide.

[0022] In one embodiment of the present invention, the mass volume ratio of fullerol powder to good solvent in step (2) is (0.5-1):1 (mg / mL); specifically, 1:1 (mg / mL) can be selected.

[0023] In one embodiment of the present invention, the poor solvent in step (2) is acetone.

[0024] In one embodiment of the present invention, the volume ratio of the good solvent to the poor solvent in step (2) is 3:1.

[0025] In one embodiment of the present invention, the rate of adding the poor solvent in step (2) is 200 μL / s.

[0026] In one embodiment of the present invention, the incubation time in step (2) is 8-24 hours, and 18 hours is specifically selected.

[0027] In one embodiment of the present invention, the divalent copper salt in step (3) is selected from the group consisting of: copper chloride, copper chloride dihydrate, copper nitrate, copper nitrate hydrate, copper carbonate, copper carbonate hydrate, copper sulfate, and copper sulfate hydrate.

[0028] In one embodiment of the present invention, the mass ratio of the flake fullerol to the divalent copper salt in step (3) is 1:3 to 1:4; preferably, the mass ratio is 1:3.3.

[0029] In one embodiment of the present invention, in step (3), a certain amount of water is further added to the mixed solution, and the volume ratio of water to the flake fullerenol dispersion is (10-20):8; specifically, 15:8 can be selected.

[0030] In one embodiment of the present invention, in step (3), the mass concentration of the flake fullerenol in the mixed solution is 0.05-0.2 mg / mL; specifically, 0.09 mg / mL can be used.

[0031] In one embodiment of the present invention, the wavelength of the laser in step (3) is 660 nm, and the excitation energy is 0.9 mW / cm 2 .

[0032] In one embodiment of the present invention, the solid-liquid separation in step (3) is performed by centrifugation, the centrifugal speed is 8000 rpm, and the centrifugal time is 6 minutes.

[0033] In one embodiment of the present invention, the drying in step (3) is performed using a vacuum oven with a vacuum degree of -1 MPa and a drying temperature of 50°C.

[0034] In one embodiment of the present invention, the method specifically includes the following process:

[0035] (1) dispersing fullerene in a toluene solvent to form a toluene dispersion, then adding 30% hydrogen peroxide and tetrabutylammonium hydroxide solution, mixing, stirring and heating; separating the upper and lower layers of the obtained mixed solution, taking the lower liquid phase and adding a precipitant and a detergent thereto, and then centrifuging, decanting and drying to obtain a fullerol powder;

[0036] (2) dissolving the fullerol powder obtained in step (1) in dimethyl sulfoxide, and then injecting acetone at a constant rate, sealing the obtained mixture and incubating it at room temperature for a period of time to obtain a flake fullerene dispersion;

[0037] (3) The flaky fullerol dispersion obtained in step (2) and copper (II) chloride dihydrate are prepared into a mixed solution in a certain ratio, and the solution is fully illuminated under a laser to coat the copper nanoparticles on the surface of the fullerol through photoelectron conversion. The solution is then centrifuged, decanted and dried to obtain a copper nanoparticle / flaky fullerol composite material in which the copper nanoparticles are well and evenly coated on the flaky fullerol.

[0038] The invention provides a copper nanoparticle / flaky fullerol composite material obtained by the method.

[0039] In one embodiment of the present invention, the particle size of the copper nanoparticle / flaky fullerol composite material is about 160 nm.

[0040] The present invention also provides an antibacterial agent, which comprises the copper nanoparticle / flaky fullerol composite material.

[0041] The present invention also provides an antibacterial method, wherein the copper nanoparticle / flaky fullerol composite material is used as an antibacterial agent for antibacterial treatment.

[0042] In one embodiment of the present invention, the antibacterial method or antibacterial agent is applicable to Staphylococcus aureus and Escherichia coli.

[0043] Beneficial effects of the present invention:

[0044] The present invention prepares flake fullerol by a simple means (liquid-liquid precipitation method), and controls the size of the flake fullerol to be about 160nm by adjusting the reaction conditions. The copper nanoparticles are uniformly grown on the surface of the flake fullerol by a light reduction method, and the coated copper nanoparticles have a smaller particle size. The copper nanoparticle / flake fullerol composite material prepared by the present invention can be used for antibacterial purposes, and can generate superoxide, hydroxyl radicals or 1 O2, thus playing an antibacterial role. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] Figure 1 This is the infrared spectrum (FT-IR) spectrum of fullerenol.

[0046] Figure 2 This is the thermogravimetric curve (TGA) of fullerene alcohol.

[0047] Figure 3 This is a scanning electron microscope (SEM) image of the copper nanoparticle / flaky fullerol composite material.

[0048] Figure 4 These are X-ray photoelectron spectroscopy (XPS) diagrams of copper nanoparticle / flaky fullerol nanocomposites, where (a) is the XPS spectrum of the composite material; (b) is the C1s XPS spectrum; (c) is the O1s XPS spectrum; and (d) is the Cu 2p XPS spectrum.

[0049] Figure 5 This is the particle size test curve of fullerol and copper nanoparticles / flaky fullerol composite material.

[0050] Figure 6 This is the particle size analysis diagram of the copper nanoparticle / flaky fullerol composite material obtained by DLS method for 7 consecutive days.

[0051] Figure 7 For use without or with 660nm visible light (0.9W / cm 2Time-dependent growth curves of Staphylococcus aureus and Escherichia coli treated with PBS, amorphous composites and copper nanoparticles / flake-like fullerol composites in LB medium at 37°C under the conditions of 15 min (min, 25 min).

[0052] Figure 8 Photos of the plates of Staphylococcus aureus and Escherichia coli after treatment and without or with 660nm visible light (0.9W / cm 2 , 15min) under the conditions of inhibition rate against Staphylococcus aureus and Escherichia coli.

[0053] Fig. 9 Scanning electron microscope (SEM) images of Staphylococcus aureus and Escherichia coli after treatment with PBS and copper nanoparticles / flake-like fullerol composites.

[0054] Fig.10 Scanning electron microscope (SEM) images of the corresponding composite materials obtained by only changing the solvent conditions of the liquid-liquid interface precipitation method, wherein (a) dimethyl sulfoxide: acetone = 1:3; (b) dimethyl sulfoxide: acetone = 3:1; (c) dimethyl sulfoxide: acetone = 1:2; (d) dimethyl sulfoxide: acetone = 2:1; (e) dimethyl sulfoxide: methanol = 1:3; (f) dimethyl sulfoxide: methanol = 3:1; (g) deionized water: acetone = 1:3; (h) deionized water: acetone = 3:1; (i) N,N-dimethylformamide: methanol = 3:1; (j) N,N-dimethylformamide: acetone = 1:3; (k) N,N-dimethylformamide: acetone = 3:1.

[0055] Fig.11 Plate photos of Staphylococcus aureus and Escherichia coli after treatment with PBS, copper nanoparticles, fullerol, amorphous composites, and copper nanoparticles / spherical fullerol composites.

[0056] Fig.12 SEM images of Staphylococcus aureus and Escherichia coli after treatment with PBS, copper nanoparticles, fullerol and amorphous composites. DETAILED DESCRIPTION

[0057] The present invention is described in detail below with reference to the accompanying drawings. The raw materials mentioned in the present invention that are not described in detail are all commercially available products; the process steps or preparation methods that are not described in detail are all process steps or preparation methods well known to those skilled in the art.

[0058] Example 1 Preparation of copper nanoparticle / flaky fullerol composite material

[0059] (1) Preparation of fullerene alcohol:

[0060] 0.1 g of fullerene was dispersed in 50 mL of toluene solution, and 10 mL of 30% hydrogen peroxide solution and 500 μL of tetrabutylammonium hydroxide solution were further added in a heated stirrer, and stirred for 16 h at 60° C. and 400 rpm.

[0061] After stirring for 16 hours, a layered solution with a clear upper layer and a turbid lower layer was obtained. A separatory funnel was used to separate the lower turbid liquid. 70 mL of isopropanol, 50 mL of anhydrous ether and 50 mL of n-hexane were added to the turbid liquid. The solution was then centrifuged at 8000 rpm for 8 minutes to fully separate the fullerol. After decantation, 10 mL of anhydrous ether was added to each centrifuge tube, and the above centrifugal decantation steps were repeated two to three times to fully remove impurities. The resulting precipitate was then dried in a vacuum oven at -1 MPa vacuum and 25°C.

[0062] The infrared spectrum of the prepared fullerenol was scanned, and the results were as follows: Figure 1 As shown. It can be seen that the spectrum of the prepared fullerene alcohol is at 3400cm -1 A broad O–H band is shown near 1080, 1370, and 1620 cm -1 Three characteristic bands are shown near the C–O , ν C–O–H and ν C=C absorption, further confirming that fullerene was successfully hydroxylated.

[0063] Thermogravimetric analysis of the prepared fullerene alcohol showed the following results: Figure 2 It can be seen that the prepared fullerol loses bound water at 120.6°C, which may be attributed to the detachment of hydroxyl groups at 120.6°C to 443.7°C, and may be attributed to the thermal loss of fullerene itself at temperatures above 443.7°C.

[0064] (2) Preparation of flake fullerol:

[0065] 2 mg of fullerol precursor powder was dissolved in 2 mL of dimethyl sulfoxide, and 6 mL of acetone was injected into the above solution at a constant rate of 200 μL / s. The mixture was then sealed and incubated at room temperature for 18 h to obtain a flake fullerol dispersion (8 mL, 0.25 mg / mL).

[0066] The flake-like fullerol dispersion prepared in step (1) was dropped onto a silicon wafer and photographed using a scanning electron microscope (SEM). The results are shown in FIG. Figure 3 As shown, it can be seen that plate-like fullerol has been successfully prepared.

[0067] (3) Preparation of copper nanoparticle / flaky fullerol composite materials:

[0068] Take 8 mL of the obtained 0.25 mg / mL flake fullerol dispersion, add 6.6 mg of copper (II) chloride dihydrate and 15 mL of water into a reagent bottle, and irradiate with a 660 nm laser (0.9 mW / cm 2 ), so that the copper chloride obtains the corresponding energy for reduction, and the mixed solution is transparent and colorless after light exposure, and almost no flocculent precipitation is produced. The solution is then centrifuged at 8000rpm for 6 minutes to fully separate the copper nanoparticles / flaky fullerol composite material, and then the obtained precipitate is placed in a vacuum oven at a vacuum degree of -1MPa and a temperature of 50°C to dry, thereby obtaining a copper nanoparticles / flaky fullerol composite material.

[0069] The prepared copper nanoparticle / fullerol composite material was subjected to X-ray photoelectron spectroscopy analysis and the results are as follows Figure 4 The Cu 2p spectrum shows two peaks at 931.9 and 951.6 eV, which are assigned to Cu 2p 3 / 2 and Cu 2p 1 / 2 , indicating that Cu 2+ existence.

[0070] The particle size of the prepared fullerene alcohol and copper nanoparticle / fullerene alcohol composite material was measured. Figure 5 As shown, the particle size of the composite material is about 160 nm. 1 mL of an aqueous solution of the composite material with a concentration of 0.1 wt% was taken at a fixed time every day for detection by a laser particle size analyzer, and each time point was repeated 3 times for 7 consecutive days. Figure 6 It is shown that the copper nanoparticle / flaky fullerol composite dispersion exhibits good stability and water solubility, and the particle size hardly changes within 7 days, and there is no obvious precipitation in the dispersion.

[0071] Example 2 Antibacterial properties of copper nanoparticles / flake-like fullerol composites

[0072] (1) S. aureus and E. coli were used as Gram-positive and Gram-negative bacteria models to evaluate the bactericidal effect of copper nanoparticles / flaky fullerol composites. First, the strain was stored in a solid culture medium. Then, 0.3 g beef powder, 1 g tryptone, and 0.5 g NaCl were weighed on an electronic balance, 100 mL deionized water was added, and the pH was adjusted to 7.4 using a 1 mol / L NaOH solution to prepare Luria-Bertani (LB) medium. The LB medium was divided into several conical flasks and sealed with sealing film. The conical flask was placed in a high-pressure steam sterilizer and sterilized with high-pressure steam at 121°C for 20 minutes. The bacteria cultured on the solid culture medium were transferred to the sterilized LB culture medium for incubation using an inoculation loop. After the incubation was completed, the optical density (OD) of the bacterial solution at a wavelength of 600 nm measured by UV-Vis was 600 ) to estimate the bacterial concentration in LB medium, and dilute the bacterial solution to the required concentration for the experiment accordingly.

[0073] (2) The bacterial growth curve was tested to investigate the time-dependent effect of the copper nanoparticle / sheet-shaped fullerol composite on the colony. 250 μL of bacterial solution (10 5 CFU / mL) under light (660nm, 0.9W / cm 2 , light exposure time: 5min) and light-protected conditions, and mixed with 250μL PBS and copper nanoparticle / flake fullerol composite dispersion (1mg / mL). The mixture was shaken continuously at 200rpm and 37℃ for 4h, and then transferred to 15mL centrifuge tubes, each containing 10mL LB medium and cultured in a shaker. At specific time intervals, take out equal volumes of the mixture of each material to measure its OD 600 , and use this to draw a description of OD 600 The relationship between the curve and time (0-8h) is as follows Figure 7 As shown, it was found that both the sample group and the sample + light group had good long-term antibacterial effects. Compared with the PBS buffer solution group, the bacteria in the light group and the non-light group of amorphous fullerol proliferated significantly over time.

[0074] (3) The antibacterial activity of the copper nanoparticle / flake fullerol composite material was evaluated by plate counting experiment. First, the bacterial solution was diluted to 10 6 CFU / mL, and then two samples (including 100 μL PBS, copper nanoparticles / sheet fullerol composite dispersion (1 mg / mL) and 100 μL bacterial solution) were placed in a dark room or irradiated with a 660 nm laser (irradiation time: 15 min, 0.9 W / cm 2) and mixed under 4% CO 2 0.5% NH 2 O. Finally, the mixture was diluted (800 times for S. aureus and 300 times for E. coli), and 20 μL of the suspension was spread on an LB agar plate. The LB agar plate was incubated in a 37°C biological incubator, and the viability of the bacterial cells was estimated by counting the number of colonies on the plate. The colony counting method is a relatively intuitive detection method that reflects the antibacterial ability of the material. We detected the antibacterial activity of the copper nanoparticle / flaky fullerol composite material, and further calculated and plotted the relevant antibacterial performance histogram based on the experimental results (antibacterial activity (%) = (PBS count-sample count) / PBS count × 100 (%)). Figure 8 It is shown in the data that under dark conditions, the copper nanoparticle / flaky fullerol composite material exhibits a good bactericidal effect against Staphylococcus aureus or Escherichia coli, with an antibacterial activity close to 80%; under laser irradiation, the inhibition efficiency of the copper nanoparticle / flaky fullerol composite material against Staphylococcus aureus and Escherichia coli is significantly improved, with the antibacterial activity against Staphylococcus aureus reaching 90% and the antibacterial activity against Escherichia coli reaching 96%.

[0075] (4) SEM was used to observe the morphological changes of bacteria before and after treatment. First, bacteria (10 7 CFU / mL) was cultured in a full-temperature shaking incubator (200rpm, 37°C) for 3h. After the incubation was completed, the mixed liquid was dripped onto the treated silicon wafer. After the liquid was naturally air-dried, the silicon wafer was placed in 2.5% glutaraldehyde for 2h. It was washed with PBS to remove unattached bacteria and dehydrated for 15 minutes with different concentrations of ethanol (30, 50, 70 and 100 v / v%). Finally, after sputtering gold on the surface of the silicon wafer, its morphological changes were observed by SEM.

[0076] The cell membrane integrity of bacteria treated with copper nanoparticle / flake-like fullerol composites was studied by SEM. Fig. 9 The figure shows that under dark conditions, the boundaries of Staphylococcus aureus (spherical) and Escherichia coli (rod-shaped) treated with copper nanoparticle / flaky fullerol composite materials are blurred and the shapes are obviously wrinkled (arrows). The SEM experimental results are consistent with the conclusions drawn from the aforementioned colony counting test.

[0077] Example 3

[0078] Referring to Example 1, only the solvent conditions of the liquid-liquid interface precipitation method in step (2) were changed, and the other conditions remained unchanged to obtain the corresponding composite material.

[0079] Referring to Example 2, the morphology of the obtained composite material was observed. Fig.10 As shown in Table 1.

[0080] Table 1 Antibacterial results of different composite materials

[0081] Soluble solvents Poorly soluble solvents A:B (volume ratio) Fullerol morphology Dimethyl sulfoxide acetone 1:3 Flake Dimethyl sulfoxide acetone 3:1 Amorphous Dimethyl sulfoxide acetone 1:2 Amorphous Dimethyl sulfoxide acetone 2:1 Amorphous Dimethyl sulfoxide Methanol 1:3 Amorphous Dimethyl sulfoxide Methanol 3:1 Block Deionized water acetone 1:3 Amorphous Deionized water acetone 3:1 Amorphous N,N-Dimethylformamide Methanol 3:1 Spherical N,N-Dimethylformamide acetone 1:3 Amorphous N,N-Dimethylformamide acetone 3:1 Amorphous

[0082] Comparative Example 1

[0083] Referring to Example 1, step (2) was omitted, and other steps remained unchanged to obtain the corresponding copper nanoparticle / amorphous fullerol composite material.

[0084] Referring to Example 1, the good solvent in step (2) was changed to N,N-dimethylformamide, the poor solvent was changed to methanol, and the other conditions remained unchanged to obtain the corresponding copper nanoparticle / spherical fullerol composite material.

[0085] Referring to Example 2, the antibacterial properties of the copper nanoparticles alone, the fullerol alone, the obtained amorphous composite material, and the copper nanoparticle / spherical fullerol composite material were measured. Fig.11 As shown in Table 2.

[0086] Referring to Example 2, the morphological changes of the bacteria before and after treatment with the copper nanoparticles alone, the fullerol alone, and the obtained amorphous composite material were observed by SEM, as shown in FIG. Fig.12 shown.

[0087] Table 2 Inhibition rate of each material against Staphylococcus aureus and Escherichia coli at different time

[0088]

[0089]

[0090] By observing the coating results of the amorphous composite material and the copper nanoparticle / spherical fullerol composite material, it was found that even under light, the amorphous composite material had a large number of colonies remaining for Staphylococcus aureus or Escherichia coli, while the copper nanoparticle / spherical fullerol composite material also had a certain antibacterial ability, but the effect was not as good as the copper nanoparticle / flake fullerol composite material. In addition, the morphological changes of bacteria before and after treatment with the amorphous composite material obtained by SEM observation showed that compared with pure copper nanoparticles or amorphous composite materials, the copper nanoparticle / flake fullerol composite material had a stronger ability to destroy bacterial cell membranes, which may be attributed to its sharp morphology.

[0091] The embodiments provided above are not intended to limit the scope of the present invention, and the steps described are not intended to limit the execution order thereof. Those skilled in the art may make obvious improvements to the present invention in combination with existing common knowledge, which also fall within the scope of protection defined by the claims of the present invention.

Claims

1. A method for preparing a copper nanoparticle / flaky fullerol composite material, characterized in that: The method comprises the following steps: (1) dispersing fullerene in an organic solvent to prepare a fullerene dispersion, then adding peroxide and tetrabutylammonium hydroxide to carry out a solvothermal reaction, and after the reaction is completed, standing to separate the layers, collecting the lower liquid phase, and then adding a precipitant to separate the solid and the liquid, collecting the solid, and drying to obtain a fullerol powder; (2) dispersing fullerol powder in a good solvent with good solubility, adding a poor solvent with relatively poor solubility for fullerol to the fullerol dispersion at a constant rate, and then sealing and incubating at room temperature for a period of time to obtain a flake fullerol dispersion; the good solvent is dimethyl sulfoxide; the poor solvent is acetone; and the volume ratio of the good solvent to the poor solvent is 1:3; (3) Mixing a divalent copper salt with the flake fullerol dispersion obtained in step (2) to obtain a mixed solution, which is then placed under laser irradiation. After the irradiation, the solid-liquid separation is performed, and the solid is collected and dried to obtain a copper nanoparticle / flake fullerol composite material.

2. The method according to claim 1, characterized in that The organic solvent in step (1) is toluene; the peroxide includes any one or more of the following: 30% hydrogen peroxide, tert-butyl hydroperoxide, dibenzoyl peroxide, and potassium permanganate.

3. The method according to claim 1, characterized in that In step (1), the mass volume ratio of fullerene to organic solvent is (1.5-3):1, mg / mL; the volume ratio of organic solvent, peroxide, and tetrabutylammonium hydroxide is 100:20:1 (mL).

4. The method according to claim 1, characterized in that The rate of adding the poor solvent in step (2) is 200 μL / s; the incubation time is 8-24h.

5. The method according to claim 1, characterized in that The divalent copper salt in step (3) is selected from the group consisting of: copper chloride, copper chloride dihydrate, copper nitrate, copper nitrate hydrate, copper carbonate, copper carbonate hydrate, copper sulfate, and copper sulfate hydrate; the mass ratio of the flaky fullerol to the divalent copper salt is 1:3 to 1:

4.

6. The method according to any one of claims 1 to 5, characterized in that: In step (3), a certain amount of water is added to the mixed solution, and the volume ratio of water to the flake fullerol dispersion is (10-20):8; the wavelength of the laser is 660 nm, and the excitation energy is 0.9 mW / cm 2 .

7. The copper nanoparticle / flaky fullerol composite material prepared by the method according to any one of claims 1 to 6.

8. An antibacterial agent, characterized in that The antibacterial agent comprises the copper nanoparticle / flaky fullerol composite material according to claim 7.

9. An antibacterial method for non-disease treatment purposes, characterized in that: The method uses the copper nanoparticle / flaky fullerol composite material according to claim 7 as an antibacterial agent for antibacterial treatment.