Preparation method and application of terbium nitride-zirconium fluoride composite carrier loaded Pd catalyst

Through the preparation of the Pd catalyst supported by terbium nitride-zirconium fluoride composite support, the problem of difficult to take into account both the acetylene conversion rate and ethylene selectivity in the acetylene hydrogenation reaction in the prior art is solved, and efficient and stable catalytic performance and economical are achieved. Catalyst preparation.

CN116673060BActive Publication Date: 2024-11-26ZHEJIANG UNIV OF TECH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202310824394.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-06
Publication Date
2024-11-26
Estimated Expiration
2043-07-06

AI Technical Summary

Technical Problem

It is difficult for existing supported Pd catalysts to take into account both acetylene conversion and ethylene selectivity in acetylene hydrogenation reaction, and the impact of the support on the catalytic performance is limited.

Method used

The preparation method of terbium nitride-zirconium fluoride composite support supported Pd catalyst was adopted to synthesize terbium nitride-zirconium fluoride composite material through ball milling and sintering technology, and deposit Pd through chloropalladium acid impregnation solution to control palladium elements and composite materials The ratio of the catalyst is formed to form an efficient catalyst.

Benefits of technology

The acetylene conversion rate and ethylene selectivity of the catalyst are improved, and good stability is maintained. The Pd content is low, the price is economical, and it is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a terbium nitride-zirconium fluoride composite carrier-loaded Pd catalyst. The preparation method of the terbium nitride-zirconium fluoride composite carrier-loaded Pd catalyst comprises the following steps: (1) terbium nitride powder and zirconium fluoride powder are mixed evenly and ball-milled; (2) the ball-milled product is sintered at high temperature in nitrogen to obtain a terbium nitride-zirconium fluoride composite material; (3) a chloropalladium acid impregnation solution is prepared; (4) the terbium nitride-zirconium fluoride composite material is dispersed in deionized water, the chloropalladium acid impregnation solution is dripped and mixed evenly, and a xenon lamp is used to irradiate the mixture for 2-6 hours under uniform stirring; (5) separation, washing, and vacuum drying are performed to obtain a terbium nitride-zirconium fluoride composite carrier-loaded Pd catalyst. The invention provides an application of a prepared terbium nitride-zirconium fluoride composite carrier-loaded Pd catalyst in acetylene selective hydrogenation reaction, which has the characteristics of high acetylene conversion and ethylene selectivity and good stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to a preparation method of a terbium nitride-zirconium fluoride composite carrier loaded with a Pd catalyst and an application of the catalyst in a selective hydrogenation reaction of acetylene. Background Art

[0002] Industrial ethylene feed usually contains trace amounts of acetylene (0.1-1 mol%). Hydrogenating acetylene to ethylene is an ideal method to remove acetylene and improve economic benefits. This method generally uses a supported Pd catalyst. In the Pd-loaded acetylene hydrogenation catalyst, the carrier has an important influence on the catalytic performance. At present, the carriers used in industry mainly include Al2O3, SiO2, TiO2 and molecular sieves, among which Al2O3 is the most widely used carrier. However, it is always difficult to balance the acetylene conversion rate and selectivity during application. Researchers have tried to modify the carrier to improve the catalytic performance of the acetylene hydrogenation catalyst.

[0003] Based on the above background, a suitable catalyst is designed to improve the ethylene selectivity of the catalyst in the selective hydrogenation reaction of acetylene, thereby facilitating the industrial production of ethylene. Summary of the invention

[0004] The purpose of the present invention is to provide a preparation method and application of a terbium nitride-zirconium fluoride composite carrier loaded with a Pd catalyst, wherein the terbium nitride-zirconium fluoride composite carrier can synergistically adjust the surface properties of the carrier so that the catalyst has a high acetylene conversion rate and ethylene selectivity as well as good stability.

[0005] Next, the technical solution used in the present invention is described in detail.

[0006] In a first aspect, the present invention provides a method for preparing a terbium nitride-zirconium fluoride composite carrier-supported Pd catalyst, comprising the following steps:

[0007] (1) mixing terbium nitride powder and zirconium fluoride powder in a mass ratio of 90-50%:10-50%, and ball milling the mixed powder to make it fully mixed;

[0008] (2) heating the ball-milled product to 400-600° C. at a heating rate of 2-20° C. / min and sintering for 3-12 hours under a nitrogen atmosphere with a flow rate of 50-200 ml / min, and then cooling the temperature to room temperature at a cooling rate of 1-20° C. / min to obtain a terbium nitride-zirconium fluoride composite material;

[0009] (3) dissolving palladium chloride with a small amount of hydrochloric acid and then diluting with deionized water to prepare a chloropalladium acid impregnation solution, wherein the mass concentration of palladium is 0.001-0.02 g / mL;

[0010] (4) dispersing the terbium nitride-zirconium fluoride composite material obtained in step (2) in deionized water, dripping the chloropalladium acid impregnation solution in step (3) and mixing evenly, irradiating the mixture with a xenon lamp for 2-6 hours while stirring at a constant speed and controlling the temperature at 10-50° C.; controlling the mass ratio of palladium element to terbium nitride-zirconium fluoride composite material to be 0.01-0.2:100;

[0011] (5) Separating a sample from the mixture obtained in step (4), and washing with deionized water and anhydrous ethanol respectively until the washing liquid is neutral, and then vacuum drying the product to obtain a terbium nitride-zirconium fluoride composite carrier-loaded Pd catalyst.

[0012] Preferably, the mixing mass ratio of terbium nitride powder to zirconium fluoride powder is 90-70%:10-30%, most preferably 70%:30%.

[0013] Preferably, in step (1), the ball milling treatment adopts wet ball milling, the ball milling jar used is a cemented carbide jar, a vacuum stainless steel jar or an agate jar, the balls used are cemented carbide balls, stainless steel balls or agate balls, anhydrous ethanol, polyvinyl alcohol or polymethyl methacrylate is used as the ball milling medium, and the ball milling working conditions are: a speed of 200-600r / min, a ball milling time of 20-40h, and after the ball milling is completed, the ball milling product is taken out and dried to obtain. It is further preferred that the ball milling speed is 500r / min, the ball milling time is 30h, and anhydrous ethanol is used as the ball milling medium.

[0014] Preferably, in step (2), the nitrogen flow rate is 100 ml / min, the temperature is increased to 500°C at a heating rate of 10°C / min, sintered for 6 hours, and then cooled to room temperature at a cooling rate of 5°C / min.

[0015] Preferably, in step (4), the temperature is controlled at 10-40° C., the power of the xenon lamp is 300 W, and the irradiation time is 3 h.

[0016] Preferably, in step (4), the mass ratio of palladium element to terbium nitride-zirconium fluoride composite material is controlled to be 0.02-0.1:100, most preferably 0.03:100.

[0017] Preferably, in step (5), the separation is carried out by centrifugal separation, the centrifuge speed is 5000-8000 rpm, and the centrifugation time is 8-20 min.

[0018] Preferably, in step (5), the vacuum drying conditions are: vacuum drying at 60° C. for 12 hours.

[0019] In a second aspect, the present invention provides the use of a Pd catalyst supported on a terbium nitride-zirconium fluoride composite carrier prepared according to the above preparation method in the selective hydrogenation reaction of acetylene.

[0020] Furthermore, the application is specifically as follows: in a fixed bed reactor, the terbium nitride-zirconium fluoride composite carrier loaded with Pd catalyst is loaded, hydrogen is introduced for reduction before the reaction, the reduction temperature is 170-350°C, the reduction time is 1-3h, and then a gas containing acetylene and hydrogen is introduced as a reaction gas, the reaction pressure is normal pressure (0.1MPa), the reaction temperature is 50-300°C, and the reaction hydrogenates the acetylene in the mixed gas to produce ethylene.

[0021] Furthermore, in the gas containing acetylene and hydrogen, the molar ratio of C2H2:H2=1:1-20.

[0022] Furthermore, the gas containing acetylene and hydrogen also contains ethylene, and nitrogen is introduced to balance it.

[0023] Furthermore, during the reaction, the gas volume space velocity (GHSV) is 5000 to 20000 h -1 .

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] (1) The terbium nitride-zirconium fluoride composite carrier prepared by the present invention has a relatively suitable specific surface area (specific surface area is 167-433m 2 / g), good stability, and more efficiently exert the catalytic effect of zirconium fluoride; terbium nitride and zirconium fluoride can synergistically adjust the surface properties of the carrier, so that the catalyst has a higher acetylene conversion rate and ethylene selectivity.

[0026] (2) The terbium nitride-zirconium fluoride composite carrier-loaded Pd catalyst provided by the present invention has a low Pd content, a low price, and is simple to prepare. When applied to the selective hydrogenation reaction of acetylene, it exhibits the characteristics of high acetylene conversion rate, high ethylene selectivity, and good stability. DETAILED DESCRIPTION

[0027] The present invention is described below with specific examples. It is necessary to point out that the embodiments are only used to further illustrate the present invention, but cannot be understood as limiting the scope of protection of the present invention, and the present invention is not limited thereto in any way. Those skilled in the art in this field can make some non-essential improvements and adjustments based on the content of the above invention.

[0028] If no specific conditions are specified in the examples of the present invention, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. If no manufacturer is specified for the reagents or instruments used, they are all conventional products that can be obtained by conventional technical means or purchased commercially.

[0029] Example 1

[0030] (1) Preparation of terbium nitride-zirconium fluoride composite material: Weigh 7g of terbium nitride and 3g of zirconium fluoride in a mortar and grind them evenly. Put them into an agate ball mill. Use agate balls with a ball-to-material ratio of 5:1. Use anhydrous ethanol as the ball milling medium to cover the mixture. Grind in a ball mill at a speed of 300r / min for 24h, take out and dry to obtain a ball milling product. Pour the ball milling product into a quartz boat and place it in the center of the heating section of a tube furnace. In a nitrogen atmosphere with a flow rate of 100ml / min, heat it to 500℃ at a heating rate of 10℃ / min, sinter it for 6h, and cool it to room temperature at a cooling rate of 5℃ / min to obtain a terbium nitride-zirconium fluoride composite material. The specific surface area of ​​the terbium nitride-zirconium fluoride composite carrier is 297m 2 / g.

[0031] (2) Preparation of impregnation solution: Weigh 3.344 g of palladium chloride with a Pd content of 59.8% or more, add a small amount of hydrochloric acid to dissolve, add deionized water to dilute and prepare 100 ml of solution, wherein the mass concentration of palladium is 0.02 g / ml.

[0032] (3) Preparation of catalyst: The terbium nitride-zirconium fluoride composite material was dispersed in deionized water, 0.15 ml of the above impregnation solution was added and mixed evenly, and the mixed solution was irradiated with a xenon lamp for 3 h while stirring at a constant speed and controlling the temperature at 20 °C. The sample was separated using a centrifuge at a speed of 6000 rpm for 10 min, and washed with deionized water and anhydrous ethanol for multiple times to make the pH value ≈ 7, and then the product was dried in a vacuum oven at 60 °C for 12 h.

[0033] (4) Application of the catalyst in acetylene hydrochlorination: Weigh 0.3 g of the catalyst, load it into a fixed bed reactor, introduce hydrogen to reduce it at 300°C for 1 hour, and then purge it with nitrogen for 1 hour. The reaction pressure is normal pressure, the reaction temperature is 170°C, and a mixed gas of acetylene, ethylene, hydrogen, and nitrogen (C2H2=0.328%, H2=0.667%, C2H4=33%, nitrogen balance) is introduced, and the volume space velocity is 10000h -1 Under the same conditions, the acetylene conversion rate is 95% and the ethylene selectivity is 90% after 50 hours of reaction. After 1000 hours of reaction, the acetylene conversion rate can reach 90% and the ethylene selectivity can reach 85%.

[0034] Example 2

[0035] (1) Preparation of terbium nitride-zirconium fluoride composite material: Weigh 9g of terbium nitride and 1g of zirconium fluoride in a mortar and grind them evenly. Put them into an agate ball mill. Use agate balls with a ball-to-material ratio of 5:1. Use anhydrous ethanol as the ball milling medium to cover the mixture. Grind in a ball mill at a speed of 300r / min for 24h, take out and dry to obtain a ball milling product. Pour the ball milling product into a quartz boat and place it in the center of the heating section of a tube furnace. In a nitrogen atmosphere with a flow rate of 100ml / min, heat it to 500℃ at a heating rate of 10℃ / min, sinter it for 6h, and cool it to room temperature at a cooling rate of 5℃ / min to obtain a terbium nitride-zirconium fluoride composite material. The specific surface area of ​​the terbium nitride-zirconium fluoride composite carrier is 433m 2 / g.

[0036] (2) Preparation of the impregnation solution: The preparation of the impregnation solution is the same as that in Example 1.

[0037] (3) Preparation of catalyst: The terbium nitride-zirconium fluoride composite material was dispersed in deionized water, 0.3 ml of the above impregnation solution was added and mixed evenly, and the mixed solution was irradiated with a xenon lamp for 6 h while stirring at a constant speed and controlling the temperature at 20°C. The sample was separated using a centrifuge at a speed of 6000 rpm for 10 min, and washed with deionized water and anhydrous ethanol for multiple times to make the pH value ≈ 7, and then the product was dried in a vacuum oven at 60°C for 12 h.

[0038] (4) Application of the catalyst in acetylene hydrochlorination: Weigh 0.3 g of the catalyst, load it into a fixed bed reactor, introduce hydrogen to reduce it at 300°C for 1 hour, and then purge it with nitrogen for 1 hour. The reaction pressure is normal pressure, the reaction temperature is 170°C, and a mixed gas of acetylene, ethylene, hydrogen, and nitrogen (C2H2=0.328%, H2=0.667%, C2H4=33%, nitrogen balance) is introduced, and the volume space velocity is 10000h -1 Under the same conditions, the acetylene conversion rate was 99% and the ethylene selectivity was 70% after 50h of reaction. After 1000h of reaction, the acetylene conversion rate could reach 99% and the ethylene selectivity could reach 75%.

[0039] Example 3

[0040] (1) Preparation of terbium nitride-zirconium fluoride composite material: Weigh 5g of terbium nitride and 5g of zirconium fluoride in a mortar and grind them evenly. Put them into an agate ball mill. Use agate balls with a ball-to-material ratio of 5:1. Use anhydrous ethanol as the ball milling medium to cover the mixture. Grind in a ball mill at a speed of 300r / min for 24h, take out and dry to obtain a ball milling product. Pour the ball milling product into a quartz boat and place it in the center of the heating section of a tube furnace. In a nitrogen atmosphere with a flow rate of 100ml / min, heat it to 500℃ at a heating rate of 10℃ / min, sinter it for 6h, and cool it to room temperature at a cooling rate of 5℃ / min to obtain a terbium nitride-zirconium fluoride composite material. The specific surface area of ​​the terbium nitride-zirconium fluoride composite carrier is 167m 2 / g.

[0041] (2) Preparation of the impregnation solution: The preparation of the impregnation solution is the same as that in Example 1.

[0042] (3) Preparation of catalyst: The terbium nitride-zirconium fluoride composite material was dispersed in deionized water, 0.15 ml of the above impregnation solution was added and mixed evenly, and the mixed solution was irradiated with a xenon lamp for 3 h while stirring at a constant speed and controlling the temperature at 20 °C. The sample was separated using a centrifuge at a speed of 6000 rpm for 10 min, and washed with deionized water and anhydrous ethanol for multiple times to make the pH value ≈ 7, and then the product was dried in a vacuum oven at 60 °C for 12 h.

[0043] (4) Application of the catalyst in acetylene hydrochlorination: Weigh 0.3 g of the catalyst, load it into a fixed bed reactor, introduce hydrogen to reduce it at 300°C for 1 hour, and then purge it with nitrogen for 1 hour. The reaction pressure is normal pressure, the reaction temperature is 170°C, and a mixed gas of acetylene, ethylene, hydrogen, and nitrogen (C2H2=0.328%, H2=0.667%, C2H4=33%, nitrogen balance) is introduced, and the volume space velocity is 10000h -1 Under the above conditions, the acetylene conversion rate was 80% and the ethylene selectivity was 93% after 50h of reaction. After 1000h of reaction, the acetylene conversion rate could reach 72% and the ethylene selectivity could reach 90%.

[0044] Example 4

[0045] The method of Example 1 was followed, except that the amount of the impregnation solution dripped in step (3) was 0.1 ml. Under the same conditions, the acetylene conversion rate was 65% and the ethylene selectivity was 97% after 50 hours of reaction; after 1000 hours of reaction, the acetylene conversion rate was 60% and the ethylene selectivity was 93%.

[0046] Example 5

[0047] The method of Example 1 was followed, except that the amount of the impregnation solution dripped in step (3) was 0.3 ml. Under the same conditions, the acetylene conversion rate was 99% and the ethylene selectivity was 60% after 50 hours of reaction; after 1000 hours of reaction, the acetylene conversion rate was 99% and the ethylene selectivity was 62%.

[0048] Example 6

[0049] The method of Example 1 was followed, except that the amount of the impregnation solution dripped in step (3) was 0.5 ml. Under the same conditions, the acetylene conversion rate was 99% and the ethylene selectivity was 40% after 50 hours of reaction; after 1000 hours of reaction, the acetylene conversion rate was 99% and the ethylene selectivity was 37%.

[0050] From the comparison between Example 1 and Examples 4-6, it can be seen that the loading amount of the active component has an important influence on the catalyst performance. Too little or too much will reduce the catalytic performance. The optimal loading amount of palladium is 0.03%wt.

[0051] Comparative Example 1

[0052] (1) Preparation of carrier: Weigh 7 g of terbium nitride and 3 g of zirconium fluoride in a mortar, grind them evenly, pour them into a quartz boat, and place it in the center of the heating section of a tube furnace. In a nitrogen atmosphere with a flow rate of 100 ml / min, heat the boat to 500°C at a heating rate of 10°C / min, sinter for 6 h, and cool the boat to room temperature at a cooling rate of 5°C / min to obtain a terbium nitride-zirconium fluoride composite material.

[0053] (2) Preparation of impregnation solution: Weigh 3.344 g of palladium chloride with a Pd content of 59.8% or more, add a small amount of hydrochloric acid to dissolve, add deionized water to dilute and prepare 100 ml of solution, wherein the mass concentration of palladium is 0.02 g / ml.

[0054] (3) Preparation of catalyst: The terbium nitride-zirconium fluoride composite material was dispersed in deionized water, 0.15 ml of the above impregnation solution was added and mixed evenly, and the mixed solution was irradiated with a xenon lamp for 3 h while stirring at a constant speed and controlling the temperature at 20°C. The sample was separated using a centrifuge at a speed of 6000 rpm for 10 min, and washed with deionized water and anhydrous ethanol for multiple times to make the pH value ≈ 7, and then the product was dried in a vacuum oven at 60°C for 12 h.

[0055] (4) Application of the catalyst in acetylene hydrochlorination: Weigh 0.3 g of the catalyst, load it into a fixed bed reactor, introduce hydrogen to reduce it at 300°C for 1 hour, and then purge it with nitrogen for 1 hour. The reaction pressure is normal pressure, the reaction temperature is 170°C, and a mixed gas of acetylene, ethylene, hydrogen, and nitrogen (C2H2=0.328%, H2=0.667%, C2H4=33%, nitrogen balance) is introduced, and the volume space velocity is 10000h-1 Under the conditions, the acetylene conversion rate was 80% and the ethylene selectivity was 65% after 50h of reaction; after 1000h of reaction, the acetylene conversion rate could reach 70% and the ethylene selectivity was 60%.

[0056] From the comparison between Example 1 and Comparative Example 1, it can be seen that the preparation method of the terbium nitride-zirconium fluoride composite material has an important influence on the catalytic performance of the acetylene selective hydrogenation catalyst prepared therefrom, and the ball milling treatment of terbium nitride and zirconium fluoride before sintering can significantly improve the catalytic performance of the catalyst and significantly improve the acetylene conversion rate and ethylene selectivity.

[0057] Comparative Example 2

[0058] (1) Preparation of carrier: Weigh 10g of terbium nitride and put it into an agate ball mill, use agate balls, the ball-to-material ratio is 5:1, and use anhydrous ethanol as the ball milling medium to cover the mixture. Grind in a ball mill at a speed of 300r / min for 24h, take out and dry to obtain the ball milling product. Pour the ball milling product into a quartz boat, pour it into the quartz boat, place it in the center of the heating section of a tube furnace, and heat it to 500℃ at a heating rate of 10℃ / min in a nitrogen atmosphere with a flow rate of 100ml / min, then sinter it for 6h, and cool it down to room temperature at a cooling rate of 5℃ / min to obtain a terbium nitride carrier.

[0059] (2) Preparation of impregnation solution: Weigh 3.344 g of palladium chloride with a Pd content of 59.8% or more, add a small amount of hydrochloric acid to dissolve, add deionized water to dilute and prepare 100 ml of solution, wherein the mass concentration of palladium is 0.02 g / ml.

[0060] (3) Preparation of catalyst: Terbium nitride was dispersed in deionized water, 0.15 ml of the above impregnation solution was added and mixed evenly, and the mixed solution was irradiated with a xenon lamp for 3 h while stirring at a constant speed and controlling the temperature at 20 °C. The sample was separated by a centrifuge at a speed of 6000 rpm for 10 min, and washed with deionized water and anhydrous ethanol for multiple times to make the pH value ≈ 7, and then the product was dried in a vacuum oven at 60 °C for 12 h.

[0061] (4) Application of the catalyst in acetylene hydrochlorination: Weigh 0.3 g of the catalyst, load it into a fixed bed reactor, introduce hydrogen to reduce it at 300°C for 1 hour, and then purge it with nitrogen for 1 hour. The reaction pressure is normal pressure, the reaction temperature is 170°C, and a mixed gas of acetylene, ethylene, hydrogen, and nitrogen (C2H2=0.328%, H2=0.667%, C2H4=33%, nitrogen balance) is introduced, and the volume space velocity is 10000h -1 Under the same conditions, the acetylene conversion rate was 99% and the ethylene selectivity was 30% after 50h of reaction. After 1000h of reaction, the acetylene conversion rate could reach 98% and the ethylene selectivity could reach 21%.

[0062] Comparative Example 3

[0063] (1) Preparation of carrier: Weigh 10g of zirconium fluoride and put it into an agate ball mill, use agate balls, the ball-to-material ratio is 5:1, and use anhydrous ethanol as the ball milling medium to cover the mixture. Grind in a ball mill at a speed of 300r / min for 24h, take out and dry to obtain the ball milling product. Pour the ball milling product into a quartz boat, place it in the center of the heating section of a tube furnace, and heat it to 500℃ at a heating rate of 10℃ / min in a nitrogen atmosphere with a flow rate of 100ml / min, then sinter for 6h, and cool it to room temperature at a cooling rate of 5℃ / min to obtain a zirconium fluoride carrier.

[0064] (2) Preparation of impregnation solution: Weigh 3.344 g of palladium chloride with a Pd content of 59.8% or more, add a small amount of hydrochloric acid to dissolve, add deionized water to dilute and prepare 100 ml of solution, wherein the mass concentration of palladium is 0.02 g / ml.

[0065] (3) Preparation of catalyst: Disperse zirconium fluoride in deionized water, drop 0.15 ml of the above impregnation solution into the mixture and mix well. Stir at a constant speed and control the temperature at 20°C. Irradiate the mixed solution with a xenon lamp for 3 hours. Separate the sample using a centrifuge at a speed of 6000 rpm for 10 minutes. Wash the sample with deionized water and anhydrous ethanol for multiple times to make the pH value ≈ 7. Then dry the product in a vacuum oven at 60°C for 12 hours.

[0066] (4) Application of the catalyst in acetylene hydrochlorination: Weigh 0.3 g of the catalyst, load it into a fixed bed reactor, introduce hydrogen to reduce it at 300°C for 1 hour, and then purge it with nitrogen for 1 hour. The reaction pressure is normal pressure, the reaction temperature is 170°C, and a mixed gas of acetylene, ethylene, hydrogen, and nitrogen (C2H2=0.328%, H2=0.667%, C2H4=33%, nitrogen balance) is introduced, and the volume space velocity is 10000h -1 Under the same conditions, the acetylene conversion rate was 30% and the ethylene selectivity was 87% after 50h of reaction. After 1000h of reaction, the acetylene conversion rate was 23% and the ethylene selectivity was 84%.

[0067] From the comparison between Example 1 and Comparative Examples 2-3, it can be seen that the terbium nitride-zirconium fluoride composite material as a carrier shows a synergistic effect of terbium nitride and zirconium fluoride in the terbium nitride-zirconium fluoride composite material, which can significantly improve the catalytic performance of the acetylene selective hydrogenation catalyst prepared therefrom, and has both high acetylene conversion rate and high ethylene selectivity.

Claims

1. A method for preparing a terbium nitride-zirconium fluoride composite carrier-supported Pd catalyst, Features: The preparation method comprises the following steps: (1) mixing terbium nitride powder and zirconium fluoride powder in a mass ratio of 90-50%:10-50%, and ball milling the mixed powder to make it fully mixed; (2) heating the ball-milled product to 400-600° C. at a heating rate of 2-20° C. / min and sintering for 3-12 hours under a nitrogen atmosphere with a flow rate of 50-200 ml / min, and then cooling the temperature to room temperature at a cooling rate of 1-20° C. / min to obtain a terbium nitride-zirconium fluoride composite material; (3) dissolving palladium chloride with a small amount of hydrochloric acid and then diluting with deionized water to prepare a chloropalladium acid impregnation solution, wherein the mass concentration of palladium is 0.001-0.02 g / mL; (4) dispersing the terbium nitride-zirconium fluoride composite material obtained in step (2) in deionized water, dripping the chloropalladium acid impregnation solution in step (3) and mixing evenly, irradiating the mixture with a xenon lamp for 2-6 hours while stirring at a constant speed and controlling the temperature at 10-50° C.; controlling the mass ratio of palladium element to terbium nitride-zirconium fluoride composite material to be 0.01-0.2:100; (5) Separating a sample from the mixture obtained in step (4), and washing with deionized water and anhydrous ethanol respectively until the washing liquid is neutral, and then vacuum drying the product to obtain a terbium nitride-zirconium fluoride composite carrier-loaded Pd catalyst.

2. The preparation method according to claim 1, Features: The mixing mass ratio of terbium nitride powder to zirconium fluoride powder is 90-70%:10-30%.

3. The preparation method according to claim 2, Features: The mixing mass ratio of the terbium nitride powder to the zirconium fluoride powder is 70%:30%.

4. The preparation method according to claim 1 or 2, Features: In step (1), the ball milling treatment adopts wet ball milling.

5. The preparation method according to claim 1 or 2, Features: In step (2), the nitrogen flow rate is 100 ml / min, the temperature is raised to 500°C at a heating rate of 10°C / min, sintered for 6 hours, and then cooled to room temperature at a cooling rate of 5°C / min.

6. The preparation method according to claim 1 or 2, Features: In step (4), the mass ratio of palladium element to terbium nitride-zirconium fluoride composite material is controlled to be 0.02-0.1:

100.

7. The preparation method according to claim 6, Features: In step (4), the mass ratio of palladium element to terbium nitride-zirconium fluoride composite material is controlled to be 0.03:

100.

8. Use of the terbium nitride-zirconium fluoride composite carrier-supported Pd catalyst prepared according to the preparation method of claim 1 or 2 in the selective hydrogenation reaction of acetylene.

9. The use according to claim 8, Features: The application is specifically as follows: in a fixed bed reactor, the terbium nitride-zirconium fluoride composite carrier loaded Pd catalyst is loaded, hydrogen is introduced for reduction before the reaction, the reduction temperature is 170-350° C., the reduction time is 1-3 hours, and then a gas containing acetylene and hydrogen is introduced as a reaction gas, the reaction pressure is normal pressure, the reaction temperature is 50-300° C., and the reaction hydrogenates the acetylene in the mixed gas to produce ethylene.

10. The use according to claim 9, Features: The gas containing acetylene and hydrogen has a molar ratio of C 2 H 2 :H 2 =1:1-20.

11. The use according to claim 9, Features: The gas containing acetylene and hydrogen also contains ethylene, and nitrogen is introduced to balance it.

12. The use according to claim 9, Features: During the reaction, the gas volume space velocity (GHSV) is 5000~20000h -1 .

Citation Information

Patent Citations

  • Rare earth doping fluozirconate luminescent material and preparing method thereof

    CN105754596A

  • Rare-earth-doped Li4ZrF8 nano-luminescence material with porous structure and preparation method and application thereof

    CN107163937A

  • Preparation method of highly dispersed Pd-IL / Al2O3 catalyst and application of same in selective hydrogenation reaction of acetylene

    CN109078655A

  • Metal organic framework composite material with core-shell structure as well as preparation method and application of metal organic framework composite material

    CN115337915A

  • Method for producing compound having acetylene bond and / or diene

    WO2015163324A1