A graphene / PI composite material and preparation method thereof

By chemically etching and covalently modifying graphene oxide, a porous structure with high active sites is formed, which solves the problems of poor dispersion and weak interfacial bonding force of GO in PI, and significantly improves the performance of graphene/PI composite materials. Strength and toughness.

CN116694074BActive Publication Date: 2024-10-01NANJING TECH UNIV
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202310574709.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-19
Publication Date
2024-10-01
Estimated Expiration
2043-05-19

AI Technical Summary

Technical Problem

Graphene oxide (GO) has poor dispersion and few active sites in polyimide (PI), resulting in weak interfacial bonding force, making it difficult to obtain graphene/PI composite materials with both high strength and high toughness.

Method used

Graphene oxide is prepared through an oxidation method, chemically etched and re-oxidized to form a porous structure, followed by covalent modification to add carboxyl functional groups, combined with ultrasonic dispersion and imidization reaction to prepare porous graphene oxide with high active sites. /polyamic acid composite material.

Benefits of technology

The dispersion and interface bonding strength of graphene oxide in PI are significantly improved, a high-strength and high-toughness graphene/PI composite material is obtained, and the tensile strength at break and elongation at break of the material are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116694074B_ABST
    Figure CN116694074B_ABST
Patent Text Reader

Abstract

The present invention discloses a graphene / PI composite material and a preparation method thereof. Nanopores are successfully formed on the surface of GO by chemical etching, and carboxyl functional groups are further grafted on the edges of the nanopores to successfully prepare active porous GO (M-O-PGO) modified with carboxyl functional groups, which greatly increases the active site content of GO. When compounded with PI, the abundant active sites of M-O-PGO enhance its dispersibility in PI and the interfacial bonding strength with PI, thereby preparing a M-O-PGO / PI composite material with both high strength and high toughness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of preparation of graphene-enhanced polymer materials, and in particular to a graphene / PI composite material and a preparation method thereof. Background Art

[0002] Graphene is a two-dimensional carbon-based material that is widely used to reinforce and modify polymer materials due to its excellent mechanical properties, electrical conductivity and thermal stability. In recent years, composite materials based on graphene and its derivatives have shown many excellent properties and have received great attention. Graphene oxide (GO), as an important derivative of graphene and a key intermediate product for the preparation of graphene by redox method, has many characteristics similar to graphene. The rich functional groups on the surface of GO give it high dispersibility and rich designability in polymers, so it is widely used in polymer composites.

[0003] The mechanical reinforcement effect of GO on polymers depends on the following two key factors: 1) the dispersibility of GO; 2) the interfacial bonding ability between GO and the matrix. There are π-π bonds and electrostatic adsorption between GO, and it is easy to agglomerate, which reduces its dispersibility in the polymer matrix. GO and polymers mainly interact through van der Waals forces or hydrogen bonds, so the binding force between the two is weak, and it is difficult to form an effective mechanical load transfer between the two. These two characteristics make the reinforcement effect of directly adding GO on polymers very limited.

[0004] In order to further enhance the performance of GO / polymer composites, GO is usually surface modified, among which covalent modification is the most common. Covalent modification enhances the dispersibility of GO in polymers and their precursors or monomers by modifying the functional groups of GO, and improves the interfacial bonding strength between GO and polymers through chemical reactions between active functional groups. According to the types of functional groups of polymer precursors or monomers, common functional groups for modifying GO include carboxyl, amino, siloxane, isocyanate, aminoquinoline, etc. However, GO defects and active sites are mainly concentrated at its edges, so that these functional groups can only be grafted to the edge of GO. Although the composite material is enhanced to a certain extent, it is still far from the expected effect. In addition, due to the small number of active sites on the GO surface, it is easy to break with the polymer from the surface, which makes the overall interaction between GO and the matrix weak, and it is difficult to obtain a composite material with both high strength and high toughness.

[0005] Nanopore etching and covalent modification on the GO surface can achieve functional group modification of the edges of GO nanosheets and the edges of holes within the GO surface, which is expected to further improve its dispersibility in polymers and the interfacial bonding strength with polymers, thereby obtaining graphene / polymer composites with higher strength and good toughness. However, the holes introduced as "defects" may cause a decrease in the mechanical properties of graphene itself, especially when the pore content is too high and the pore size is too large. Therefore, it is necessary to systematically study the conditions of pore etching and covalent modification to strictly control the content and size of the pores to avoid the problem of insignificant enhancement effect due to the decrease in the performance of graphene itself.

[0006] Polyimide (PI) is a common thermosetting polymer material. As a special engineering material, it has good heat resistance, high mechanical strength and low thermal expansion coefficient. It is widely used in high-tech fields such as photovoltaics, microelectronics and aerospace engineering. A large number of studies have used (oxidized) graphene or modified (oxidized) graphene to enhance PI, but the effect is still not ideal, and it is difficult to obtain graphene / PI composite materials with both high strength and high toughness. Summary of the invention

[0007] Purpose of the invention: The purpose of the present invention is to solve the problem that GO has poor dispersibility in PI and few active sites, resulting in weak interfacial bonding force, which in turn leads to insignificant reinforcement effect, so as to obtain a graphene / PI composite material with both high strength and high toughness.

[0008] In order to achieve the above object, the technical solution adopted by the present invention is as follows:

[0009] A method for preparing a graphene / PI composite material comprises the following steps:

[0010] (1) Obtaining graphene oxide (GO) by oxidation method;

[0011] (2) chemically etching the graphene oxide obtained in step (1) to obtain porous graphene oxide (PGO);

[0012] (3) re-oxidizing the porous graphene oxide obtained in step (2) by strong acid to obtain secondary oxidized porous graphene oxide (O-PGO) powder;

[0013] (4) covalently modifying the secondary oxidized porous graphene oxide powder obtained in step (3) to obtain active porous graphene oxide (MO-PGO) powder modified with carboxyl functional groups;

[0014] (5) adding the active porous graphene oxide powder modified with carboxyl functional groups obtained in step (4) into an organic solvent, dispersing it by ultrasonication, adding 4,4'-diaminodiphenyl ether (ODA) and stirring it evenly, and then adding bisphenol A diether dianhydride (BPADA), reacting at room temperature to obtain a porous graphene oxide / polyamic acid (MO-PGO / PAA) composite dispersion;

[0015] (6) Casting the porous graphene oxide / polyamic acid composite dispersion obtained in step (5) on a substrate to form a film, vacuum drying, and heating to perform an imidization reaction to obtain a MO-PGO / PI composite material.

[0016] In step (1), GO can be prepared by various methods in the prior art. The graphene oxide of the present invention is prepared by an improved Hummers method. The prepared graphene oxide is ultrasonically exfoliated, cleaned, and centrifuged to obtain a GO slurry. The ultrasonic exfoliation method is described in Patent No.: ZL201110372309.X.

[0017] In step (2), the chemical etching adopts oxidation etching method or nanoparticle catalytic etching method to form a large number of nanopores on the surface of graphene oxide.

[0018] Preferably, in step (2), the graphene oxide is chemically etched with hydrogen peroxide, the concentration of hydrogen peroxide is 20-40wt.%, preferably 30wt.%, the reaction time is 2-5 hours, the reaction temperature is 85-110°C, and the size of the etched nanopores is 1-2nm.

[0019] Preferably, in step (3), the porous graphene oxide is reoxidized with concentrated nitric acid or concentrated sulfuric acid, the reaction temperature is 80-100°C, the reaction time is 3-10 hours, and after the reaction, it is washed with deionized water for multiple times, centrifuged to neutrality, and freeze-dried. Preferably, the strong acid is concentrated nitric acid, the reaction temperature is 85-90°C, and the reaction time is 5-7 hours. In step (2), after chemical etching, PGO undergoes different degrees of reduction, so that the oxygen-containing functional groups on its surface are reduced, which is not conducive to the dispersion and covalent modification of GO. Step (3) can increase the oxygen-containing functional groups of PGO, such as carboxyl and hydroxyl groups. Among them, the carboxyl group is an active functional group that can directly participate in the in-situ polymerization reaction and enhance the interfacial bonding strength between GO and PI; and the hydroxyl group can be used for covalent modification to further enhance the content of active functional groups.

[0020] Preferably, in step (4), the covalent modification reagent is any one of chloroacetic acid, succinic acid acyl peroxide or aminocaproic acid, preferably chloroacetic acid, the reaction time is 1 to 3 hours, and the modification mechanism is: first, the electrophilic functional group phosgene reacts with the hydroxyl group by electrophilic addition reaction, and then the acyl chloride is eliminated, thereby grafting the carboxyl group at the hydroxyl group. Compared with O-PGO, the carboxyl content of MO-PGO is increased, and the activity and active site content are further enhanced. After modification, it is washed with deionized water several times, centrifuged to neutrality, and freeze-dried.

[0021] Preferably, in step (5), the ultrasonic time is 0.5 to 3 hours, the organic solvent is N,N-dimethylformamide (DMF) and / or N,N-dimethylacetamide (DMAC), and the reaction time is 6 to 24 hours, preferably 8 to 12 hours.

[0022] Preferably, in step (6), the porous graphene oxide / polyamic acid composite dispersion is cast into a film on the surface of a glass substrate, and then vacuum dried at 60 to 120° C. for 3 to 24 hours.

[0023] Preferably, in step (6), the imidization reaction is carried out at 100-300° C. for 0.5-2 hours.

[0024] Furthermore, the present invention also claims protection for the graphene / PI composite material prepared by the above preparation method.

[0025] The present invention successfully forms nanopores on the surface of GO by chemical etching, and further grafts carboxyl functional groups on the edges of the nanopores to successfully prepare active porous GO (MO-PGO) modified with carboxyl functional groups, which greatly increases the active site content of GO. When compounded with PI, the rich active sites of MO-PGO enhance its dispersibility in PI and the interfacial bonding strength with PI, thereby preparing a MO-PGO / PI composite material with both high strength and high toughness.

[0026] Beneficial effects:

[0027] The present invention obtains active porous GO by chemically etching and covalently modifying GO. Compared with the traditional GO covalently modified by edge active sites, the surface of the GO contains more abundant active functional groups, which solves the problem that GO has poor dispersibility in PI and few active sites, resulting in weak interface bonding force, and thus insignificant enhancement effect. The present invention can significantly improve the strength and toughness of PI by adding a very small amount of active porous GO, and the improvement effect is far better than unmodified GO and traditional GO covalently modified by edge active sites. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] The present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments, and the above and / or other advantages of the present invention will become more clear.

[0029] Figure 1 It is a schematic diagram of the structural and functional group changes of GO→PGO→O-PGO→MO-PGO in the process of preparing MO-PGO according to the present invention.

[0030] Figure 2 These are transmission electron microscope images of (a) PGO, (b) O-PGO, and (c) MO-PGO of the present invention.

[0031] Figure 3 The figures are X-ray photoelectron spectra of (a) GO, (b) PGO, (c) O-PGO and (d) MO-PGO of the present invention, as well as the peak fitting curves of each chemical bond and the peak area ratio, which specifically illustrate the functional group changes of GO→PGO→O-PGO→MO-PGO during the preparation of MO-PGO.

[0032] Figure 4 It is the tensile stress-strain curve of all embodiments and comparative examples in the present invention. DETAILED DESCRIPTION

[0033] The present invention can be better understood with reference to the following examples.

[0034] Example 1

[0035] Combination Figure 1 The preparation process of the MO-PGO powder and the MO-PGO / PI composite material of the present invention is as follows:

[0036] (1) 1 g of natural graphite powder was cooled in an ice-water bath, and 120 mL of concentrated sulfuric acid (98 wt.%) and 13 mL of phosphoric acid (≥ 85 wt.%) were added in sequence, and stirred for 10 minutes to obtain a uniform mixture; 7 g of potassium permanganate was slowly added to the above mixture under stirring conditions, and stirred for 30 minutes; then the temperature of the reaction system was raised to 50°C, and after reacting for 4 hours, 100 mL of deionized water and 10 mL of hydrogen peroxide (30 wt.%) were added in sequence and mixed uniformly; finally, the mixture was washed with deionized water until the pH was 5-7, and deionized water was added for ultrasonic exfoliation to obtain a GO dispersion;

[0037] (2) adding 10 mL of hydrogen peroxide (30 wt.%) to the GO dispersion obtained in step (1), stirring at 95° C. for 4 hours, washing with deionized water for multiple times and centrifuging to collect the lower layer slurry, i.e., PGO slurry;

[0038] (3) taking 40 mL of the PGO slurry obtained in step (2), adding 48 mL of concentrated nitric acid (68 wt.%), reacting at 90° C. for 12 hours, then washing with deionized water for multiple times, centrifuging, and freeze-drying to obtain O-PGO powder;

[0039] (4) taking 0.1 g of the O-PGO powder obtained in step (3), adding 1.2 g of sodium hydroxide and 1 g of chloroacetic acid, ultrasonicating for 2 hours, washing with deionized water for multiple times, centrifuging, and freeze-drying to obtain MO-PGO powder;

[0040] (5) Take 0.015 g of the MO-PGO powder obtained in step (4), add 11.2 g of DMF, ultrasonically disperse for 1 hour, add 0.5556 g of ODA and stir for 1 hour, add 1.4444 g of BPADA, and react at room temperature for 12 hours to obtain a MO-PGO / PAA composite dispersion;

[0041] (6) Casting the MO-PGO / PAA composite dispersion obtained in step (5) onto a glass surface to form a film, and drying it in a vacuum drying oven at 60° C. for 12 hours; then moving it into an oven and maintaining it at 100, 150, 200 and 300° C. for 1 hour each to carry out an imidization reaction, thereby preparing a MO-PGO / PI composite material.

[0042] Table 1 shows the N element content of GO, PGO, O-PGO, and MO-PGO grafted by reaction with ODA in Example 1. The specific reaction conditions are: GO, PGO, O-PGO, and MO-PGO are added to 11.3g DMF respectively, ultrasonically dispersed for 1 hour, 0.5556g ODA is added, and the reaction is carried out at room temperature and under nitrogen protection for 12 hours. After the reaction is completed, the unreacted ODA is washed away with DMF. The product is freeze-dried to obtain a powder, and X-ray photoelectron spectroscopy is performed to analyze the grafting of different GOs with ODA by the N element content. It can be seen that the N element content on MO-PGO is 3.58wt.%, which is 143% of GO, which shows that the abundant active sites on MO-PGO significantly improve its grafting rate with ODA, indicating that the interface bonding ability between MO-PGO and PI is greatly improved; relatively, the N element content of PGO with less active site content is only 2.13wt.%. This shows that chemical etching and covalent modification of GO in the present invention can significantly improve the interfacial bonding ability between GO and PI.

[0043] Table 1

[0044] sample GO PGO O-PGO MO-PGO N element content (wt.%) 2.50 2.13 2.92 3.58

[0045] The PGO, O-PGO and MO-PGO in Example 1 were characterized by transmission electron microscopy. The results are shown in the attached figure. Figure 2 As shown. The results show that, under the premise of keeping the sheet intact, there are abundant nanopore structures on the surface of PGO, O-PGO and MO-PGO, and the size is about 1-2nm. The GO, PGO, O-PGO and MO-PGO in Example 1 were characterized by X-ray photoelectron spectroscopy, and the peak fitting and peak area ratio of each chemical bond were calculated. The results are shown in the attached figure. Figure 3 The results show that the carboxyl functional group contents of O-PGO and MO-PGO are significantly increased, reaching 132% and 149% of GO respectively.

[0046] Example 2

[0047] (1) The preparation method of GO dispersion is the same as that in Example 1;

[0048] (2) taking the GO dispersion obtained in step (1), adding 0.02 g of nickel acetate, stirring evenly, freeze-drying, then reacting at 800° C. for 2 hours, washing and centrifuging with dilute hydrochloric acid and deionized water multiple times in sequence to obtain PGO slurry;

[0049] (3) The remaining steps and conditions are the same as those in Example 1 to obtain a MO-PGO / PI composite material.

[0050] Example 3

[0051] The reaction time at 50° C. in step (1) of Example 1 was reduced from 4 hours to 2 hours, while the other steps and conditions remained unchanged to obtain a MO-PGO / PI composite material.

[0052] Example 4

[0053] The ultrasonic time in step (4) of Example 1 was increased from 2 hours to 3 hours, and the other steps and conditions remained unchanged to obtain a MO-PGO / PI composite material.

[0054] Comparative Example 1

[0055] 11.2 g of DMF was weighed, 0.5556 g of ODA was added, and the mixture was stirred for 1 hour. 1.4444 g of BPADA was added, and the mixture was reacted at room temperature for 12 hours to obtain a PAA / DMF solution. The solution was used to prepare PI in the same manner as in step (6) of Example 1.

[0056] Comparative Example 2

[0057] (1) preparing a GO dispersion by the same method as in Example 1, and freeze-drying to obtain GO powder;

[0058] (2) The GO powder obtained in step (1) is directly used to reinforce PI. The preparation method is the same as that in Example 1 to prepare a GO / PI composite material.

[0059] Comparative Example 3

[0060] (1) PGO slurry was prepared by the same method as in Example 1, and freeze-dried to obtain PGO powder;

[0061] (2) The PGO powder obtained in step (1) is directly used to reinforce PI. The preparation method is the same as that in Example 1 to prepare a PGO / PI composite film.

[0062] Comparative Example 4

[0063] (1) preparing a GO dispersion by the same method as in Example 1, and freeze-drying to obtain GO powder;

[0064] (2) taking 0.1 g of the GO powder obtained in step (1), adding 100 mL of deionized water, 1.2 g of sodium hydroxide and 1 g of chloroacetic acid, ultrasonicating for 1 hour, washing and centrifuging with deionized water several times, and freeze-drying to obtain chloroacetic acid-modified GO powder;

[0065] (3) Take 0.015 g of the chloroacetic acid-modified GO powder obtained in step (2) and use it to reinforce PI. The steps and conditions are the same as those in Example 1 to prepare a chloroacetic acid-modified GO / PI composite material.

[0066] Table 2 shows the tensile properties of all embodiments and comparative examples of the present invention, and the test standard thereof refers to the international standard ISO1184-1983. It can be seen that: in Example 1, GO is chemically etched and covalently modified, and its chemical site content is greatly increased, and its interface bonding ability with PI is significantly improved. The tensile strength at break and the elongation at break of the composite material are increased by 133% and 630% respectively compared with the pure PI material; Example 2 adopts the nanoparticle catalytic etching method. During the reaction at 800°C for 2 hours, on the one hand, nanopores are formed, and on the other hand, GO is highly reduced. The active oxygen-containing functional groups generated by oxidation in the later stage are relatively low in content compared with the oxidation etching method, so the tensile properties are relatively low; in Example 3, the oxidation time of GO is only half of that in Example 1, resulting in a lower active site of GO than in Example 1, and the modification effect is reduced compared with Example 1; in Example 4, the ultrasonic time during the reaction with chloroacetic acid is extended from 2 hours to 3 hours, resulting in a reduction in the size of GO, thereby reducing the tensile properties. In contrast, in Comparative Example 2, GO was directly added to PI, in Comparative Example 3, GO was chemically etched, and in Comparative Example 4, GO was edge-modified, but the active site content of GO was not effectively increased, and the tensile strength at break and elongation at break of the composite material were not significantly improved. This shows that the active porous graphene oxide in the present invention can significantly improve the tensile strength at break and elongation at break of the PI material.

[0067] Table 2

[0068] Example 1 Example 2 Example 3 Example 4 Tensile strength at break (MPa) 136.9±7.2 82.0±7.8 90.0±4.3 113.5±5.2 Elongation at break (%) 95.6±6.2 76.2±5.3 83.2±7.9 91.3±6.3 Young's modulus(GPa) 2.44±0.32 1.85±0.26 1.62±0.18 2.32±0.58 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Tensile strength at break (MPa) 58.8±3.8 54.8±5.2 68.4±2.1 77.0±3.1 Elongation at break (%) 13.1±2.2 6.9±1.7 7.0±0.8 46.7±6.2 Young's modulus(GPa) 1.31±0.11 1.38±0.21 1.32±0.09 1.70±0.14

[0069] The present invention provides a graphene / PI composite material and a method for preparing the same. There are many methods and approaches to implement the technical solution. The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention. All components not specified in this embodiment can be implemented using existing technologies.

Claims

1. A method for preparing a graphene / PI composite material, characterized in that: The steps include: (1) Obtaining graphene oxide by oxidation method; (2) chemically etching the graphene oxide obtained in step (1) to obtain porous graphene oxide; (3) re-oxidizing the porous graphene oxide obtained in step (2) by strong acid to obtain secondary oxidized porous graphene oxide powder; (4) covalently modifying the secondary oxidized porous graphene oxide powder obtained in step (3) to obtain active porous graphene oxide powder modified with carboxyl functional groups; (5) adding the active porous graphene oxide powder modified with carboxyl functional groups obtained in step (4) into an organic solvent, dispersing it by ultrasonication, adding 4,4'-diaminodiphenyl ether and stirring it evenly, and then adding bisphenol A type diether dianhydride, reacting at room temperature to obtain a porous graphene oxide / polyamic acid composite dispersion; (6) casting the porous graphene oxide / polyamic acid composite dispersion obtained in step (5) on a substrate to form a film, vacuum drying, and heating to carry out an imidization reaction to obtain; In step (1), the graphene oxide is prepared by ultrasonic exfoliation, washing and centrifugation using the Hummers method to obtain a GO dispersion; In step (2), the chemical etching adopts a nanoparticle catalytic etching method, taking the GO dispersion obtained in step (1), adding 0.02 g of nickel acetate, stirring evenly, freeze-drying, and then reacting at 800 ° C for 2 hours, washing with dilute hydrochloric acid and deionized water in turn, and centrifuging to obtain a PGO slurry, and etching nanopores with a size of 1-2 nm; In step (3), the porous graphene oxide is re-oxidized with concentrated nitric acid or concentrated sulfuric acid at a reaction temperature of 80 to 100° C. for a reaction time of 3 to 10 hours. After the reaction is completed, the porous graphene oxide is washed with deionized water, centrifuged, and freeze-dried; In step (4), chloroacetic acid is used as a covalent modification reagent to achieve grafting of carboxyl groups at the hydroxyl groups. After modification, the product is washed with deionized water, centrifuged, and freeze-dried.

2. The method for preparing the graphene / PI composite material according to claim 1, characterized in that: In step (5), the ultrasonic time is 0.5 to 3 hours, the organic solvent is N,N-dimethylformamide and / or N,N-dimethylacetamide, and the reaction time is 6 to 24 hours.

3. The method for preparing the graphene / PI composite material according to claim 1, characterized in that: In step (6), the porous graphene oxide / polyamic acid composite dispersion is cast onto the surface of a glass substrate to form a film, and then vacuum dried at 60-120° C. for 3-24 hours.

4. The method for preparing the graphene / PI composite material according to claim 1, characterized in that: In step (6), the imidization reaction is carried out at 100-300 °C for 0.5-2 hours.

5. The graphene / PI composite material prepared by the preparation method according to any one of claims 1 to 4.

Citation Information

Patent Citations

  • Porous graphene / polymer composite structure and preparation method and application thereof

    CN103146024A

  • Preparation method of graphene / polyimide composite material

    CN105440678A

  • Preparation method of water-dispersible conducting graphene

    CN106744834A

  • High-efficiency electrocatalyst composite material based on graphene aerogel of hierarchical pore structure and preparation method and application of material

    CN109300701A

  • Method for preparing high-dispersion graphene reinforced bismaleimide resin-based composite material

    CN110452415A