A TiB2 / TiC ceramic reinforced aluminum alloy matrix composite piston and preparation method thereof

By using the in-situ reaction technology of TiB2/TiC ceramic reinforced aluminum alloy matrix composite in piston preparation, the problems of ceramic particle agglomeration and poor interface bonding are solved, and the preparation of high-performance pistons is realized, with high strength, wear resistance and Characteristics of low thermal expansion coefficient.

CN116716508BActive Publication Date: 2024-11-22KUNMING UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310685339.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-12
Publication Date
2024-11-22
Estimated Expiration
2043-06-12

AI Technical Summary

Technical Problem

The existing preparation methods of ceramic-metal-based composites have problems such as agglomeration of ceramic particles, poor interface bonding, high cost and unfriendly environment. Traditional materials cannot meet the needs of high-performance pistons.

Method used

The preparation method of TiB2/TiC ceramic reinforced aluminum alloy matrix composite piston is adopted. By mixing boron carbide powder, titanium powder, boron powder, carbon powder and aluminum powder, ball milling into a prefabricated body, combined with electromagnetic stirring, mechanical stirring and ultrasonic stirring, A uniform dispersion and in-situ reaction of ceramic particles are achieved to generate micron-sized TiC and nano-sized TiB2 particles.

Benefits of technology

It effectively solves the problem of ceramic particles agglomeration, improves the strength, wear resistance and low thermal expansion coefficient of the material, reduces the preparation cost, and obtains a high-performance TiB2/TiC ceramic reinforced aluminum alloy matrix composite piston.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116716508B_ABST
    Figure CN116716508B_ABST
Patent Text Reader

Abstract

The present invention discloses a TiB 2 The invention relates to a piston of a composite material of a / TiC ceramic reinforced aluminum alloy matrix and a preparation method thereof, belonging to the technical field of metal matrix composite materials. The preparation method comprises: mixing boron carbide powder, titanium powder, boron powder, carbon powder and aluminum powder and pressing them into a preform by ball milling; melting the intermediate alloy A and adding it to the preform, adding a covering agent under electromagnetic stirring, lowering the temperature to 850°C and adding the intermediate alloy B, and sequentially stirring mechanically and ultrasonically stirring to obtain a mixed melt; refining, slagging and casting the mixed melt to obtain TiB 2 / TiC ceramic reinforced aluminum alloy matrix composite piston. The present invention presses the ceramic raw material into a preform, and directly reacts with the aluminum alloy liquid in situ to generate micron TiC particles and nano TiB 2 The ceramic particles are uniformly dispersed in the aluminum alloy matrix by combining electromagnetic stirring, mechanical stirring and ultrasonic stirring, which effectively solves the problem of ceramic particle agglomeration. 2 The composite piston made of TiC ceramic reinforced aluminum alloy matrix has high strength, wear resistance and low thermal expansion coefficient.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metal matrix composite materials, and in particular relates to a TiB2 / TiC ceramic reinforced aluminum alloy matrix composite material piston and a preparation method thereof. Background Art

[0002] As the requirements of automobiles for engine power, economy, environmental protection and reliability become more and more stringent, the piston, as an important part of automobile engines, works under high temperature, high pressure, high speed and poor lubrication conditions. The piston is in direct contact with high-temperature gas, and the instantaneous temperature can reach more than 2500K. Therefore, it is seriously heated, and the heat dissipation conditions are very poor. Therefore, the temperature of the piston is very high when working, up to 600-700K at the top, and the temperature distribution is very uneven; the top of the piston is under great gas pressure, so the performance of the piston directly determines the performance of the vehicle, but traditional materials can no longer meet the needs of today's automobile piston performance. It is urgent to develop new materials for pistons that are both high-performance and economical.

[0003] Particle-reinforced metal matrix composites are one of the most promising advanced materials in the 21st century. They have high specific strength, high specific stiffness, high specific modulus, and good high temperature performance. They are also wear-resistant, fatigue-resistant, have low thermal expansion coefficients, and good thermal conductivity. Particle-reinforced aluminum matrix composites are highly valued for their simple production process, low cost, and isotropic materials. They can adjust the performance of composite materials by changing the size, volume fraction, and heat treatment process of the reinforcing particles. They have broad application prospects in the field of automobile manufacturing.

[0004] In recent years, there are more and more methods for preparing ceramic-metal matrix composite materials. According to the different ways of adding particles, the preparation methods of ceramic reinforced aluminum matrix composite materials are generally divided into two categories: external addition method and endogenous method. The external addition method has problems such as easy surface pollution and poor interface bonding between matrix and reinforcement. For example, Chinese invention patent CN115921798A prepares composite piston by combining external addition of titanium carbide ceramic particles with mechanical stirring. The method uses the external addition method, which will cause the surface of the added particles to be polluted, resulting in the deterioration of the interface strength between the matrix and the particles, which is not conducive to the improvement of material properties and simple mechanical stirring cannot solve the small-sized agglomeration. The endogenous method can be subdivided into many types, among which the contact reaction method has the problem of large-scale agglomeration of ceramic particles. For example, Chinese invention patent CN1422971A uses an in-situ self-generated method to prepare Al2O3 / TiC reinforced aluminum matrix composite piston. The method uses the method of reacting the blown gas with the alloy element to prepare the composite material. During the preparation process, argon gas needs to be introduced as a protective gas. The experimental process is difficult to control and the cost is high, and the particles are prone to agglomeration. Chinese invention patent CN108796316A adopts an in-situ autogenous method to prepare a TiB2-reinforced aluminum-based composite piston. This method uses a mixed salt method to prepare the composite piston, which is not environmentally friendly and only generates a single reinforcement particle. Summary of the invention

[0005] In view of the above-mentioned shortcomings of the prior art, the present invention provides a TiB2 / TiC ceramic reinforced aluminum alloy matrix composite piston and a preparation method thereof.

[0006] To achieve the above object, the technical solution adopted by the present invention is: a method for preparing a TiB2 / TiC ceramic reinforced aluminum alloy matrix composite piston, comprising the following steps:

[0007] (1) mixing boron carbide powder, titanium powder, boron powder, carbon powder and aluminum powder uniformly, ball milling and pressing into a preform;

[0008] (2) melting the master alloy A into a molten liquid to a temperature of 950-1050° C., then adding the preform, completely dissolving the preform under electromagnetic stirring, adding a covering agent and keeping the temperature for 10-40 min, lowering the temperature to 850° C., adding the master alloy B and keeping the temperature for 10 min, and then sequentially using mechanical stirring and ultrasonic stirring to obtain a mixed melt;

[0009] (3) refining and deslagging the mixed melt, and then transferring it to a casting device to prepare a TiB2 / TiC ceramic reinforced aluminum alloy matrix composite piston;

[0010] Master alloy A and master alloy B are raw materials for aluminum alloy matrix; master alloy A is composed of aluminum silicon alloy, aluminum nickel alloy and aluminum iron alloy; master alloy B is composed of aluminum copper alloy, aluminum titanium alloy, aluminum magnesium alloy, aluminum zinc alloy, aluminum zirconium alloy, aluminum cerium alloy and pure aluminum.

[0011] The present invention suppresses the anisotropic growth of primary silicon crystals through electromagnetic stirring, promotes the spheroidization of primary silicon crystals and the transformation of columnar crystals to equiaxed crystals, thereby suppressing the harmful effects of primary silicon crystals and improving the performance of composite materials.

[0012] In the present invention, boron powder and carbon powder are introduced into the ceramic preform, so that the reaction can be carried out more fully, the problem of reactant residue can be solved, and the generation of harmful intermediate product Al3Ti can be reduced. The characteristics of the finally generated micron particle TiC can significantly improve the strength, hardness and wear resistance of the aluminum-based composite material and the advantages of the nano particle TiB2 can maintain good plasticity and toughness while improving the strength are utilized to prepare a high-performance TiB2 / TiC ceramic reinforced aluminum alloy matrix composite material. The present invention also changes the ratio of carbon powder and boron powder, thereby changing the ratio of the generated titanium diboride and titanium carbide, and finally realizes a high-performance micro-nano ceramic particle reinforced aluminum-based composite material with high strength, high wear resistance, low thermal expansion coefficient and casting performance.

[0013] The amount of the preform added in the present invention is determined according to the volume fraction of the ceramic phase to be prepared in the TiB2 / TiC ceramic reinforced aluminum alloy matrix composite material.

[0014] The present invention generates intermetallic compounds Al3CuNi and Al7Cu4Ni by adding Cu, Ni and Al into an aluminum alloy matrix; adds Mg and silicon to form Mg2Si, which helps to improve the high-temperature strength of the material; and the added Ce can promote further dispersion of particles.

[0015] As a preferred embodiment of the present invention, the rotation speed of the mechanical stirring is 400 rpm to 800 rpm, and the time is 10 to 30 minutes.

[0016] As a preferred embodiment of the present invention, the power of the ultrasonic stirring is 1000w-3000w, and the time is 3-10min.

[0017] As a preferred embodiment of the present invention, the molar ratio of the boron carbide powder, titanium powder and aluminum powder is 3:1-2:6-8, and the boron powder and carbon powder account for 1%-2% of the mass of the preform.

[0018] As a preferred embodiment of the present invention, the aluminum alloy matrix includes the following components in mass percentage: Si: 12% to 18%, Cu: 1.5% to 5.0%, Mg: 0.3% to 1.0%, Ni: 0.5% to 4%, Ti: 0.1% to 3.5%, Zn: 1% to 3%, Zr: 0.5% to 2.0%, Fe: 0.5% to 1.5%, Ce: 0.1% to 1.0%, single impurity: ≤0.05%, total impurities: ≤0.15% and balance Al.

[0019] As a preferred embodiment of the present invention, the particle size of the boron carbide powder, titanium powder, boron powder, carbon powder and aluminum powder is 5-500 microns.

[0020] As a preferred embodiment of the present invention, the rotation speed of the ball mill is 200-400r / min.

[0021] As a preferred embodiment of the present invention, the parameters of the casting equipment are: filling pressure of 0.1MPa to 0.3MPa, punching speed of 10 to 20cm / s, and holding time of 20 to 60s.

[0022] The covering agent described in the present invention is a commonly used covering agent in the art. The present invention uses the covering agent for heat preservation to ensure that the preform and the alloy melt fully react.

[0023] The present invention also claims protection for the TiB2 / TiC ceramic reinforced aluminum alloy matrix composite material piston prepared by the preparation method of the TiB2 / TiC ceramic reinforced aluminum alloy matrix composite material piston.

[0024] As a preferred embodiment of the present invention, the TiB2 / TiC ceramic phase of the TiB2 / TiC ceramic reinforced aluminum alloy matrix composite piston includes micron-sized TiC particles and nano-sized TiB2 particles.

[0025] The size of the TiC particles is less than 1.5 micrometers, and the size of the TiB2 ceramic particles is less than 300 nanometers.

[0026] The volume fraction of TiB2 / TiC ceramics in the TiB2 / TiC ceramics reinforced aluminum alloy matrix composite material piston of the present invention is 10%.

[0027] Compared with the prior art, the present invention has the following beneficial effects:

[0028] (1) The present invention presses the ceramic phase raw material into a preform, and directly reacts it with the eutectic aluminum-silicon alloy liquid in situ to generate micron-phase TiC particles and nano-phase TiB2 particles. The in-situ reacted ceramic particles are uniformly dispersed in the aluminum alloy matrix by combining electromagnetic stirring, mechanical stirring and ultrasonic stirring, which effectively solves the problems of ceramic particle agglomeration and difficulty in dispersion, while reducing the preparation cost.

[0029] (2) Compared with the single-phase ceramic reinforced aluminum alloy composite material, the TiB2 / TiC ceramic reinforced aluminum alloy matrix composite piston prepared by the preparation method of the present invention has high strength, high wear resistance, low thermal expansion coefficient and casting performance due to the mixing effect and size effect between different reinforcement particles. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 This is a three-dimensional model diagram of the TiB2 / TiC ceramic reinforced aluminum alloy matrix composite piston of the present invention.

[0031] Figure 2 This is a stress-strain curve diagram of the TiB2 / TiC ceramic reinforced aluminum alloy matrix composite material piston at 350°C. DETAILED DESCRIPTION

[0032] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments.

[0033] Example 1

[0034] A method for preparing a TiB2 / TiC ceramic reinforced aluminum alloy matrix composite piston comprises the following steps:

[0035] (1) Boron carbide powder, titanium powder, boron powder, carbon powder and aluminum powder are mixed uniformly, and after being ball-milled alternately at a speed of 200 r / min for 1 hour, the uniformly mixed powder is placed in an automatic tablet press to press a preform to obtain a cylindrical preform with a diameter of 28 mm and a height of 15 mm; the particle sizes of boron carbide powder, titanium powder, boron powder, carbon powder and aluminum powder are all 5 to 500 μm, the molar ratio of titanium powder, boron carbide powder and aluminum powder is 3:1:6, the amount of boron powder added is 1% of the mass of the preform, and the amount of carbon powder added is 2% of the mass of the preform;

[0036] (2) The master alloy A was melted into a molten liquid at a temperature of 1000° C., and then 520 g of the preform was added. The preform was fully reacted under electromagnetic stirring, and a covering agent was added to keep the temperature for 40 min. The temperature was lowered to 850° C., and the master alloy B was added to keep the temperature for 10 min. Then, mechanical stirring was performed for 10 min at a speed of 700 rpm, and ultrasonic stirring was performed for 6 min at a power of 2000 W to obtain a mixed melt.

[0037] (3) The mixed melt is refined and slag-beaten, and then transferred to a low-pressure casting device to prepare a piston with a volume fraction of 10% TiB2 / TiC ceramic reinforced aluminum alloy matrix composite material; the parameters of the casting equipment are: filling pressure of 0.3 MPa, punching speed of 10 cm / s, and holding time of 60 s.

[0038] The intermediate alloy A and the intermediate alloy B are raw materials for an aluminum alloy matrix; the intermediate alloy A is composed of an aluminum silicon alloy, an aluminum nickel alloy and an aluminum iron alloy; the intermediate alloy B is composed of an aluminum copper alloy, an aluminum titanium alloy, an aluminum magnesium alloy, an aluminum zinc alloy, an aluminum zirconium alloy, an aluminum cerium alloy and pure aluminum; the aluminum alloy matrix comprises the following components in mass percentage: Si: 12% to 18%, Cu: 1.5% to 5.0%, Mg: 0.3% to 1.0%, Ni: 0.5% to 4%, Ti: 0.1% to 3.5%, Zn: 1% to 3%, Zr: 0.5% to 2.0%, Fe: 0.5% to 1.5%, Ce: 0.1% to 1.0%, a single impurity: ≤0.05%, a total impurity: ≤0.15% and a balance of Al.

[0039] Example 2

[0040] A method for preparing a TiB2 / TiC ceramic reinforced aluminum alloy matrix composite piston comprises the following steps:

[0041] (1) Boron carbide powder, titanium powder, boron powder, carbon powder and aluminum powder are mixed uniformly, and after being ball-milled alternately at a speed of 400 r / min for 1 hour, the uniformly mixed powder is placed in an automatic tablet press to press a preform to obtain a cylindrical preform with a diameter of 28 mm and a height of 15 mm; the particle sizes of boron carbide powder, titanium powder, boron powder, carbon powder and aluminum powder are all 5 to 500 μm, the molar ratio of titanium powder, boron carbide powder and aluminum powder is 3:1:6, the amount of boron powder added is 2% of the mass of the preform, and the amount of carbon powder added is 1% of the mass of the preform;

[0042] (2) The master alloy A was melted into a molten liquid at a temperature of 1000° C., and then 520 g of the preform was added. The preform was fully reacted under electromagnetic stirring, and a covering agent was added to keep the temperature for 30 min. The temperature was lowered to 850° C., and the master alloy B was added to keep the temperature for 10 min. Then, mechanical stirring was performed for 10 min at a speed of 800 rpm, and ultrasonic stirring was performed for 6 min at a power of 2000 W to obtain a mixed melt.

[0043] (3) The mixed melt is refined and slag-beaten, and then transferred to a low-pressure casting device to prepare a piston with a volume fraction of 10% TiB2 / TiC ceramic reinforced aluminum alloy matrix composite material; the parameters of the casting equipment are: filling pressure of 0.1 MPa, punching speed of 20 cm / s, and holding time of 20 s.

[0044] The intermediate alloy A and the intermediate alloy B are raw materials for an aluminum alloy matrix; the intermediate alloy A is composed of an aluminum silicon alloy, an aluminum nickel alloy and an aluminum iron alloy; the intermediate alloy B is composed of an aluminum copper alloy, an aluminum titanium alloy, an aluminum magnesium alloy, an aluminum zinc alloy, an aluminum zirconium alloy, an aluminum cerium alloy and pure aluminum; the aluminum alloy matrix comprises the following components in mass percentage: Si: 12% to 18%, Cu: 1.5% to 5.0%, Mg: 0.3% to 1.0%, Ni: 0.5% to 4%, Ti: 0.1% to 3.5%, Zn: 1% to 3%, Zr: 0.5% to 2.0%, Fe: 0.5% to 1.5%, Ce: 0.1% to 1.0%, a single impurity: ≤0.05%, a total impurity: ≤0.15% and a balance of Al.

[0045] Example 3

[0046] A method for preparing a TiB2 / TiC ceramic reinforced aluminum alloy matrix composite piston comprises the following steps:

[0047] (1) Boron carbide powder, titanium powder, boron powder, carbon powder and aluminum powder are mixed uniformly, and after being ball-milled alternately at a speed of 400 r / min for 1 hour, the uniformly mixed powder is placed in an automatic tablet press to press a preform to obtain a cylindrical preform with a diameter of 28 mm and a height of 15 mm; the particle sizes of boron carbide powder, titanium powder, boron powder, carbon powder and aluminum powder are all 5 to 500 μm, the molar ratio of titanium powder, boron carbide powder and aluminum powder is 3:1:6, the amount of boron powder added is 1.5% of the mass of the preform, and the amount of carbon powder added is 1.5% of the mass of the preform;

[0048] (2) The master alloy A was melted into a molten liquid to a temperature of 1000° C., and then 520 g of the preform was added. The preform was fully reacted under electromagnetic stirring, and a covering agent was added to keep the temperature for 35 min. The temperature was lowered to 850° C., and the master alloy B was added to keep the temperature for 10 min. Then, mechanical stirring was performed for 10 min at a speed of 800 rpm, and ultrasonic stirring was performed for 10 min at a power of 2400 W to obtain a mixed melt.

[0049] (3) The mixed melt is refined and slag-beaten, and then transferred to a low-pressure casting device to prepare a piston with a volume fraction of 10% TiB2 / TiC ceramic reinforced aluminum alloy matrix composite material; the parameters of the casting equipment are: filling pressure of 0.1 MPa, punching speed of 20 cm / s, and holding time of 20 s.

[0050] The intermediate alloy A and the intermediate alloy B are raw materials for an aluminum alloy matrix; the intermediate alloy A is composed of an aluminum silicon alloy, an aluminum nickel alloy and an aluminum iron alloy; the intermediate alloy B is composed of an aluminum copper alloy, an aluminum titanium alloy, an aluminum magnesium alloy, an aluminum zinc alloy, an aluminum zirconium alloy, an aluminum cerium alloy and pure aluminum; the aluminum alloy matrix comprises the following components in mass percentage: Si: 12% to 18%, Cu: 1.5% to 5.0%, Mg: 0.3% to 1.0%, Ni: 0.5% to 4%, Ti: 0.1% to 3.5%, Zn: 1% to 3%, Zr: 0.5% to 2.0%, Fe: 0.5% to 1.5%, Ce: 0.1% to 1.0%, a single impurity: ≤0.05%, a total impurity: ≤0.15% and a balance of Al.

[0051] Example 4

[0052] A method for preparing a TiB2 / TiC ceramic reinforced aluminum alloy matrix composite piston comprises the following steps:

[0053] (1) Boron carbide powder, titanium powder, boron powder, carbon powder and aluminum powder are mixed uniformly, and after being ball-milled alternately in forward and reverse rotation at a speed of 350 r / min for 1 hour, the uniformly mixed powder is placed in an automatic tablet press to press a preform to obtain a cylindrical preform with a diameter of 28 mm and a height of 15 mm; the particle sizes of boron carbide powder, titanium powder, boron powder, carbon powder and aluminum powder are all 5 to 500 μm, the molar ratio of titanium powder, boron carbide powder and aluminum powder is 3:2:8, the amount of boron powder added is 1% of the mass of the preform, and the amount of carbon powder added is 2% of the mass of the preform;

[0054] (2) The master alloy A was melted into a molten liquid at a temperature of 1050° C., and then 520 g of the preform was added. The preform was fully reacted under electromagnetic stirring, and a covering agent was added to keep the temperature for 10 min. The temperature was lowered to 850° C., and the master alloy B was added to keep the temperature for 10 min. Then, mechanical stirring was performed for 30 min at a speed of 400 rpm, and ultrasonic stirring was performed for 3 min at a power of 1000 W to obtain a mixed melt.

[0055] (3) The mixed melt is refined and slag-beaten, and then transferred to a low-pressure casting device to prepare a piston with a volume fraction of 10% TiB2 / TiC ceramic reinforced aluminum alloy matrix composite material; the parameters of the casting equipment are: filling pressure of 0.1 MPa, punching speed of 20 cm / s, and holding time of 20 s.

[0056] The intermediate alloy A and the intermediate alloy B are raw materials for an aluminum alloy matrix; the intermediate alloy A is composed of an aluminum silicon alloy, an aluminum nickel alloy and an aluminum iron alloy; the intermediate alloy B is composed of an aluminum copper alloy, an aluminum titanium alloy, an aluminum magnesium alloy, an aluminum zinc alloy, an aluminum zirconium alloy, an aluminum cerium alloy and pure aluminum; the aluminum alloy matrix comprises the following components in mass percentage: Si: 12% to 18%, Cu: 1.5% to 5.0%, Mg: 0.3% to 1.0%, Ni: 0.5% to 4%, Ti: 0.1% to 3.5%, Zn: 1% to 3%, Zr: 0.5% to 2.0%, Fe: 0.5% to 1.5%, Ce: 0.1% to 1.0%, a single impurity: ≤0.05%, a total impurity: ≤0.15% and a balance of Al.

[0057] Comparative Example 1

[0058] A method for preparing an aluminum alloy material comprises the following steps:

[0059] (1) The master alloy A is melted into a molten liquid to a temperature of 1000°C, and electromagnetic stirring is used. A covering agent is added and the temperature is kept for 40 minutes. The temperature is lowered to 850°C, and the master alloy B is added and kept for 10 minutes. Then, mechanical stirring is used for 10 minutes at a speed of 700 rpm, and ultrasonic stirring is used for 6 minutes at a power of 2000 W to obtain a mixed melt.

[0060] (2) Refining and deslagging the mixed melt, and then transferring it to a low-pressure casting device to prepare an aluminum alloy material; the parameters of the casting device are: a filling pressure of 0.3 MPa, a punching speed of 10 cm / s, and a holding time of 60 s.

[0061] The intermediate alloy A and the intermediate alloy B are raw materials for an aluminum alloy matrix; the intermediate alloy A is composed of an aluminum silicon alloy, an aluminum nickel alloy and an aluminum iron alloy; the intermediate alloy B is composed of an aluminum copper alloy, an aluminum titanium alloy, an aluminum magnesium alloy, an aluminum zinc alloy, an aluminum zirconium alloy, an aluminum cerium alloy and pure aluminum; the aluminum alloy matrix comprises the following components in mass percentage: Si: 12% to 18%, Cu: 1.5% to 5.0%, Mg: 0.3% to 1.0%, Ni: 0.5% to 4%, Ti: 0.1% to 3.5%, Zn: 1% to 3%, Zr: 0.5% to 2.0%, Fe: 0.5% to 1.5%, Ce: 0.1% to 1.0%, a single impurity: ≤0.05%, a total impurity: ≤0.15% and a balance of Al.

[0062] Comparative Example 2

[0063] The only difference between the method for preparing a TiB2 / TiC ceramic reinforced aluminum alloy matrix composite piston and Example 1 is that in step (1), no boron powder and carbon powder are added.

[0064] Comparative Example 3

[0065] The only difference between the method for preparing a TiB2 / TiC ceramic reinforced aluminum alloy matrix composite piston and Example 1 is that in step (1), no boron powder is added and the amount of carbon powder added is 2% of the mass of the preform.

[0066] Comparative Example 4

[0067] The only difference between the method for preparing a TiB2 / TiC ceramic reinforced aluminum alloy matrix composite piston and Example 1 is that in step (1), no carbon powder is added and the amount of boron powder added is 1% of the mass of the preform.

[0068] Comparative Example 5

[0069] A method for preparing a TiB2 / TiC ceramic reinforced aluminum alloy matrix composite piston comprises the following steps:

[0070] (1) 90 g of titanium carbide powder with a particle size of 3 to 5 μm and 208 g of titanium diboride with a particle size of 300 to 500 nm were mixed uniformly, and the mixture was subjected to forward and reverse alternating ball milling at a speed of 200 r / min for 1 hour. The uniformly mixed powder was placed in an automatic tablet press and pressed into a preform to obtain a cylindrical ceramic particle blank with a diameter of 28 mm and a height of 15 mm;

[0071] (2) The intermediate alloy A is melted into a melt to a temperature of 1000°C, and then the prepared cylindrical ceramic particle blank is added, and the ceramic particles and the aluminum alloy melt are fully mixed under electromagnetic stirring, and a covering agent is added to keep the temperature for 40 minutes, and the temperature is reduced to 850°C, and the intermediate alloy B is added to keep the temperature for 10 minutes, and then mechanical stirring is used for 10 minutes at a speed of 700 rpm, and ultrasonic stirring is used for 6 minutes at a power of 2000 W to obtain a mixed melt;

[0072] (3) The mixed melt is refined and slag-beaten, and then transferred to a low-pressure casting device to prepare a piston with a volume fraction of 10% TiB2 / TiC ceramic reinforced aluminum alloy matrix composite material; the parameters of the casting equipment are: filling pressure of 0.3 MPa, punching speed of 10 cm / s, and holding time of 60 s.

[0073] The intermediate alloy A and the intermediate alloy B are raw materials for an aluminum alloy matrix; the intermediate alloy A is composed of an aluminum silicon alloy, an aluminum nickel alloy and an aluminum iron alloy; the intermediate alloy B is composed of an aluminum copper alloy, an aluminum titanium alloy, an aluminum magnesium alloy, an aluminum zinc alloy, an aluminum zirconium alloy, an aluminum cerium alloy and pure aluminum; the aluminum alloy matrix comprises the following components in mass percentage: Si: 12% to 18%, Cu: 1.5% to 5.0%, Mg: 0.3% to 1.0%, Ni: 0.5% to 4%, Ti: 0.1% to 3.5%, Zn: 1% to 3%, Zr: 0.5% to 2.0%, Fe: 0.5% to 1.5%, Ce: 0.1% to 1.0%, a single impurity: ≤0.05%, a total impurity: ≤0.15% and a balance of Al.

[0074] Comparative Example 6

[0075] A method for preparing a TiB2 / TiC ceramic reinforced aluminum alloy matrix composite piston comprises the following steps:

[0076] (1) 90 g of titanium carbide powder with a particle size of 3 to 5 μm and 208 g of titanium diboride with a particle size of 3 to 5 μm were mixed uniformly, and the mixture was subjected to forward and reverse alternating ball milling at a speed of 200 r / min for 1 hour. The uniformly mixed powder was placed in an automatic tablet press and pressed into a preform to obtain a cylindrical ceramic particle blank with a diameter of 28 mm and a height of 15 mm;

[0077] (2) The intermediate alloy A is melted into a melt to a temperature of 1000°C, and then the cylindrical ceramic particle blank is added, and the preform is fully reacted under electromagnetic stirring, and a covering agent is added to keep the temperature for 40 minutes, and the temperature is reduced to 850°C, and the intermediate alloy B is added to keep the temperature for 10 minutes, and then mechanical stirring is used for 10 minutes at a speed of 700 rpm, and ultrasonic stirring is used for 6 minutes at a power of 2000 W to obtain a mixed melt;

[0078] (3) The mixed melt is refined and slag-beaten, and then transferred to a low-pressure casting device to prepare a piston with a volume fraction of 10% TiB2 / TiC ceramic reinforced aluminum alloy matrix composite material; the parameters of the casting equipment are: filling pressure of 0.3 MPa, punching speed of 10 cm / s, and holding time of 60 s.

[0079] The intermediate alloy A and the intermediate alloy B are raw materials for an aluminum alloy matrix; the intermediate alloy A is composed of an aluminum silicon alloy, an aluminum nickel alloy and an aluminum iron alloy; the intermediate alloy B is composed of an aluminum copper alloy, an aluminum titanium alloy, an aluminum magnesium alloy, an aluminum zinc alloy, an aluminum zirconium alloy, an aluminum cerium alloy and pure aluminum; the aluminum alloy matrix comprises the following components in mass percentage: Si: 12% to 18%, Cu: 1.5% to 5.0%, Mg: 0.3% to 1.0%, Ni: 0.5% to 4%, Ti: 0.1% to 3.5%, Zn: 1% to 3%, Zr: 0.5% to 2.0%, Fe: 0.5% to 1.5%, Ce: 0.1% to 1.0%, a single impurity: ≤0.05%, a total impurity: ≤0.15% and a balance of Al.

[0080] Comparative Example 7

[0081] A method for preparing a TiB2 / TiC ceramic reinforced aluminum alloy matrix composite piston comprises the following steps:

[0082] (1) 90 g of titanium carbide powder with a particle size of 300 to 500 nanometers and 208 g of titanium diboride with a particle size of 300 to 500 nanometers were mixed uniformly, and the mixture was subjected to forward and reverse alternating ball milling at a speed of 200 r / min for 1 hour. The uniformly mixed powder was placed in an automatic tablet press and pressed into a preform to obtain a cylindrical ceramic particle blank with a diameter of 28 mm and a height of 15 mm;

[0083] (2) The intermediate alloy A is melted into a melt to a temperature of 1000°C, and then the cylindrical ceramic particle blank is added, and the preform is fully reacted under electromagnetic stirring, and a covering agent is added to keep the temperature for 40 minutes, and the temperature is reduced to 850°C, and the intermediate alloy B is added to keep the temperature for 10 minutes, and then mechanical stirring is used for 10 minutes at a speed of 700 rpm, and ultrasonic stirring is used for 6 minutes at a power of 2000 W to obtain a mixed melt;

[0084] (3) The mixed melt is refined and slag-beaten, and then transferred to a low-pressure casting device to prepare a piston with a volume fraction of 10% TiB2 / TiC ceramic reinforced aluminum alloy matrix composite material; the parameters of the casting equipment are: filling pressure of 0.3 MPa, punching speed of 10 cm / s, and holding time of 60 s.

[0085] The intermediate alloy A and the intermediate alloy B are raw materials for an aluminum alloy matrix; the intermediate alloy A is composed of an aluminum silicon alloy, an aluminum nickel alloy and an aluminum iron alloy; the intermediate alloy B is composed of an aluminum copper alloy, an aluminum titanium alloy, an aluminum magnesium alloy, an aluminum zinc alloy, an aluminum zirconium alloy, an aluminum cerium alloy and pure aluminum; the aluminum alloy matrix comprises the following components in mass percentage: Si: 12% to 18%, Cu: 1.5% to 5.0%, Mg: 0.3% to 1.0%, Ni: 0.5% to 4%, Ti: 0.1% to 3.5%, Zn: 1% to 3%, Zr: 0.5% to 2.0%, Fe: 0.5% to 1.5%, Ce: 0.1% to 1.0%, a single impurity: ≤0.05%, a total impurity: ≤0.15% and a balance of Al.

[0086] Effect example

[0087] The tensile strength, elastic modulus and thermal expansion coefficient of the TiB2 / TiC ceramic reinforced aluminum alloy matrix composite pistons prepared in Examples 1-4 and Comparative Examples 1-7 were tested. The results are shown in Table 1.

[0088] Table 1

[0089] Tensile strength (MPa) Elastic modulus(GPa) <![CDATA[Coefficient of thermal expansion (10 -6 / K)]]> Example 1 116.2 126 16.3 Example 2 127.6 133 17.6 Example 3 135.8 129 16.5 Example 4 109.2 117 18.1 Comparative Example 1 52.5 40 26.1 Comparative Example 2 63.1 98 20.1 Comparative Example 3 75.3 92 19.3 Comparative Example 4 68.4 106 18.5 Comparative Example 5 94.9 121 16.8 Comparative Example 6 70.6 109 17.2 Comparative Example 7 60.3 100 16.5

[0090] According to Table 1, compared with the samples prepared by the examples and comparative examples, the mechanical effect of the TiB2 / TiC ceramic reinforced aluminum alloy matrix composite piston described in the examples is better. According to Example 1 and Comparative Examples 2-4, it can be seen that the ceramic phase raw material lacks one or all of boron powder and carbon powder, which has a greater impact on the material performance, because the addition of carbon powder and boron powder can consume the unreacted titanium powder and the Ai3Ti in the organization that is not conducive to the performance, and generate ceramic particles that are beneficial to the material performance, and the generated titanium diboride and titanium carbide can enhance the performance of the material in all directions. According to Example 1 and Comparative Example 5, it can be seen that the performance of the TiB2 / TiC ceramic reinforced aluminum alloy matrix composite piston described in Example 1 is better, because compared with the external particle method, the particles prepared by the in-situ autogenous method are small in size, clean in surface, and have high bonding strength with the matrix interface, so that the composite material prepared by the in-situ autogenous method has more superior performance. According to Example 1 and Comparative Examples 6-7, the size of the dual-phase ceramic particles has a greater impact on the material because micron particles can significantly improve the strength and hardness of aluminum-based composite materials, but the plastic toughness is greatly reduced; while nanoparticles can maintain good plastic toughness while improving strength, but due to the large specific surface energy of nanoparticles and easy agglomeration, it is difficult to prepare high volume fraction particle-reinforced aluminum-based composite materials, so the application of traditional aluminum-based composite materials in high-tech fields is subject to certain restrictions. The design concept of micro-nano hybrid particle reinforcement is adopted to give full play to the advantages and coupling effects of each reinforcement phase to prepare a high-performance hybrid particle-reinforced aluminum-based composite material.

[0091] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A method for preparing a TiB2 / TiC ceramic reinforced aluminum alloy matrix composite piston, characterized in that: The steps include: (1) mixing boron carbide powder, titanium powder, boron powder, carbon powder and aluminum powder uniformly, ball milling and pressing into a preform; (2) melting the master alloy A into a molten liquid to a temperature of 950-1050° C., then adding the preform, completely dissolving the preform under electromagnetic stirring, adding a covering agent and keeping the temperature for 10-40 min, lowering the temperature to 850° C., adding the master alloy B and keeping the temperature for 10 min, and then sequentially using mechanical stirring and ultrasonic stirring to obtain a mixed melt; (3) refining and deslagging the mixed melt, and then transferring it to a casting device to prepare a TiB2 / TiC ceramic reinforced aluminum alloy matrix composite piston; Master alloy A and master alloy B are raw materials for aluminum alloy matrix; master alloy A is composed of aluminum silicon alloy, aluminum nickel alloy and aluminum iron alloy; master alloy B is composed of aluminum copper alloy, aluminum titanium alloy, aluminum magnesium alloy, aluminum zinc alloy, aluminum zirconium alloy, aluminum cerium alloy and pure aluminum; The aluminum alloy matrix is ​​composed of the following components in mass percentage: composition: Si: 12% ~ 18%, Cu: 1.5% ~ 5.0%, Mg: 0.3% ~ 1.0%, Ni: 0.5% ~ 4%, Ti: 0.1% ~ 3.5%, Zn: 1% ~ 3%, Zr: 0.5% ~ 2.0%, Fe: 0.5% ~ 1.5%, Ce: 0.1% ~ 1.0%, single impurity: ≤ 0.05%, total impurity: ≤ 0.15% and the balance of Al; The molar ratio of the boron carbide powder, titanium powder and aluminum powder is 3:1-2:6-8, and the added amounts of the boron powder and carbon powder are 1%-2% of the mass of the preform respectively.

2. The method for preparing the TiB2 / TiC ceramic reinforced aluminum alloy matrix composite piston according to claim 1, characterized in that: The mechanical stirring has a rotation speed of 400 rpm to 800 rpm and a stirring time of 10 to 30 minutes.

3. The method for preparing the TiB2 / TiC ceramic reinforced aluminum alloy matrix composite piston according to claim 1, characterized in that: The power of the ultrasonic stirring is 1000w-3000w, and the time is 3-10min.

4. The method for preparing the TiB2 / TiC ceramic reinforced aluminum alloy matrix composite piston according to claim 1, characterized in that: The particle sizes of the boron carbide powder, titanium powder, boron powder, carbon powder and aluminum powder are 5-500 microns.

5. The method for preparing the TiB2 / TiC ceramic reinforced aluminum alloy matrix composite piston according to claim 1, characterized in that: The parameters of the casting equipment are: filling pressure of 0.1MPa-0.3MPa, punching speed of 10-20cm / s, and holding time of 20-60s.

6. A TiB2 / TiC ceramic reinforced aluminum alloy matrix composite piston prepared by the method for preparing a TiB2 / TiC ceramic reinforced aluminum alloy matrix composite piston according to any one of claims 1 to 5.

7. The TiB2 / TiC ceramic reinforced aluminum alloy matrix composite piston according to claim 6, characterized in that: The TiB2 / TiC ceramic reinforced aluminum alloy matrix composite piston comprises micron-sized TiC particles and nano-sized TiB2 particles; the size of the TiC particles is less than 1.5 microns, and the size of the TiB2 ceramic particles is less than 300 nanometers.

8. The TiB2 / TiC ceramic reinforced aluminum alloy matrix composite piston according to claim 7, characterized in that: The volume fraction of the TiB2 / TiC ceramic phase in the TiB2 / TiC ceramic reinforced aluminum alloy matrix composite material piston is 10%.