An environmentally friendly SiC heat storage material using PVC as raw material and a preparation method thereof

By combining the SiC porous skeleton prepared from PVC plastic with the phase change material, a highly thermally conductive SiC ceramic composite phase change material is formed, which solves the problems of low thermal conductivity and environmental pollution of traditional thermal storage materials, and realizes efficient and low-cost thermal storage materials. Preparation and recycling.

CN116751063BActive Publication Date: 2024-10-01NANJING UNIV OF AERONAUTICS & ASTRONAUTICS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310647232.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-02
Publication Date
2024-10-01
Estimated Expiration
2043-06-02

AI Technical Summary

Technical Problem

The thermal conductivity of traditional phase change heat storage materials is low, which results in a prolonged heat storage process and increased heat loss, which hinders the large-scale and commercial use of heat storage systems. At the same time, the preparation of porous media materials is complex, energy-consuming, and harmful to the environment.

Method used

PVC plastic is used as the precursor, SiC porous skeleton is prepared through dehalogenation and carbonization processes, and combined with phase change materials to form SiC ceramic composite phase change materials with high thermal conductivity. Vacuum impregnation technology is used to improve the filling rate and thermal conductivity of the phase change materials. .

Benefits of technology

It significantly improves the thermal conductivity and heat storage density of heat storage materials, reduces preparation costs, is environmentally friendly, solves the problems of plastic recycling and energy utilization, and improves heat storage efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116751063B_ABST
    Figure CN116751063B_ABST
Patent Text Reader

Abstract

The present invention discloses an environmentally friendly SiC heat storage material using PVC as raw material and a preparation method thereof. The heat storage material is prepared by a composite of a SiC ceramic skeleton and a multi-element phase change material. The SiC skeleton is a high thermal conductivity porous filler obtained by carbonizing in an inert atmosphere and melting silicon at high temperature in a vacuum using waste PVC plastic as raw material. After the porous SiC skeleton is treated, the pores are rich and interconnected, and the porosity can reach 90%. After that, it is composited with a phase change material to provide an internally connected high thermal conductivity network for the phase change material, greatly increasing the thermal conductivity of the composite material. The rich pores enable the phase change enthalpy of the composite material to reach more than 90% of that of the pure phase change material. The method uses PVC plastic as raw material to prepare a high thermal conductivity, high heat storage density, and environmentally friendly heat storage material. Its excellent performance can not only reduce carbon emissions, but also effectively alleviate the environmental pollution problem of plastics.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a heat storage material and a preparation method thereof, and in particular to an environmentally friendly SiC heat storage material using PVC as a raw material and a preparation method thereof. Background Art

[0002] The development of human society cannot get rid of its dependence on energy. As the speed of human social development gradually accelerates, the demand for energy has also begun to show an exponential growth trend in the past two decades. However, the shortage of traditional fossil energy and the adverse environmental changes caused by greenhouse gases such as carbon dioxide have caused widespread concern among people, and have put forward new requirements for countries around the world to find alternative energy solutions in a short period of time. Finding alternative energy and quickly realizing efficient utilization has become one of the most important issues in today's energy field.

[0003] Solar energy has become one of the key research objects in the current energy structure transformation of various countries due to its advantages such as being renewable, clean and widely distributed. However, solar energy is affected by the alternation of day and night, weather changes, etc., and cannot provide energy continuously and stably, resulting in insufficient development and mismatch between the supply side and the demand side. Since solar energy usually exists on the earth in the form of thermal energy, the development of solar energy absorption and thermal storage system coupling has become the most effective solution at present. It can store excess solar energy in the form of thermal energy, and release and convert it into electrical energy when needed, effectively solving the shortcoming of intermittent solar energy.

[0004] The most important thing in a heat storage system is the heat storage material, which directly determines the heat storage density of the heat storage system. Currently, there are three main types of heat storage: sensible heat, phase change, and thermochemical heat storage. Phase change heat storage has received widespread attention because its temperature remains almost unchanged during phase change, but its heat storage density is very high and it is relatively stable during operation. However, in practical applications, traditional phase change materials have extremely low thermal conductivity (usually less than 1W·m -1 ·K -1 ), which greatly prolongs the heat transfer time during the heat storage process. As a result, heat loss also increases, reducing the overall efficiency of the heat storage system and hindering the large-scale and commercial use of phase change heat storage systems. In order to solve this problem, researchers have proposed a research idea to embed high thermal conductivity porous skeletons into phase change materials to improve the comprehensive thermal conductivity of composite materials. These high thermal conductivity porous skeletons include but are not limited to graphene / graphene oxide aerogels, expanded graphite, metal foams, and porous ceramics (AlN, SiC, BN). Because these porous media can construct intricate high-speed heat transport channels in phase change materials, the composite materials have an exponential increase in thermal conductivity at the cost of extremely small heat storage density.

[0005] However, the raw materials used in the porous media materials mentioned above are extremely harmful to the environment, and the preparation methods are also quite complex and energy-intensive, so careful selection is required. For example, graphene-based aerogels require the use of highly corrosive reagents such as strong acids and strong alkalis in the preparation process; graphite materials need to be annealed in a high temperature environment of 3000°C in order to pursue high thermal conductivity. Therefore, high thermal conductivity ceramic materials have gradually come into the sight of researchers. Compared with traditional carbon materials, ceramic materials have better high temperature properties and corrosion resistance, and have extremely high research value. However, the forming technology of porous ceramics is relatively simple. The pore structure of porous ceramics prepared from powders or nanowires is uncontrollable, and the thermal conductivity is not high enough, which limits its use in the field of heat storage. Therefore, the strategy of using porous precursors as templates to ensure that the shape does not change much and directly transforming into porous ceramics has been favored by researchers. Plastics, as a huge and irreplaceable raw material used in modern society, also have problems such as difficulty in recycling and serious environmental pollution. Every year, there are countless marine and soil pollution caused by discarded plastics. At present, there are a lot of studies on the recycling and reuse of plastics, but there are few reports on the research strategy of directly converting waste plastics into useful materials in the energy field through a series of means. If it is possible to use plastics as precursors to prepare porous ceramic skeletons and combine them with phase change materials for heat storage, it will promote the development of waste recycling, environmental protection, energy utilization and other aspects at the same time. Summary of the invention

[0006] Purpose of the invention: The present invention aims to provide a SiC ceramic composite phase change material with high thermal conductivity using PVC as raw material; another purpose of the present invention is to provide a method for preparing an environmentally friendly SiC heat storage material using PVC as raw material.

[0007] Technical solution: The environmentally friendly SiC heat storage material with PVC as raw material described in the present invention is composited by a SiC porous skeleton and a phase change material; the phase change material is filled in the pores of the SiC skeleton, and the silicon carbide skeleton is prepared from waste PVC plastic, with a volume fraction between 8% and 15%.

[0008] Furthermore, the phase change material may be paraffin, alkyl acid, inorganic salt, etc. The volume filling rate of the phase change material in the heat storage material is between 75% and 90%.

[0009] The method for preparing the environmentally friendly SiC heat storage material using PVC as a raw material of the present invention comprises the following steps:

[0010] (1) Preparation of porous carbon templates using PVC plastic as raw material;

[0011] (2) Preparation of porous silicon carbide ceramics;

[0012] (3) The phase change material is filled into the porous silicon carbide skeleton by vacuum impregnation to obtain a composite heat storage material.

[0013] Furthermore, the carbon template in step (1) comprises the following preparation steps:

[0014] (11) Dehalogenation: Place the PVC plastic in a container and place it in a tube furnace, heat it in an inert gas environment and keep it warm to dehalogenate the plastic;

[0015] (12) Carbonization: Continue to increase the temperature in the furnace and keep it warm to ensure that the material is completely dehalogenated, and then continue to increase the temperature and keep it warm to completely carbonize the carbon skeleton;

[0016] (13) The temperature was then lowered to room temperature and a Cl - The samples were thoroughly washed with an aqueous solution and dried thoroughly.

[0017] Furthermore, the PVC plastic described in step (11) needs to be placed in a covered crucible or any container that can limit the expansion of the internal material but allow the gas to escape. The volume of the container is 1.5 to 2 times the volume of the PVC plastic placed therein to limit its free expansion. Its advantage is that the expansion in a limited space can make the material morphology controllable. More importantly, the pores of the carbon skeleton obtained by free expansion are closed, and the connectivity between the pores is poor, which prevents the impregnation of the phase change material and the heat storage density is not high. Under a limited volume, after the gas decomposes, in order to escape, it will break through the wall of the skeleton and form a channel connected to the outside world. The connectivity between the pores is high, and the impregnation rate of the phase change material is greatly improved.

[0018] Furthermore, in the heating process described in step (11), the heating rate should be less than or equal to 1°C / min. Too high a heating rate will cause the PVC plastic to undergo a too rapid dehalogenation process and deteriorate the pore structure. The heating temperature is 300°C to 350°C, and the holding time is 1 to 3 hours.

[0019] Furthermore, in step (12), the heating temperature for ensuring complete dehalogenation of the material is 400°C to 450°C, the heating temperature for complete carbonization of the carbon skeleton is 800°C to 1000°C, and the insulation time is 1h to 2h.

[0020] Furthermore, in the washing process described in step (13), a solution containing chloride ions, such as a saturated NaCl solution, needs to be used. Since additives such as lead stearate are added to PVC plastics during molding for flame retardancy and stability, the use of a solution containing chloride ions can dissolve lead ions in the form of coordinated ions. In addition, the selection of NaCl can promote the formation of β-SiC during molten silicon.

[0021] Furthermore, the porous silicon carbide ceramic described in step (2) comprises the following preparation steps:

[0022] (21) Molten silicon: The dried and completely carbonized carbon skeleton is placed in a crucible, and excess silicon powder is added, which is then placed in a vacuum melting furnace, heated and kept warm to perform a molten silicon reaction;

[0023] (22) Silicon removal: The smelting furnace is heated up and kept warm for a sufficient period of time until the excess silicon is removed.

[0024] Furthermore, the mass ratio of the excess silicon powder to the carbon skeleton in step (21) is 2.4 to 3, and should not be too much, otherwise the silicon removal process will take too long.

[0025] Furthermore, the molten silicon environment in step (21) is a vacuum environment. A vacuum environment is conducive to the diffusion of molten silicon powder into the carbon skeleton and is conducive to the removal of excess insoluble impurities.

[0026] Furthermore, the vacuum impregnation in step (3) specifically refers to: placing a SiC porous skeleton in a container and adding an excess of phase change material, raising the temperature to above the melting point of the phase change material in a vacuum environment, and then lowering it to room temperature to remove excess phase change material on the surface of the composite material.

[0027] Furthermore, the temperature in step (3) is raised to 40 to 100° C. above the melting point of the phase change material.

[0028] The preparation principle of the present invention is to optimize the method of dehalogenation of PVC plastics, and the expansion pyrolysis under limited space can obtain a skeleton with higher porosity and greater through-porosity. It can improve the impregnation rate of phase change materials (improve heat storage density) and improve the thermal conductivity. After obtaining the carbon skeleton, the sample is washed with a saturated chlorine-containing aqueous solution, and vacuum high-temperature molten silicon is used to effectively remove residual impurities and improve thermal conductivity.

[0029] The present invention uses PVC plastic as a precursor to provide a new idea for the recycling of plastics and a new method for preparing heat storage materials. The silicon carbide skeleton provides a good heat conduction channel for the heat transport of the phase change material, and the thermal conductivity of the composite material is significantly improved compared to the pure phase change material. The porosity and through-hole rate are greatly improved during the preparation process, so that as much phase change material as possible can fill the skeleton, ensuring the high heat storage density of the composite material.

[0030] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages: (1) The heat storage material has a high thermal conductivity. The present invention improves the preparation technology and successfully removes the residual stubborn impurities in PVC, effectively improving the purity of the SiC skeleton and further improving the thermal conductivity; (2) The SiC thermal conductive porous skeleton is prepared using PVC plastic as a precursor, which has the characteristics of environmental friendliness, low cost, high stability, etc., and at the same time improves the two major problems of difficult plastic recycling and low energy storage efficiency; (3) The preparation method can use different PVC templates to obtain SiC skeletons of corresponding shapes. The preparation method is simple, low cost, wide controllable range, and high practicality. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is a simplified diagram of the synthesis process of silicon carbide skeleton;

[0032] Figure 2 (a) is the SEM image of waste PVC plastic; (b) and (c) are the SEM images of carbon skeletons prepared without and with limited space expansion, respectively; (d) is the SEM image of SiC skeleton; (e) and (f) are the EDS energy spectra of Si and C element distribution of SiC skeleton; (g) is the XRD spectrum of carbon skeleton and SiC skeleton without impurity removal treatment;

[0033] Figure 3 (a) Thermal conductivity of phase change materials, carbon skeleton composites, and SiC composites; (b) Heat flow curves and phase change enthalpy of phase change materials, SiC composites without limited space expansion, and SiC composites with limited expansion;

[0034] Figure 4 It is a comparison chart of thermal conductivity and latent heat retention rate of phase change composite materials prepared from industrial waste solids reported in literature data in the present invention. DETAILED DESCRIPTION

[0035] The technical solution of the present invention is further described below in conjunction with specific embodiments.

[0036] The method for measuring each parameter in the embodiment of the present invention is:

[0037] 1. Use a laser thermal conductivity meter to measure the thermal conductivity of the material.

[0038] 2. Use differential scanning calorimeter to measure the heat flow curve of the material.

[0039] 3. Use differential scanning calorimeter to measure the phase change enthalpy of the material.

[0040] Example 1

[0041] Cut the PVC plastic into blocks of appropriate size, wash with anhydrous ethanol, and dry. Put it into a corundum crucible with a lid that is twice as large as the crucible, and place it in a tube furnace. In an Ar or N2 atmosphere, raise the temperature in the furnace to 320°C at a heating rate of 1°C / min, and keep it warm for 1 hour for dehalogenation. In this process, use saturated NaHCO3 solution and activated carbon for tail gas treatment. Then raise the temperature to 450°C at a heating rate of 1°C / min and keep it warm for 1 hour to ensure that it is fully dehalogenated. Then raise the temperature to 800°C at a heating rate of 1°C / min and anneal for 1 hour. Wait for the temperature to drop to room temperature and take out the dehalogenated carbon skeleton. Soak in a saturated NaCl solution for thorough washing and drying.

[0042] Place the dried carbon skeleton into a graphite crucible, and weigh silicon powder with a mass ratio of 1:2.4 and add it into it. Place the graphite crucible containing the sample into a vacuum melting furnace, raise the temperature to 1600°C at a heating rate of 20°C / min under a vacuum environment, and keep it warm for 1 hour to melt the silicon. Then raise the temperature to 1800°C at the same heating rate, and keep it warm for 1 hour to completely remove the excess silicon. When the temperature drops to room temperature, the SiC skeleton of the present invention is obtained. The schematic diagram of the synthesis process is shown below. Figure 1 shown.

[0043] Place the skeleton in a container of suitable size, add excess high enthalpy paraffin, and place it in a drying oven at 70°C. After the phase change material melts, keep it warm for another hour until it cools down to room temperature. Repeat this step once to ensure a high filling rate of the phase change material. After removing the excess phase change material on the surface, an environmentally friendly heat storage material made of PVC plastic is obtained.

[0044] Example 2

[0045] Select a PVC plastic pipe with a diameter of about 2 cm and cut it into small tubes of 5 to 10 cm in length. Clean it with anhydrous ethanol and deionized water to remove impurities such as surface oxide layer, light, and pyrolysis products. After it is dried, put it into a round bushing made of quartz or other high-temperature resistant materials, and put a quartz plug inside the tube. The volume ratio of the gap between the bushing and the plug to the volume of the PVC pipe is also controlled at about 2 / 1. Place it in a tubular furnace, and in an Ar or N2 atmosphere, raise the temperature in the furnace to 320°C at a heating rate of 1°C / min, and keep it warm for 1 hour for dehalogenation. In this process, saturated NaHCO3 solution and activated carbon are used for tail gas treatment. Then, the temperature is raised to 450°C at a heating rate of 1°C / min and kept warm for 1 hour to ensure that it is fully dehalogenated. Then, the temperature is raised to 800°C at a heating rate of 1°C / min and annealed for 1 hour. Wait for the temperature to drop to room temperature and take out the dehalogenated carbon skeleton. Soak in a saturated NaCl solution for thorough washing and drying. Subsequently, the dried carbon skeleton is placed in a graphite crucible, and silicon powder with a mass ratio of 1:2.4 is weighed and added thereto. The graphite crucible containing the sample is placed in a vacuum melting furnace, and the temperature is raised to 1600°C at a heating rate of 20°C / min under a vacuum environment, and kept warm for 1 hour to melt silicon. The temperature is then raised to 1800°C at the same heating rate, and kept warm for 1 hour to completely remove excess silicon. When the temperature drops to room temperature, the SiC skeleton of the present invention is obtained. Place the skeleton in a container of suitable size, add excess high enthalpy paraffin, and place it in a drying oven at 70°C. After the phase change material is melted, keep warm for another 1 hour to cool to room temperature. Repeat this step once to ensure a higher filling rate of the phase change material.

[0046] In this way, a cylindrical SiC heat storage material can be obtained. The cylindrical SiC heat storage material can be used for thermal management of batteries. When the battery is working under high load, the heat generated is large. At this time, the SiC heat storage material coated on the outer surface can absorb the heat released by the battery. When the temperature reaches the melting point of the phase change material, the temperature of the SiC heat storage material no longer continues to rise, ensuring that the battery operating temperature is low and stable. When the battery is in a relatively cold working environment, the SiC heat storage material can also provide a certain amount of heat, allowing the battery to work at a higher temperature relative to the environment and with higher efficiency. It can be widely used in scenarios such as electric vehicles and energy storage power stations.

[0047] Example 3

[0048] The preparation method is the same as that of Example 1

[0049] Take a large amount of sheet-type PVC plastic with a length, width and thickness of about 30cm, 15cm and 2cm, and perform the synthesis steps in Example 1 or Example 2. A large-sized flaky SiC porous material is obtained, and it is stacked into a piece and compounded with a large amount of low-melting point paraffin (melting point is 22°C to 28°C). Synthesize a large-sized SiC heat storage material and encapsulate it into a heat storage brick using cement and other materials. This heat storage brick can be built into an indoor decorative wall, which can absorb a large amount of heat from the environment during the day and control the indoor temperature between 22°C and 28°C. It slowly releases heat at night to ensure that the indoor temperature difference is small, which can reduce the need for the use of air conditioning and indoor electric heating equipment, thereby saving energy. Especially in areas with sufficient sunlight and large temperature difference between day and night, such as Xinjiang, Tibet, and Gansu. The heat storage brick can be laid on the roof or exterior wall, which can absorb a large amount of heat generated by sunlight during the day and release heat at night to heat the house.

[0050] In addition, the high-temperature heat storage bricks prepared by compounding large-sized SiC blocks with high-temperature molten salt (melting point greater than 220°C) can be put into use in concentrated solar power stations. When there is sufficient sunlight during the day, the excess heat energy collected by concentrated solar energy can be stored in high-temperature SiC heat storage bricks, and released in rainy weather or at night for power generation. By using latent heat storage, the energy storage density of the heat storage brick can be increased by more than 50% compared with the sensible heat storage of liquid molten salt (solar salt: NaNO3 / KNO3=60wt% / 40wt%) currently used in commercial applications.

[0051] Comparative Example

[0052] The preparation method is the same as that in Example 1, except that the dehalogenation and carbonization of the PVC plastic is carried out in an open space, that is, the sample is not placed in a crucible, and is cracked in a tubular furnace to obtain a carbon skeleton.

[0053] In the above preparation method, the use of a covered crucible with a volume ratio of 2 / 1 and the washing with a saturated NaCl solution are more important. Figure 2 As can be seen in the SEM image, Figure 2 (b) is the carbon skeleton obtained by cracking the sample in a tube furnace without putting it into a crucible. The pores are large, the number is small, and the connectivity between the pores is poor. Such a pore structure is not conducive to the filling of phase change materials. This will cause many voids to appear inside the composite material, which will reduce the heat storage density of the material. At the same time, the pores contain a large amount of air, which will significantly reduce the thermal conductivity of the material. Figure 2 (c) is the carbon skeleton obtained by cracking in a covered crucible. Its microstructure is significantly improved. The pores are small, uniform in size, and well connected. This is conducive to the filling of phase change materials. Figure 2It can be seen from the XRD spectrum of (g) that the carbon skeleton obtained by direct pyrolysis has many impurity peaks in addition to amorphous carbon and graphite. These impurity peaks are impurities formed because stabilizers and flame retardants such as lead stearate in PVC cannot be removed at high temperatures. These impurities, led by lead stearate, are neither soluble in water nor in organic solvents. However, they can form coordination compounds with chloride ions in the solution and dissolve in water. Therefore, it can be seen that the SiC skeleton after washing has no other impurity peaks except the characteristic peaks of SiC. These impurities not only affect the crystallization of SiC at high temperatures, but also affect the phonon transfer in the skeleton. Impurities will cause interfaces to form within the skeleton, resulting in strong scattering of phonons at the interface, resulting in a significant reduction in thermal conductivity. For example Figure 3 As shown in Figure 1, when the volume fraction of SiC skeleton is about 10%, the thermal conductivity can reach 2.4W / (m·K), which is 6 times that of pure phase change material. The heat storage density only loses 9.9%, and the melting enthalpy is 226.7J / g.

[0054] Figure 4 The thermal conductivity and latent heat retention of phase change composite materials prepared with industrial waste solids as raw materials reported in high-level international journals since 2019 are summarized in Table 1, and compared with the performance of the materials of the present invention. It can be found that the thermal conductivity and latent heat retention of silicon carbide porous skeleton phase change composite materials prepared with PVC are significantly at the leading level among these materials. Most of the materials reported in the literature can only achieve high thermal conductivity or high latent heat retention, but the materials reported in the present invention have both high levels of thermal conductivity and latent heat retention. This is due to the following points:

[0055] 1) The selected PVC material can produce carbon source, and there is only this kind of raw material.

[0056] 2) Limited volume expansion makes the material have small pores, interconnected pores, and rich pores, which is conducive to the filling of phase change materials.

[0057] 3) Saturated NaCl washes away excess impurities, reduces interface phonon scattering, and further improves thermal conductivity.

[0058] In addition, the volume preparation technology of the present invention does not require any highly polluting reagents. When preparing materials such as graphene, graphene oxide, and Mexene, a large amount of highly corrosive reagents such as hydrochloric acid, sulfuric acid, nitric acid, and sodium hydroxide need to be used. Compared with other SiC preparation methods, the silicon removal method of this method is also more environmentally friendly, and there is no need to use highly corrosive reagents such as hydrofluoric acid for etching. And there is no need to use other toxic and harmful inorganic and organic solvents for washing and other operations, and only low-cost, pollution-free reagents such as NaCl are required. Therefore, the materials and preparation methods described in the present invention are environmentally friendly and low-cost, and can solve the problems of plastic pollution and energy shortage at the same time.

[0059] Table 1 is a detailed comparison of thermal conductivity and latent heat retention of phase change composite materials prepared from industrial waste solids reported in the present invention and in literature data.

[0060] Table 1

[0061]

[0062] The references mentioned in Table 1 are as follows:

[0063] [1]Liu Y, Jiang Z, Zhang X, Wu B, Shen Y, Wu L, Zhang

[0064] [2] Singh P, Sharma RK, G, A,Gencel O,Tyagi V V.Expandedwaste glass / methyl palmitate / carbon nanofibers as effective shape stabilized and thermal enhanced composite phase change material for thermal energystorage[J].J.Energy.Storage.,2023,64:107205.

[0065] [3] Al-Gunaid T, P,Chriaa I,Karkri M,Mrlik M, M, T,Popelka A,Krupa I.Phase change materials designed from Tetra Pak waste and paraffin wax as unique thermal energy storage systems[J].J.Energy.Storage.,2023,64:107173.

[0066] [4]Xiong Y,Wang H,Wu Y,Zhang J,Li H,Xu Q,Zhang X,Li C,Ding Y.Carbideslag based shape-stable phase change materials for waste recycling andthermal energy storage[J].J.Energy.Storage.,2022,50:104256.

[0067] [5]Chen Q,Wang H,Gao H,Wang X,Ma B.Effects of porous silicon carbidesupports prepared from pyrolyzed precursors on the thermal conductivity andenergy storage properties of paraffin-based composite phase change materials[J].J.Energy.Storage.,2022,56:106046.

[0068] [6]Qu A,Zhao J,Peng H,Jiang F.Recycled blast furnace slag to form-stabilize NaNO3 with high performance for high-temperature thermal energystorage[J].J.Energy.Storage.,2022,55:105870.

[0069] [7]Xiong Y,Yao C,Ren J,Wu Y,Xu Q,Nie B,Li C,Ding Y.Waste semicoke ashutilized to fabricate shape-stable phase change composites for buildingheating and cooling[J].Constr.Build.Mater.,2022,361:129638.

[0070] [8]Luo Y,Li C,Zhang F,Li Z.Novel industrial waste-based shape-stabilized composite phase change materials with high heat storageperformance from calcium carbide furnace dust[J].Sol.Energy Mater.Sol.Cells,2022,242:111745.

[0071] [9]Wang Y,Bailey J,Zhu Y,Zhang Y,Boetcher S K S,Li Y,Wu C.Applicationof carbon nanotube prepared from waste plastic to phase change materials:Thepotential for battery thermal management[J].Waste Manage.,2022,154:96-104.

[0072]

[10] Liu P,Zhang Z,Gu X,Rao J,Shi J,Bian L.Fabrication of a novelshape-stabilized composite phase change material based on multivariatesupporting materials by using typical solid wastes[J].Constr.Build.Mater.,2020,240:118156.

[0073]

[11] Sari A,Saleh T A,Hekimoglu G,Tuzen M,Tyagi V V.Evaluation ofcarbonized waste tire for development of novel shape stabilized compositephase change material for thermal energy storage[J].Waste Manag,2020,103:352-360.

[0074]

[12] Zhang Y,Sun K,Kou Y,Wang S,Shi Q.Afacile strategy of constructingcomposite form-stable phase change materials with superior high thermalconductivity using silicagel industrial wastes[J].Sol.Energy,2020,207:51-58.

[0075]

[13] Liu C,Ma X,Du P,Rao Z.Fabrication of highly efficient thermalenergy storage composite from waste polystyrenes[J].Chem.Eng.Sci.,2020,216:115477.

[0076]

[14] Qian M,Li Z,Fan L,Wang H,Xu J,Zhao W,Huang F.Ultra-Light GrapheneTile-Based Phase-Change Material for Efficient Thermal and Solar EnergyHarvest[J].ACS Appl.Energ.Mater.,2020,3(6):5517-5522.

[0077]

[15] Zhang Y,Wang J,Yang X,Ali H M,Said Z,Liu C.Fabrication of shape-stabilized phase change materials based on waste plastics for energy storage[J].J.Energy.Storage.,2022,52(104973):104973.

[0078]

[16] Li R,Zhou Y,Duan X.A novel composite phase change material withparaffin wax in tailings porous ceramics[J].Appl.Therm.Eng.,2019,151:115-123.

Claims

1. An environmentally friendly SiC heat storage material using PVC as raw material, Features: The heat storage material is composed of a porous SiC skeleton and a phase change material, wherein the volume fraction of the porous SiC skeleton accounts for 8% to 15%, and the volume fraction of the phase change material accounts for 75% to 90%. The preparation method of the SiC heat storage material comprises the following steps: (1) Dehalogenation: The PVC plastic is placed in a container that can limit the expansion of the internal material but allow the gas to escape, and is placed in a tube furnace, heated and kept warm in an inert gas environment to dehalogenate the plastic; the volume of the container is 1.5 to 2 times the volume of the PVC plastic placed therein; (2) Carbonization: Continue to increase the temperature in the furnace and keep it warm to ensure that the material is completely dehalogenated, then continue to increase the temperature, and then anneal to completely carbonize the carbon skeleton; then reduce the temperature to room temperature and use a Cl-containing - The sample is thoroughly washed with an aqueous solution; (3) Molten silicon: The dried and completely carbonized carbon skeleton is placed in a crucible, excess silicon powder is added, and then placed in a vacuum melting furnace, heated and kept warm to carry out a molten silicon reaction; (4) Silicon removal: Continue to heat up the smelting furnace and keep it warm until the excess silicon is removed; (5) Composite: The obtained SiC skeleton is placed in a crucible and an excess of phase change material is added. The temperature is raised to above the melting point of the phase change material in a vacuum environment, and then lowered to room temperature. The excess phase change material on the surface of the composite material is removed to obtain an environmentally friendly SiC heat storage material made of PVC as raw material.

2. The environmentally friendly SiC heat storage material using PVC as raw material according to claim 1, Features: The phase change material is at least one of paraffin, alkyl acid or inorganic salt.

3. The environmentally friendly SiC heat storage material using PVC as raw material according to claim 1, Features: The raw material for preparing the porous SiC skeleton is waste PVC.

4. A method for preparing an environmentally friendly SiC heat storage material using PVC as a raw material as claimed in any one of claims 1 to 3, Features: The steps include: (1) Dehalogenation: The PVC plastic is placed in a container that can limit the expansion of the internal material but allow the gas to escape, and is placed in a tube furnace, heated and kept warm in an inert gas environment to dehalogenate the plastic; the volume of the container is 1.5 to 2 times the volume of the PVC plastic placed therein; (2) Carbonization: Continue to increase the temperature in the furnace and keep it warm to ensure that the material is completely dehalogenated, then continue to increase the temperature, and then anneal to completely carbonize the carbon skeleton; then reduce the temperature to room temperature and use a Cl-containing - The sample is thoroughly washed with an aqueous solution; (3) Molten silicon: The dried and completely carbonized carbon skeleton is placed in a crucible, excess silicon powder is added, and then placed in a vacuum melting furnace, heated and kept warm to carry out a molten silicon reaction; (4) Silicon removal: Continue to heat up the smelting furnace and keep it warm until the excess silicon is removed; (5) Composite: The obtained SiC skeleton is placed in a crucible and an excess of phase change material is added. The temperature is raised to above the melting point of the phase change material in a vacuum environment, and then lowered to room temperature. The excess phase change material on the surface of the composite material is removed to obtain an environmentally friendly SiC heat storage material made of PVC as raw material.

5. The method for preparing the environmentally friendly SiC heat storage material using PVC as raw material according to claim 4, Features: The heating temperature in step (1) is 300°C to 350°C, the holding time is 1 to 3 h, and the heating rate during the heating process is less than or equal to 1°C / min.

6. The method for preparing the environmentally friendly SiC heat storage material using PVC as raw material according to claim 4, Features: In step (2), the heating temperature for ensuring complete dehalogenation of the material is 400°C to 450°C, the heating temperature for completely carbonizing the carbon skeleton is 800°C to 1000°C, and the holding time is 1h to 2h.

7. The method for preparing the environmentally friendly SiC heat storage material using PVC as raw material according to claim 4, Features: The temperature after heating in step (3) is 1550°C to 1650°C, and the insulation time is 1h to 1.5h.

8. The method for preparing the environmentally friendly SiC heat storage material using PVC as raw material according to claim 4, Features: In step (3), the mass ratio of silicon powder to carbon skeleton is 2.4 to 3, and the molten silicon environment is vacuum.

9. The method for preparing the environmentally friendly SiC heat storage material using PVC as raw material according to claim 4, Features: The compounding process described in step (5) is carried out in a vacuum environment.

10. The method for preparing the environmentally friendly SiC heat storage material using PVC as raw material according to claim 4, Features: In step (5), the temperature is raised to 40 to 100° C. above the melting point of the phase change material.