A kind of highly dispersed carbon nanotube conductive slurry and preparation method thereof

By preparing high-efficiency dispersant and synergistic dispersant, combined with mechanical mixing and grinding treatment, the problem of insufficient dispersion and stability of carbon nanotube conductive paste is solved, and its conductive performance and quality is improved.

CN116759136BActive Publication Date: 2024-11-15ANHUI XINMINHUI NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310729065.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-16
Publication Date
2024-11-15
Estimated Expiration
2043-06-16

AI Technical Summary

Technical Problem

The dispersion and stability performance of carbon nanotube conductive paste on the market has poor performance, which affects its product performance.

Method used

Special chemical reactions are used to prepare high-efficiency dispersants and synergistic dispersants, and the dispersion performance and stability of carbon nanotubes are improved through mechanical mixing and grinding.

Benefits of technology

The dispersion and stability of the carbon nanotube conductive paste are improved, ensuring the excellent and quality of its conductive properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004298558850000081
    Figure BDA0004298558850000081
Patent Text Reader

Abstract

The present invention relates to the technical field of conductive pastes, and specifically to a highly dispersed carbon nanotube conductive paste and a preparation method thereof; the highly dispersed carbon nanotube conductive paste comprises the following components, calculated by weight content of 100%, including 0.8-8wt% carbon nanotubes, 0.07-3wt% high-efficiency dispersant, 0.05-1.5wt% synergistic dispersant, and the remainder being a solvent; the synergistic coordination between the high-efficiency dispersant and the synergistic dispersant prepared by the present invention not only enables the carbon nanotubes to gradually transition from a disordered state of aggregation to a smooth and orderly state, but also effectively increases the packing density of the carbon nanotubes, reduces the viscosity threshold generated when the carbon nanotubes are dispersed, and effectively improves their dispersion performance; it can be seen that the carbon nanotube conductive paste prepared by the present application not only has excellent conductivity, but also has excellent dispersion performance and stability performance, effectively ensuring its quality or grade.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of conductive pastes, in particular to a highly dispersed carbon nanotube conductive paste and a preparation method thereof. Background Art

[0002] Carbon nanotube conductive paste is a class of hybrid materials based on carbon nanotubes. Due to the unique extremely small size and excellent conductivity of carbon nanotubes, they can become a very valuable conductive material. Carbon nanotube conductive paste has many advantages, including: low impedance, excellent durability, excellent conduction behavior and variable energy storage capacity.

[0003] Carbon nanotube conductive paste plays an important role in electronic components, power systems, sensors, batteries, solar energy and other industries. For example, in the solar energy industry, solar cells using carbon nanotube conductive paste have overcome the high production cost problem of the original solar energy industry, greatly improving the availability and efficiency of the solar energy industry. Carbon nanotube conductive paste is also widely used in the heat dissipation system of electronic components, which can greatly improve the reliability and stability of electronic components. In addition, carbon nanotube conductive paste is also used to manufacture ultra-high efficiency, ultra-high capacity and high stability battery materials, which can be used in household appliances and automotive batteries, as well as other rechargeable batteries. Due to these characteristics, the application scope of carbon nanotube conductive paste is rapidly expanding, and there will be more application fields for carbon nanotube conductive paste to exert its excellent performance.

[0004] At present, although the carbon nanotube conductive paste on the market has excellent conductive properties, its own dispersion and stability are relatively poor, which to a certain extent affects the product performance of the carbon nanotube conductive paste. Based on the above, the present invention provides a highly dispersed carbon nanotube conductive paste and a preparation method thereof to solve the above-mentioned related technical problems. Summary of the invention

[0005] The purpose of the present invention is to provide a highly dispersed carbon nanotube conductive paste and a preparation method thereof. The prepared carbon nanotube conductive paste not only has good conductive properties, but also has good dispersion and stability properties, effectively ensuring its quality.

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] A highly dispersed carbon nanotube conductive paste comprises the following components based on 100% by mass: 0.8-8wt% carbon nanotubes, 0.07-3wt% high-efficiency dispersant, 0.05-1.5wt% synergistic dispersant, and the balance is solvent.

[0008] Furthermore, the preparation method of the high-efficiency dispersant comprises the following steps:

[0009] Step 1: Mix and stir the vinyl formic acid, the reaction intermediate and 3-mercaptopropionic acid in a mass ratio of 1:0.8-2.0:0.01-0.02, and the mixture is recorded as the first mixed component, which is stored and reserved for future use;

[0010] Step 2: Mix the reaction accelerator and deionized water in a mass ratio of 1:18-25 and stir evenly, the resultant is recorded as the second mixed component, and is stored for later use;

[0011] Step 3, distilled water and 0.25-0.58% of the reaction accelerator are mixed and stirred to obtain a reaction accelerator aqueous dispersion, and the temperature is raised to 65-75° C. under the protection of a nitrogen atmosphere; then the first mixed component and the second mixed component are simultaneously and slowly dripped into the reaction accelerator aqueous dispersion; after the dripping is completed, the temperature of the obtained mixture is raised to 93-98° C., and the mixture is kept at this temperature for 2-5 hours;

[0012] The amount of the first mixed component is 75-90% of the aqueous dispersion of the reaction accelerator; the amount of the second mixed component is 10-20% of the aqueous dispersion of the reaction accelerator;

[0013] Step 4: After the reaction is completed, the resulting components are naturally cooled to 35-45° C., and then the pH value is adjusted to 7.8-8.5. The final mixed material is the finished product of the high-efficiency dispersant.

[0014] Furthermore, the reaction accelerator is selected from any one of sodium persulfate, ammonium persulfate and potassium persulfate.

[0015] Furthermore, the preparation method of the reaction intermediate is: adding a dimethyl ketone solution of methylvinyl formate-N, N-dimethylaminoethyl ester with a concentration of 1.2 to 1.6 mol / L into the reaction equipment, and adding a dimethyl ketone solution of α-chlorotoluene with a volume of half and a concentration of 2.4 to 3.2 mol / L to the dimethyl ketone solution of dimethylaminoethyl methylvinyl formate while stirring; then raising the temperature of the obtained mixed component to 50 to 60° C., and stirring and reacting at this temperature for 4 to 6 hours; after the reaction is completed, dimethyl ketone in the product component is evaporated, and then ether is added for washing 3 to 5 times, and then filtered and dried to obtain the reaction intermediate.

[0016] Furthermore, the carbon nanotubes are selected from any one or more combinations of single-walled carbon nanotubes, double-walled carbon nanotubes, and multi-walled carbon nanotubes.

[0017] Furthermore, the synergistic dispersant is selected from any one or more combinations of polyethylene glycol octylphenyl ether, sodium carboxymethyl cellulose, sodium dodecyl sulfate, and polyvinyl pyrrolidone.

[0018] Furthermore, the solvent is selected from any one or more combinations of isopropanol, N-methylpyrrolidone, ethanol, and deionized water.

[0019] A method for preparing a highly dispersed carbon nanotube conductive slurry comprises the following steps:

[0020] S1. Accurately weigh various raw materials required for preparing highly dispersed carbon nanotube conductive slurry, and then transfer the high-efficiency dispersant, synergistic dispersant and solvent into a mixing device for mechanical mixing to mix the materials uniformly; after the materials are uniformly mixed, the obtained mixed liquid is stored and used for later use;

[0021] S2, adding carbon nanotubes to the mixed liquid obtained in S1 while stirring, and mechanically stirring to obtain a mixed slurry;

[0022] S3, transferring the mixed slurry obtained in step S2 into a grinding device, and subjecting it to sand grinding for 20 to 80 minutes using a grinding medium; after the grinding is completed, the result is a finished product of a highly dispersed carbon nanotube conductive slurry.

[0023] Furthermore, the grinding medium is selected from any one of aluminum dioxide beads, zirconium silicate beads, and zirconium dioxide beads, and the particle size of the grinding medium is 0.8 to 2.5 mm.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] In the present invention, a dimethyl ketone solution of dimethylaminoethyl methylvinyl formate and a dimethyl ketone solution of α-chlorotoluene are used as raw materials, and a reaction intermediate with high reaction activity is prepared through a specific chemical reaction. Then, the prepared reaction intermediate, vinyl formic acid and 3-mercaptopropionic acid are used as raw materials of the first mixed component, and they are mixed with a second mixed component composed of a reaction accelerator and deionized water to cause a chemical reaction, and finally a high-efficiency dispersant with excellent dispersibility is prepared. The synergistic effect between the prepared high-efficiency dispersant and the synergistic dispersant not only makes the carbon nanotubes gradually transition from a disordered state of agglomeration to a smooth and orderly state, but also effectively increases the packing density of the carbon nanotubes, reduces the viscosity threshold generated when the carbon nanotubes are dispersed, and effectively improves its dispersibility. It can be seen from this that the carbon nanotube conductive slurry prepared in the present application not only has excellent conductive properties, but also has excellent dispersibility and stability, effectively ensuring its quality or grade. DETAILED DESCRIPTION

[0026] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0027] Example 1

[0028] A highly dispersed carbon nanotube conductive paste comprises the following components based on 100% by mass: 0.8wt% single-walled carbon nanotubes, 0.07wt% high-efficiency dispersant, 0.05wt% polyethylene glycol octylphenyl ether, and the balance is isopropanol.

[0029] The preparation method of the high-efficiency dispersant comprises the following steps:

[0030] Step 1: Mix vinyl formic acid, reaction intermediate and 3-mercaptopropionic acid in a mass ratio of 1:0.8:0.01 and stir evenly, the obtained mixture is recorded as the first mixed component, and is stored for later use;

[0031] Step 2: Mix sodium persulfate and deionized water in a mass ratio of 1:18 and stir evenly, the mixture is recorded as the second mixed component, and is stored for later use;

[0032] Step 3, distilled water and 0.25% sodium persulfate by mass are mixed and stirred to obtain a sodium persulfate aqueous dispersion, and the temperature thereof is raised to 65° C. under the protection of a nitrogen atmosphere; then the first mixed component and the second mixed component are simultaneously and slowly dripped into the sodium persulfate aqueous dispersion; after the dripping is completed, the temperature of the obtained mixture is raised to 93° C., and the mixture is kept at this temperature for 2 hours;

[0033] The dosage of the first mixed component is 75% of the sodium persulfate aqueous dispersion; the dosage of the second mixed component is 10% of the sodium persulfate aqueous dispersion;

[0034] Step 4: After the reaction is completed, the resulting components are naturally cooled to 35° C., and then the pH value is adjusted to 7.8. The final mixed material is the finished product of the high-efficiency dispersant.

[0035] The preparation method of the reaction intermediate is as follows: a dimethyl ketone solution of N, N-dimethylaminoethyl methylvinyl formate with a concentration of 1.2 mol / L is added to a reaction device, and a dimethyl ketone solution of α-chlorotoluene with a volume of half and a concentration of 2.4 mol / L is added dropwise to the dimethyl ketone solution of dimethylaminoethyl methylvinyl formate while stirring; then the temperature of the obtained mixed component is raised to 50° C., and the mixture is stirred and reacted at this temperature for 4 hours; after the reaction is completed, the excess dimethyl ketone in the resultant component is evaporated, and ether is added for washing 3 times, and then the mixture is filtered and dried to obtain the reaction intermediate.

[0036] A method for preparing a highly dispersed carbon nanotube conductive slurry comprises the following steps:

[0037] S1. Accurately weigh various raw materials required for preparing highly dispersed carbon nanotube conductive slurry, and then transfer the high-efficiency dispersant, synergistic dispersant and solvent into a mixing device for mechanical mixing to mix the materials uniformly; after the materials are uniformly mixed, the obtained mixed liquid is stored and used for later use;

[0038] S2, adding carbon nanotubes to the mixed liquid obtained in S1 while stirring, and mechanically stirring to obtain a mixed slurry;

[0039] S3. The mixed slurry obtained in step S2 is transferred into a grinding device and subjected to sand milling treatment for 20 minutes using a grinding medium. After the grinding is completed, a finished product of a highly dispersed carbon nanotube conductive slurry is obtained. Alumina beads are used as the grinding medium, and the particle size of the grinding medium is 0.8 mm.

[0040] Example 2

[0041] The preparation method of the highly dispersed carbon nanotube conductive paste in this embodiment is basically the same as that in Example 1. The difference between the two is that the specific ratio of the raw materials used and the preparation methods of the high-efficiency dispersant and the reaction intermediates are different. The specific ratio of the raw materials used in this embodiment and the preparation methods of the high-efficiency dispersant and the reaction intermediates are as follows:

[0042] The highly dispersed carbon nanotube conductive paste comprises the following components based on 100% by weight: 5wt% double-walled carbon nanotubes, 2wt% high-efficiency dispersant, 1.0wt% sodium carboxymethyl cellulose, and the balance is N-methyl pyrrolidone.

[0043] The preparation method of the high-efficiency dispersant comprises the following steps:

[0044] Step 1: Mix and stir the vinyl formic acid, the reaction intermediate and 3-mercaptopropionic acid in a mass ratio of 1:1.5:0.015, and the mixture is recorded as the first mixed component, which is stored and reserved for future use;

[0045] Step 2: Mix ammonium persulfate and deionized water in a mass ratio of 1:20 and stir evenly, the resultant mixture is recorded as the second mixed component, and is stored for later use;

[0046] Step 3, distilled water and 0.45% of ammonium persulfate are mixed and stirred to obtain an ammonium persulfate aqueous dispersion, and the temperature is raised to 70° C. under the protection of a nitrogen atmosphere; then the first mixed component and the second mixed component are simultaneously and slowly dripped into the ammonium persulfate aqueous dispersion; after the dripping is completed, the temperature of the obtained mixture is raised to 95° C., and the mixture is kept at this temperature for 3 hours;

[0047] The dosage of the first mixed component is 85% of the aqueous dispersion of ammonium persulfate; the dosage of the second mixed component is 15% of the aqueous dispersion of ammonium persulfate;

[0048] Step 4: After the reaction is completed, the resulting components are naturally cooled to 40° C., and then the pH value is adjusted to 8.0. The final mixed material is the finished product of the high-efficiency dispersant.

[0049] The preparation method of the reaction intermediate is as follows: a dimethyl ketone solution of N, N-dimethylaminoethyl methylvinyl formate with a concentration of 1.4 mol / L is added into a reaction device, and a dimethyl ketone solution of α-chlorotoluene with a volume of half and a concentration of 3.0 mol / L is added dropwise into the dimethyl ketone solution of dimethylaminoethyl methylvinyl formate while stirring; then the temperature of the obtained mixed component is raised to 55° C., and the mixture is stirred and reacted at this temperature for 5 hours; after the reaction is completed, the excess dimethyl ketone in the resultant component is evaporated, and ether is added for washing 4 times, and then the mixture is filtered and dried to obtain the reaction intermediate.

[0050] Example 3

[0051] The preparation method of the highly dispersed carbon nanotube conductive paste in this embodiment is basically the same as that in Example 1. The difference between the two is that the specific ratio of the raw materials used and the preparation methods of the high-efficiency dispersant and the reaction intermediates are different. The specific ratio of the raw materials used in this embodiment and the preparation methods of the high-efficiency dispersant and the reaction intermediates are as follows:

[0052] The highly dispersed carbon nanotube conductive paste comprises the following components based on 100% by weight: 8wt% multi-walled carbon nanotubes, 3wt% high-efficiency dispersant, 1.5wt% sodium dodecyl sulfate, and the balance is ethanol.

[0053] The preparation method of the high-efficiency dispersant comprises the following steps:

[0054] Step 1: Mix and stir the vinyl formic acid, the reaction intermediate and 3-mercaptopropionic acid in a mass ratio of 1:2.0:0.02, and the mixture is recorded as the first mixed component, which is stored and used for later use;

[0055] Step 2: Mix potassium persulfate and deionized water in a mass ratio of 1:25 and stir evenly, the mixture is recorded as the second mixed component, and is stored for later use;

[0056] Step 3, distilled water and 0.58% potassium persulfate are mixed and stirred to obtain a potassium persulfate aqueous dispersion, and the temperature is raised to 75° C. under the protection of a nitrogen atmosphere; then the first mixed component and the second mixed component are simultaneously and slowly dripped into the potassium persulfate aqueous dispersion; after the dripping is completed, the temperature of the obtained mixture is raised to 98° C., and the mixture is kept at this temperature for 5 hours;

[0057] The dosage of the first mixed component is 90% of the potassium persulfate aqueous dispersion; the dosage of the second mixed component is 20% of the potassium persulfate aqueous dispersion;

[0058] Step 4: After the reaction is completed, the resulting components are naturally cooled to 45° C., and then the pH value is adjusted to 8.5. The final mixed material is the finished product of the high-efficiency dispersant.

[0059] The preparation method of the reaction intermediate is as follows: a dimethyl ketone solution of N, N-dimethylaminoethyl methylvinyl formate with a concentration of 1.6 mol / L is added into a reaction device, and a dimethyl ketone solution of α-chlorotoluene with a volume of half and a concentration of 3.2 mol / L is added dropwise into the dimethyl ketone solution of dimethylaminoethyl methylvinyl formate while stirring; then the temperature of the obtained mixed component is raised to 60° C., and the mixture is stirred and reacted at this temperature for 6 hours; after the reaction is completed, the excess dimethyl ketone in the resultant component is evaporated, and ether is added for washing 5 times, and then the mixture is filtered and dried to obtain the reaction intermediate.

[0060] The difference between Comparative Example 1 and Example 1 is that an equal amount of polyethylene glycol octylphenyl ether is used in this example to replace the high-efficiency dispersant prepared in the present invention.

[0061] The difference between Comparative Example 2 and Example 1 is that an equal amount of a high-efficiency dispersant is used in this example to replace polyethylene glycol octylphenyl ether.

[0062] Performance test: The relevant properties of the highly dispersed carbon nanotube conductive pastes prepared in equal amounts in Examples 1 to 3 and Comparative Examples 1 to 2 were tested, and the obtained experimental data were recorded in the following table:

[0063]

[0064] By comparing and analyzing the relevant data in the table, it can be seen that the carbon nanotube conductive paste prepared by the present invention not only has good conductive properties, but also has good dispersion and stability, which effectively guarantees its quality. Therefore, it is shown that the highly dispersed carbon nanotube conductive paste prepared by the present invention has a broader market prospect and is more suitable for promotion.

[0065] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0066] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A highly dispersed carbon nanotube conductive slurry, characterized in that: The highly dispersed carbon nanotube conductive paste comprises the following components based on 100% by weight: 0.8-8wt% carbon nanotubes, 0.07-3wt% high-efficiency dispersant, 0.05-1.5wt% synergistic dispersant, and the balance is solvent; The preparation method of the high-efficiency dispersant comprises the following steps: Step 1: Mix and stir the vinyl formic acid, the reaction intermediate and 3-mercaptopropionic acid in a mass ratio of 1:0.8-2.0:0.01-0.02, and the mixture is recorded as the first mixed component, which is stored and reserved for future use; Step 2: Mix the reaction accelerator and deionized water in a mass ratio of 1:18-25 and stir evenly, the resultant is recorded as the second mixed component, and is stored for later use; Step 3: Mix distilled water and 0.25-0.58% of a reaction accelerator and stir evenly to obtain a reaction accelerator aqueous dispersion, and raise its temperature to 65-75° C. under the protection of a nitrogen atmosphere; then slowly drip the first mixed component and the second mixed component into the reaction accelerator aqueous dispersion simultaneously; after the dripping is completed, raise the temperature of the obtained mixture to 93-98° C., and keep the mixture at this temperature for 2-5 hours; The amount of the first mixed component is 75-90% of the aqueous dispersion of the reaction accelerator; the amount of the second mixed component is 10-20% of the aqueous dispersion of the reaction accelerator; Step 4: After the reaction is completed, the resulting components are naturally cooled to 35-45° C., and then the pH thereof is adjusted to 7.8-8.

5. The final mixed material is the finished product of the high-efficiency dispersant; The preparation method of the reaction intermediate comprises the following steps: adding a dimethyl ketone solution of N, N-dimethylaminoethyl methylvinyl formate with a concentration of 1.2-1.6 mol / L into a reaction device, and dripping a dimethyl ketone solution of α-chlorotoluene with a volume of half of the dimethyl ketone solution and a concentration of 2.4-3.2 mol / L into the dimethyl ketone solution of dimethylaminoethyl methylvinyl formate while stirring; then raising the temperature of the obtained mixed component to 50-60° C., and stirring and reacting at this temperature for 4-6 hours; after the reaction is completed, dimethyl ketone in the product component is evaporated, and then ether is added for washing for 3-5 times, and then filtered and dried to obtain the reaction intermediate.

2. The highly dispersed carbon nanotube conductive paste according to claim 1, characterized in that: The reaction accelerator is selected from any one of sodium persulfate, ammonium persulfate and potassium persulfate.

3. The highly dispersed carbon nanotube conductive paste according to claim 1, characterized in that: The carbon nanotubes are selected from any one or more combinations of single-walled carbon nanotubes, double-walled carbon nanotubes, and multi-walled carbon nanotubes.

4. The highly dispersed carbon nanotube conductive paste according to claim 1, characterized in that: The synergistic dispersant is selected from any one or more combinations of polyethylene glycol octylphenyl ether, sodium carboxymethyl cellulose, sodium dodecyl sulfate, and polyvinyl pyrrolidone.

5. The highly dispersed carbon nanotube conductive paste according to claim 1, characterized in that: The solvent is selected from any one or more combinations of isopropanol, N-methylpyrrolidone, ethanol, and deionized water.

6. A method for preparing a highly dispersed carbon nanotube conductive paste according to any one of claims 1 to 5, characterized in that: The following steps are involved: S1. Accurately weigh various raw materials required for preparing highly dispersed carbon nanotube conductive slurry, and then transfer the high-efficiency dispersant, synergistic dispersant and solvent into a mixing device for mechanical mixing to mix the materials uniformly; after the materials are uniformly mixed, the obtained mixed liquid is stored and used for later use; S2, adding carbon nanotubes to the mixed liquid obtained in S1 while stirring, and mechanically stirring to obtain a mixed slurry; S3, transferring the mixed slurry obtained in step S2 into a grinding device, and subjecting it to sand grinding for 20 to 80 minutes using a grinding medium; after the grinding is completed, the result is a finished product of a highly dispersed carbon nanotube conductive slurry.

7. The method for preparing a highly dispersed carbon nanotube conductive paste according to claim 6, characterized in that: The grinding medium is selected from any one of aluminum dioxide beads, zirconium silicate beads and zirconium dioxide beads, and the particle size of the grinding medium is 0.8 to 2.5 mm.