A kind of polyarylpyridine and its preparation method and application
Polyarylpyridine with aggregation-induced luminescence properties was prepared by polymerization reaction between binary aryl et al. et al. et al. et al. et al. et al. et al. et al. et al. et al. et al. et al. et al. et al. et al. et al. et al. et al. et al. et al. et al. et al. et al. et al. et al. et al. et al. et al. et al. et al. et al. et al. et al. et al. et al. et al. et al. et al. et al. et al. et al. et al. et al. et al. et al. et al. et al. et al. et al. et al. et al. et al. et al. et al. et al. et al. et The function of detection of polynitroaromatic explosives avoids the negative impact of transition metal catalysts on material properties.
Patent Information
- Application Number
- CN202310534131.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-12
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-05-12
AI Technical Summary
The existing polymerization reactions are weakened or non-luminous in the solid state, which limits the application of polymer materials in the solid state, and the residue of transition metal catalysts in the multi-component polymerization reaction affects the mechanical and photoelectric properties of the material.
The solution polymerization reaction of binary aryl ethanone monomer and binary alkyne monomer under the catalyzed potassium tert-butoxide was prepared to prevent the use of transition metal catalysts and in polar aprotons It is carried out in a solvent to achieve the aggregation-induced luminescence (AIE) performance.
The prepared polyarylpyridine has good thermal stability, solubility and film formation, has AIE properties, and is suitable for the detection of polynitroaromatic explosives, avoiding the influence of catalyst residue on material properties.
Smart Images

Figure CN116769159B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of polymer synthesis and material technology, in particular to a polyarylpyridine and a preparation method and application thereof. Background Art
[0002] The development of new polymerization reactions and the preparation of polymer materials with new structures have important application value. Among the methods for synthesizing functional polymers developed in recent years, multi-component polymerization reactions have attracted widespread attention due to their advantages such as high synthesis efficiency, simple operation, product structure diversity, and high atom economy. In addition, the in-situ construction of new functional groups such as heterocycles in multi-component polymerization is difficult to achieve with other polymerization methods. At the same time, in multi-component polymerization reactions, multiple reaction steps can be completed in a one-pot method in a specific order, wherein the intermediate formed in the first step is directly added to the new component for subsequent reaction without separation and purification, and a product with high efficiency and good specificity can be obtained. For example, a multi-component polymerization reaction consisting of an improved Sonogashira coupling reaction of alkyne / carbonyl chloride and a continuous addition-cyclization reaction can easily obtain conjugated polythiophenes (Macromolecules 2014, 47, 4920-4929) and polypyrazoles (Macromolecules 2016, 49, 9291-9300) with clear structures, high molecular weights, and high yields. In addition, multi-component polymerization can also effectively control the order of functional groups on the polymer backbone. For example, a metal-free multi-component polymerization reaction of activated alkynes, aromatic diamines and formaldehyde can be used to obtain structurally adjustable and sequence-controllable polytetrahydropyrimidine (Polym.Chem.2015,6,4436-4446). Most of these multi-component polymerization reactions are based on terminal alkynes, and internal alkynes are rarely used to prepare heterocyclic polymers due to their large steric hindrance and relatively low reactivity. In the multi-component polymerization reactions that have been reported so far, transition metal catalysts are often used to reduce the activation energy of the reaction. However, the residual catalyst will affect the mechanical properties and photoelectric properties of polymer functional materials. In 2021, Trofimov's research group reported a multi-component one-pot reaction of methyl ketone, active alkyne and ammonium acetate to generate 2,4,6-triarylpyridine in situ by potassium tert-butoxide (Org.Biomol.Chem.2021,19,2703-2715.). This reaction is expected to develop into a polymerization reaction for preparing polyarylpyridine.
[0003] Traditional organic and polymer luminescent materials emit strong light in solution, but the light emission is weakened or non-emitting in the aggregated state or solid state, which limits the use of such materials in the solid state. In 2001, the Tang research group of the Hong Kong University of Science and Technology reported a novel photophysical phenomenon, namely aggregation-induced emission (AIE): organic small molecule thiole derivatives are almost not observed to emit light in solution, but once they form nanoparticles or films, the fluorescence intensity shows a significant increase (Chem. Commun. 2001, 1740-1741). Materials with AIE properties have been widely used in display, chemical detection and biosensing fields (Chem. Rev. 2015, 115, 11718-11940). Compared with small molecule materials, there are fewer reports on AIE-active polymer materials (Prog. Polym. Sci. 2020, 100, 101176). The preparation of new structure AIE polymers based on new polymerization reactions has important application value. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides a polyarylpyridine and a preparation method and application thereof. The present invention uses a binary aryl ethyl ketone monomer, a binary aryl alkynyl ketone monomer and ammonium acetate as raw materials, and reacts in the presence of potassium tert-butoxide and a polar aprotic solvent to obtain polyarylpyridine. The preparation method is simple, has a wide range of substrate applicability and good functional group compatibility, is easy to introduce a variety of functional groups, and realizes the preparation of different polymer functional materials.
[0005] The first object of the present invention is to provide a polyarylpyridine, wherein the polyarylpyridine has the following structural formula:
[0006]
[0007] Formula I, wherein n is 2 to 200;
[0008] R1 is one of groups 1 to 20, R2 is one of groups 1 to 20, and the structural formulas of the groups 1 to 20 are as follows:
[0009]
[0010] m is an integer of 1 to 18, and * is a substitution position.
[0011] The second object of the present invention is to provide a method for preparing polyarylpyridine, comprising the following steps:
[0012] Diaryl ketone monomer With diaryl alkynyl ketone monomer The polyaryl pyridine is obtained by solution polymerization in a reaction solvent using ammonium acetate or ammonium iodide as a raw material.
[0013] R1 is one of groups 1 to 20, R2 is one of groups 1 to 20, and the structural formulas of the groups 1 to 20 are as follows:
[0014]
[0015] m is an integer of 1 to 18, and * is a substitution position.
[0016] In one embodiment of the present invention, the polymerization reaction is carried out in an air atmosphere and mediated by a catalyst, potassium tert-butoxide.
[0017] In one embodiment of the present invention, the polymerization reaction conditions are: reaction temperature is 30-120° C., preferably 80-110° C.; reaction time is 3-15 hours, preferably 4-12 hours.
[0018] In one embodiment of the present invention, the reaction solvent is selected from one or more of N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide and toluene. The solvent can be a conventional high boiling point solvent.
[0019] In one embodiment of the present invention, the molar ratio of the divalent aromatic ethyl ketone monomer to the divalent aromatic alkynyl ketone monomer is 1:1.1 to 1:3.
[0020] In one embodiment of the present invention, the concentration of the diaryl ethyl ketone monomer is 0.02 to 1 mol / L, and preferably 0.05 to 0.33 mol / L.
[0021] In one embodiment of the present invention, the concentration of the divalent aryl alkynyl ketone monomer is 0.02 to 1 mol / L, and preferably 0.05 to 0.33 mol / L.
[0022] Furthermore, after the polymerization reaction is completed, post-treatment is further included. Preferably, the post-treatment is as follows: the polymerization reaction solution is diluted with a first organic solvent and then dripped into a second organic solvent to precipitate to obtain polyarylpyridine.
[0023] Furthermore, the first organic solvent is tetrahydrofuran or chloroform.
[0024] Furthermore, the second organic solvent is methanol, petroleum ether or n-hexane.
[0025] Furthermore, the preparation method of polyarylpyridine is specifically as follows:
[0026] The dibasic aryl ethyl ketone monomer, the dibasic aryl alkynyl ketone monomer, ammonium acetate and a reaction solvent are mixed to obtain a mixed solution, and then a solution polymerization reaction is performed to obtain polyaryl pyridine.
[0027] The third object of the present invention is to provide a fluorescence sensor, wherein the sensor comprises the polyarylpyridine or the polyarylpyridine prepared by the above preparation method.
[0028] The fourth object of the present invention is to provide the fluorescent sensor for detecting polynitroaromatic explosives.
[0029] The above technical solution of the present invention has the following advantages compared with the prior art:
[0030] 1. The present invention uses diaryl acetone, diaryl ketone and ammonium acetate as reaction raw materials, and reacts to synthesize polyaryl pyridine under the mediation of potassium tert-butoxide. The polyaryl pyridine prepared by the present invention has good thermal stability, good solubility in organic solvents such as chloroform, tetrahydrofuran, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, etc., and good processability and film-forming properties. In addition, the polyaryl pyridine containing AIE active units (such as tetraphenylethylene, etc.) prepared by the present invention has AIE performance and can be used as a fluorescent sensor for the detection of polynitroaromatic explosives.
[0031] 2. The present invention develops a polymerization reaction mediated by potassium tert-butoxide, which has mild reaction conditions, and the reaction raw materials are easily available and can be directly purchased or synthesized through simple reactions, and no transition metal catalyst is required, which can avoid the influence of the residual transition metal catalyst on the biological and optical properties of polymer materials; the polymerization reaction has a wide range of substrate applicability and good functional group compatibility, and can conveniently introduce a variety of functional groups. Therefore, the polymerization reaction has important application value in polymer synthesis and polymer functional materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] In order to make the content of the present invention more clearly understood, the present invention is further described in detail below according to specific embodiments of the present invention in conjunction with the accompanying drawings, wherein
[0033] Figure 1 is the structural formula diagram of the polyarylpyridine of the present invention (n=4);
[0034] Figure 2 This is a hydrogen nuclear magnetic resonance spectrum of the polyarylpyridine and its corresponding monomer prepared in Example 1 of the present invention in CDCl3 ("*" represents the solvent peak);
[0035] Figure 3 The thermogravimetric curves of the polyarylpyridines prepared in Examples 1, 13, 14, 15 and 16 of the present invention are shown in FIG. 1 , under a nitrogen atmosphere and at a heating rate of 10° C. / min.
[0036] Figure 4 is an AIE curve diagram of the polyarylpyridine prepared in Example 1 of the present invention;
[0037] Figure 5 This is a fluorescence spectrum diagram of picric acid (PA) detected in the aggregated state of the polyaryl pyridine prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0038] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention. In the present invention, unless otherwise specified, It only indicates the molecular connection relationship.
[0039] Example 1
[0040] This embodiment provides a method for preparing polyarylpyridine, which specifically comprises the following steps:
[0041]
[0042] (1) Preparation of diacetophenone
[0043] The first monomer, diacetophenone, is a commercial chemical and can be purchased directly.
[0044] (2) Preparation of dibasic acetylene ketone monomer
[0045] The second monomer, dibasic acetylene ketone monomer, was synthesized by referring to the preparation method of the published literature (Acta Chim. Sinica. 2016, 74, 885-892).
[0046]
[0047] Weigh the compound dialkynyl tetraphenylethylene (0.76g, 2.0mmol), benzoyl chloride (0.56g, 4.0mmol), bis(triphenylphosphine) palladium dichloride (56mg, 0.08mmol), and cuprous iodide (64mg, 0.32mmol) into a 100mL two-necked bottle, evacuate, and replace with nitrogen to remove oxygen and water vapor in the bottle. Then inject tetrahydrofuran (50mL) and triethylamine (0.6mL) into the bottle in sequence, stir and react at room temperature for 4h. After the reaction is completed, extract with dichloromethane and water, concentrate the obtained organic layer by rotary evaporation, purify by silica gel column chromatography, and use a mixed solvent of petroleum ether / ethyl acetate (20:1, v / v) as the eluent to obtain 0.96g of yellow-green solid with a yield of 82%. The NMR characterization data are as follows: 1 H NMR (400MHz, CDCl3), δ (TMS, ppm): 8.26–8.14 (m, 4H), 7.67–7.40 (m, 10H), 7.23–6.92 (m, 14H).
[0048] (3) Preparation of ammonium acetate
[0049] The third component, ammonium acetate, is a commercial chemical and can be purchased directly.
[0050] (4) Preparation of polyarylpyridine
[0051] Add the first monomer diacetophenone (16.2 mg, 0.10 mmol), the second monomer diacetyl ketone monomer (88.2 mg, 0.15 mmol), potassium tert-butoxide (22.4 mg, 0.2 mmol), and DMSO (1.0 mL) to a 10 mL polymerization tube with a side arm. After reacting in a 60°C constant temperature oil bath for 0.5 h, add the third component ammonium acetate (38.5 mg, 0.5 mmol), and continue to react in a 90°C constant temperature oil bath for 11.5 h. After the polymerization is completed, add 3 mL of tetrahydrofuran for dilution, and then add the dilution dropwise into the stirred anhydrous methanol (120 mL) through a glass tube plugged with cotton, let it stand and filter it with a funnel to obtain a polymer that is dried to constant weight.
[0052] Characterization data: yellow solid, yield 70.1%. GPC results show: weight average molecular weight (M w ) is 13400 and the molecular weight distribution (PDI) is 3.00. 1 H NMR (400MHz, CDCl3), δ (TMS, ppm): 7.86, 7.79, 7.25, 6.69, 2.50.
[0053] The comparison of the H NMR spectra of the polymer and its corresponding monomer is shown in the attached Figure 2 From the figure, it can be determined that the polymer is polyarylpyridine. The peak at δ2.58 (6) is the proton resonance peak of the first monomer diacetophenone methyl group. The intensity of the polymer's H NMR spectrum has been significantly reduced, indicating that the monomer has reacted. At the same time, a new resonance peak at δ7.85 appeared. By comparing it with the model product, it was attributed to the hydrogen on the newly generated pyridine ring. At the same time, it can be determined that the newly generated pyridine ring in the polymer is a single 2,4,6-configuration, indicating that the multi-component reaction has regional selectivity.
[0054] Performance research and application:
[0055] (1) Solubility
[0056] The polyarylpyridine prepared in this example is easily soluble in common organic solvents such as chloroform, tetrahydrofuran, N,N-dimethylformamide, N,N-dimethylacetamide and dimethyl sulfoxide at room temperature, and has good processability and film-forming properties.
[0057] (2) Thermal stability
[0058] Thermogravimetric analysis was performed on the polyarylpyridine prepared in this example. The test results are as follows: Figure 3 As shown, the polyarylpyridine polymer loses only 5% of its weight when heated to 460° C., which also shows that the polyarylpyridine prepared in this example has good thermal stability.
[0059] (3) AIE performance
[0060] The polyarylpyridine prepared in this example is dispersed in tetrahydrofuran solutions with different water contents, such as Figure 4 As shown, the polymer emits extremely weak light in tetrahydrofuran solution, but the fluorescence is significantly enhanced after adding poor solvent water, and the fluorescence is enhanced as the water content increases, showing excellent aggregation-induced emission properties.
[0061] (4) Application of polyarylpyridine in the detection of nitroaromatic explosives
[0062] Using picric acid (PA) as a model explosive, the process of testing PA is as follows: First, prepare 10 -5 mol / L tetrahydrofuran aqueous solution of polyarylpyridine (water volume fraction is 90%) is used as the test object, and different amounts of the test object PA are added in sequence to quickly test the fluorescence spectrum. Figure 4 As shown, when no PA is added, the detected object has strong fluorescence; when PA is added, the fluorescence weakens, and as the content of PA added gradually increases, the fluorescence intensity gradually weakens. This result shows that the polyarylpyridine prepared by the present invention can be used as a sensor for detecting nitroaromatic explosives.
[0063] Example 2
[0064] This embodiment provides a method for preparing polyarylpyridine, which specifically comprises the following steps:
[0065] The binary acetophenone monomer, the binary acetylenic ketone monomer and ammonium acetate are the same as in Example 1. Add the first monomer binary acetophenone (16.2 mg, 0.10 mmol), the second monomer binary acetylenic ketone monomer (88.2 mg, 0.15 mmol), potassium tert-butoxide (22.4 mg, 0.2 mmol) and DMSO (1.0 mL) to a 10 mL polymerization tube with a side arm. After reacting in a 60°C constant temperature oil bath for 0.5 h, add ammonium acetate (38.5 mg, 0.5 mmol) and continue to react in an 80°C constant temperature oil bath for 5.5 h. After the polymerization is completed, add 3 mL of tetrahydrofuran for dilution, and then add the dilution dropwise into the stirred anhydrous methanol (120 mL) through a glass tube plugged with cotton. After standing, filter with a funnel to obtain a polymer and dry it to constant weight. The yield is 64.7%. The gel permeation chromatography GPC results show that the weight average molecular weight (M w ) is 9300 and the molecular weight distribution (PDI) is 2.23.
[0066] The polymer prepared in this example also has good solubility and thermal stability; since it contains tetraphenylethylene groups with aggregation-induced light activity, the polymer also has aggregation-induced light performance and can be used for the detection of nitroaromatic explosives, as in Example 1.
[0067] Example 3
[0068] This embodiment provides a method for preparing polyarylpyridine, which specifically comprises the following steps:
[0069] The binary acetophenone monomer, the binary acetylenic ketone monomer and ammonium acetate are the same as in Example 1. Add the first monomer binary acetophenone (16.2 mg, 0.10 mmol), the second monomer binary acetylenic ketone monomer (88.2 mg, 0.15 mmol), potassium tert-butoxide (22.4 mg, 0.2 mmol) and DMSO (1.0 mL) to a 10 mL polymerization tube with a side arm. After reacting in a 60°C constant temperature oil bath for 0.5 h, add ammonium acetate (38.5 mg, 0.5 mmol) and continue to react in a 100°C constant temperature oil bath for 5.5 h. After the polymerization is completed, add 3 mL of tetrahydrofuran for dilution, and then add the dilution dropwise into the stirred anhydrous methanol (120 mL) through a glass tube plugged with cotton. After standing, filter with a funnel to obtain a polymer and dry it to constant weight. The yield is 84.0%. The gel permeation chromatography GPC results show that the weight average molecular weight (M w ) is 26800 and the molecular weight distribution (PDI) is 4.22.
[0070] The polymer prepared in this example also has good solubility and thermal stability; since it contains tetraphenylethylene groups with aggregation-induced light activity, the polymer also has aggregation-induced light performance and can be used for the detection of nitroaromatic explosives, as in Example 1.
[0071] Example 4
[0072] This embodiment provides a method for preparing polyarylpyridine, which specifically comprises the following steps:
[0073] The binary acetophenone monomer, the binary acetylenic ketone monomer and ammonium acetate are the same as in Example 1. Add the first monomer binary acetophenone (16.2 mg, 0.10 mmol), the second monomer binary acetylenic ketone monomer (88.2 mg, 0.15 mmol), potassium tert-butoxide (22.4 mg, 0.2 mmol) and DMSO (1.0 mL) to a 10 mL polymerization tube with a side arm. After reacting in a 60°C constant temperature oil bath for 0.5 h, add ammonium acetate (38.5 mg, 0.5 mmol) and continue to react in a 110°C constant temperature oil bath for 5.5 h. After the polymerization is completed, add 3 mL of tetrahydrofuran for dilution, and then add the dilution dropwise into the stirred anhydrous methanol (120 mL) through a glass tube plugged with cotton. After standing, filter with a funnel to obtain a polymer and dry it to constant weight. The yield is 67.6%. The gel permeation chromatography GPC results show that the weight average molecular weight (M w ) is 26800 and the molecular weight distribution (PDI) is 4.53.
[0074] The polymer prepared in this example also has good solubility and thermal stability; since it contains tetraphenylethylene groups with aggregation-induced light activity, the polymer also has aggregation-induced light performance and can be used for the detection of nitroaromatic explosives, as in Example 1.
[0075] Example 5
[0076] This embodiment provides a method for preparing polyarylpyridine, which specifically comprises the following steps:
[0077] Add the first monomer, diacetophenone (16.2 mg, 0.10 mmol), the second monomer, diacetyl ketone monomer (88.2 mg, 0.15 mmol), potassium tert-butoxide (22.4 mg, 0.2 mmol), and DMSO (2.0 mL) to a 10 mL polymerization tube with a side arm. After reacting in a 60°C constant temperature oil bath for 0.5 h, add ammonium acetate (38.5 mg, 0.5 mmol), and continue to react in a 90°C constant temperature oil bath for 5.5 h. After the polymerization is completed, add 3 mL of tetrahydrofuran for dilution, and then add the dilution dropwise into the stirred anhydrous methanol (120 mL) through a glass tube plugged with cotton. After standing, filter with a funnel to obtain a polymer and dry it to constant weight. The yield is 66.7%. The gel permeation chromatography GPC results show that the weight average molecular weight (M w ) is 7000 and the molecular weight distribution (PDI) is 2.21.
[0078] The polymer prepared in this example also has good solubility and thermal stability; since it contains tetraphenylethylene groups with aggregation-induced light activity, the polymer also has aggregation-induced light performance and can be used for the detection of nitroaromatic explosives, as in Example 1.
[0079] Example 6
[0080] This embodiment provides a method for preparing polyarylpyridine, which specifically comprises the following steps:
[0081] The binary acetophenone monomer, the binary acetylenic ketone monomer and the ammonium acetate monomer are the same as in Example 1. Add the first monomer binary acetophenone (16.2 mg, 0.10 mmol), the second monomer binary acetylenic ketone monomer (88.2 mg, 0.15 mmol), potassium tert-butoxide (22.4 mg, 0.2 mmol) and DMSO (1.5 mL) to a 10 mL polymerization tube with a side arm. After reacting in a 60°C constant temperature oil bath for 0.5 h, add ammonium acetate (38.5 mg, 0.5 mmol) and continue to react in a 90°C constant temperature oil bath for 5.5 h. After the polymerization is completed, add 3 mL of tetrahydrofuran for dilution, and then add the dilution dropwise into the stirred anhydrous methanol (120 mL) through a glass tube plugged with cotton. After standing, filter with a funnel to obtain a polymer and dry it to constant weight. The yield is 75.0%. The gel permeation chromatography GPC results show that the weight average molecular weight (M w ) is 8700 and the molecular weight distribution (PDI) is 2.30.
[0082] The polymer prepared in this example also has good solubility and thermal stability; since it contains tetraphenylethylene groups with aggregation-induced light activity, the polymer also has aggregation-induced light performance and can be used for the detection of nitroaromatic explosives, as in Example 1.
[0083] Example 7
[0084] This embodiment provides a method for preparing polyarylpyridine, which specifically comprises the following steps:
[0085] The binary acetophenone monomer, the binary acetylenic ketone monomer and the ammonium acetate monomer are the same as those in Example 1. Add the first monomer binary acetophenone (16.2 mg, 0.10 mmol), the second monomer binary acetylenic ketone monomer (88.2 mg, 0.15 mmol), potassium tert-butoxide (22.4 mg, 0.2 mmol) and DMSO (0.5 mL) to a 10 mL polymerization tube with a side arm. After reacting in a 60°C constant temperature oil bath for 0.5 h, add ammonium acetate (38.5 mg, 0.5 mmol) and continue to react in a 90°C constant temperature oil bath for 5.5 h. After the polymerization is completed, add 3 mL of tetrahydrofuran for dilution, and then add the dilution dropwise into the stirred anhydrous methanol (120 mL) through a glass tube plugged with cotton. After standing, filter with a funnel to obtain a polymer and dry it to constant weight. The yield is 70.0%. The gel permeation chromatography GPC results show that the weight average molecular weight (M w ) is 8200 and the molecular weight distribution (PDI) is 1.86.
[0086] The polymer prepared in this example also has good solubility and thermal stability; since it contains tetraphenylethylene groups with aggregation-induced light activity, the polymer also has aggregation-induced light properties and can be used for the detection of nitroaromatic explosives, as in Example 1.
[0087] Example 8
[0088] This embodiment provides a method for preparing polyarylpyridine, which specifically comprises the following steps:
[0089] The binary acetophenone monomer, the binary acetylenic ketone monomer and the ammonium acetate monomer are the same as those in Example 1. Add the first monomer binary acetophenone (16.2 mg, 0.10 mmol), the second monomer binary acetylenic ketone monomer (88.2 mg, 0.15 mmol), potassium tert-butoxide (22.4 mg, 0.2 mmol) and DMSO (0.3 mL) to a 10 mL polymerization tube with a side arm. After reacting in a 60°C constant temperature oil bath for 0.5 h, add ammonium acetate (38.5 mg, 0.5 mmol) and continue to react in a 90°C constant temperature oil bath for 5.5 h. After the polymerization is completed, add 3 mL of tetrahydrofuran for dilution, and then add the dilution dropwise into the stirred anhydrous methanol (120 mL) through a glass tube plugged with cotton. After standing, filter with a funnel to obtain a polymer and dry it to constant weight. The yield is 13.9%. The gel permeation chromatography GPC results show that the weight average molecular weight (M w ) is 3200 and the molecular weight distribution (PDI) is 1.24.
[0090] The polymer prepared in this example also has good solubility and thermal stability; since it contains tetraphenylethylene groups with aggregation-induced light activity, the polymer also has aggregation-induced light properties and can be used for the detection of nitroaromatic explosives, as in Example 1.
[0091] Example 9
[0092] This embodiment provides a method for preparing polyarylpyridine, which specifically comprises the following steps:
[0093] The binary acetophenone monomer, the binary acetylenic ketone monomer and the ammonium acetate monomer are the same as those in Example 1. Add the first monomer binary acetophenone (16.2 mg, 0.10 mmol), the second monomer binary acetylenic ketone monomer (88.2 mg, 0.15 mmol), potassium tert-butoxide (11.2 mg, 0.1 mmol) and DMSO (1.0 mL) to a 10 mL polymerization tube with a side arm. After reacting in a 60°C constant temperature oil bath for 0.5 h, add ammonium acetate (38.5 mg, 0.5 mmol) and continue to react in a 90°C constant temperature oil bath for 5.5 h. After the polymerization is completed, add 3 mL of tetrahydrofuran for dilution, and then add the dilution dropwise into the stirred anhydrous methanol (120 mL) through a glass tube plugged with cotton. After standing, filter with a funnel to obtain a polymer and dry it to constant weight. The yield is 47.2%. The gel permeation chromatography GPC results show that the weight average molecular weight (M w ) is 3100 and the molecular weight distribution (PDI) is 1.35.
[0094] The polymer prepared in this example also has good solubility and thermal stability; since it contains tetraphenylethylene groups with aggregation-induced light activity, the polymer also has aggregation-induced light properties and can be used for the detection of nitroaromatic explosives, as in Example 1.
[0095] Example 10
[0096] This embodiment provides a method for preparing polyarylpyridine, which specifically comprises the following steps:
[0097] The binary acetophenone monomer, the binary acetylenic ketone monomer and the ammonium acetate monomer are the same as those in Example 1. Add the first monomer binary acetophenone (16.2 mg, 0.10 mmol), the second monomer binary acetylenic ketone monomer (88.2 mg, 0.15 mmol), potassium tert-butoxide (16.8 mg, 0.15 mmol) and DMSO (1.0 mL) to a 10 mL polymerization tube with a side arm. After reacting in a 60°C constant temperature oil bath for 0.5 h, add ammonium acetate (38.5 mg, 0.5 mmol) and continue to react in a 90°C constant temperature oil bath for 5.5 h. After the polymerization is completed, add 3 mL of tetrahydrofuran for dilution, and then add the dilution dropwise into the stirred anhydrous methanol (120 mL) through a glass tube plugged with cotton. After standing, filter with a funnel to obtain a polymer and dry it to constant weight. The yield is 55.6%. The gel permeation chromatography GPC results show that the weight average molecular weight (M w ) is 4100 and the molecular weight distribution (PDI) is 1.60.
[0098] The polymer prepared in this example also has good solubility and thermal stability; since it contains tetraphenylethylene groups with aggregation-induced light activity, the polymer also has aggregation-induced light properties and can be used for the detection of nitroaromatic explosives, as in Example 1.
[0099] Embodiment 11
[0100] This embodiment provides a method for preparing polyarylpyridine, which specifically comprises the following steps:
[0101] The binary acetophenone monomer, the binary acetylenic ketone monomer and the ammonium acetate monomer are the same as in Example 1. Add the first monomer binary acetophenone (16.2 mg, 0.10 mmol), the second monomer binary acetylenic ketone monomer (88.2 mg, 0.15 mmol), potassium tert-butoxide (28.0 mg, 0.25 mmol) and DMSO (1.0 mL) to a 10 mL polymerization tube with a side arm. After reacting in a 60°C constant temperature oil bath for 0.5 h, add ammonium acetate (38.5 mg, 0.5 mmol) and continue to react in a 90°C constant temperature oil bath for 5.5 h. After the polymerization is completed, add 3 mL of tetrahydrofuran for dilution, and then add the dilution dropwise into the stirred anhydrous methanol (120 mL) through a glass tube plugged with cotton. After standing, filter with a funnel to obtain a polymer and dry it to constant weight. The yield is 75.0%. The gel permeation chromatography GPC results show that the weight average molecular weight (M w ) is 13600 and the molecular weight distribution (PDI) is 3.79.
[0102] The polymer prepared in this example also has good solubility and thermal stability; since it contains tetraphenylethylene groups with aggregation-induced light activity, the polymer also has aggregation-induced light properties and can be used for the detection of nitroaromatic explosives, as in Example 1.
[0103] Example 12
[0104] This embodiment provides a method for preparing polyarylpyridine, which specifically comprises the following steps:
[0105] The binary acetophenone monomer, the binary acetylenic ketone monomer and the ammonium acetate monomer are the same as those in Example 1. Add the first monomer binary acetophenone (16.2 mg, 0.10 mmol), the second monomer binary acetylenic ketone monomer (88.2 mg, 0.15 mmol), potassium tert-butoxide (33.6 mg, 0.30 mmol) and DMSO (1.0 mL) to a 10 mL polymerization tube with a side arm. After reacting in a 60°C constant temperature oil bath for 0.5 h, add ammonium acetate (38.5 mg, 0.5 mmol) and continue to react in a 90°C constant temperature oil bath for 5.5 h. After the polymerization is completed, add 3 mL of tetrahydrofuran for dilution, and then add the dilution dropwise into the stirred anhydrous methanol (120 mL) through a glass tube plugged with cotton. After standing, filter with a funnel to obtain a polymer and dry it to constant weight. The yield is 76.4%. The gel permeation chromatography GPC results show that the weight average molecular weight (M w ) is 9100 and the molecular weight distribution (PDI) is 2.42.
[0106] The polymer prepared in this example also has good solubility and thermal stability; since it contains tetraphenylethylene groups with aggregation-induced light activity, the polymer also has aggregation-induced light properties and can be used for the detection of nitroaromatic explosives, as in Example 1.
[0107] Example 12-1
[0108] This embodiment provides a method for preparing polyarylpyridine, which specifically comprises the following steps:
[0109] The binary acetophenone monomer and the binary acetylenic ketone monomer are the same as those in Example 1. Add the first monomer binary acetophenone (16.2 mg, 0.10 mmol), the second monomer binary acetylenic ketone monomer (88.2 mg, 0.15 mmol), potassium tert-butoxide (33.6 mg, 0.30 mmol) and DMSO (1.0 mL) to a 10 mL polymerization tube with a side arm. After reacting in a 60°C constant temperature oil bath for 0.5 h, add ammonium iodide (72.5 mg, 0.5 mmol) and continue to react in a 90°C constant temperature oil bath for 11.5 h. After the polymerization is completed, add 3 mL of tetrahydrofuran for dilution, and then add the dilution dropwise to the stirred anhydrous methanol (120 mL) through a glass tube plugged with cotton. After standing, filter with a funnel to obtain a polymer and dry it to constant weight. The yield is 68.4%. The gel permeation chromatography GPC results show that the weight average molecular weight (M w ) is 6400 and the molecular weight distribution (PDI) is 6.19.
[0110] The polymer prepared in this example also has good solubility and thermal stability; since it contains tetraphenylethylene groups with aggregation-induced light activity, the polymer also has aggregation-induced light properties and can be used for the detection of nitroaromatic explosives, as in Example 1.
[0111] Example 13
[0112] This embodiment provides a method for preparing polyarylpyridine, which specifically comprises the following steps:
[0113]
[0114] (1) Synthesis of diaryl ethyl ketone monomers:
[0115] The synthesis of the first monomer, a diaryl ethyl ketone monomer, was synthesized according to the preparation method of the published literature (Polym. Adv. Technol. 2021, 33 (1), 427-439).
[0116] In a 250mL three-necked round-bottom flask, 6.6g (0.04mol) of 4-hydroxyacetophenone, 13.5g (0.09mol) of potassium carbonate, 6g (0.02mol) of 1,6-dibromohexane and 25mL of N,N-dimethylformamide (DMF) were added. The contents were stirred at 110°C under a nitrogen atmosphere at room temperature for 24 hours. After the reaction was complete, the product was extracted with ethyl acetate and washed twice in a sodium hydroxide solution. The organic layer was dried under anhydrous sodium sulfate, and the organic layer was evaporated under vacuum to obtain 1,1-((hexane-1,6-diylbis(oxy))bis(4,1-phenylene))diethyl ketone as a yellow solid (yield 80%). 1 H NMR (400MHz, CDCl3), δ (TMS, ppm): 7.92 (d, J = 8.4Hz, 4H), 6.92 (d, J = 8.4Hz, 4H), 4.04 (t, J = 6.4Hz, 4H), 2.55 (s, 6H), 1.84 (q, J = 6.5Hz, 4H), 1.54 (s, 4H).
[0117] (2) The second monomer is a diacetylenic ketone monomer, which is the same as in Example 1.
[0118] (3) The third component, ammonium acetate, is the same as in Example 1.
[0119] (4) Preparation of polyarylpyridine:
[0120] Add the first monomer, diacetophenone (35.4 mg, 0.10 mmol), the second monomer, diacetyl ketone monomer (88.2 mg, 0.15 mmol), potassium tert-butoxide (22.4 mg, 0.2 mmol), and DMSO (1.0 mL) to a 10 mL polymerization tube with a side arm. After reacting in a 60°C constant temperature oil bath for 0.5 h, add ammonium acetate (38.5 mg, 0.5 mmol), and continue to react in a 90°C constant temperature oil bath for 11.5 h. After the polymerization is completed, add 3 mL of tetrahydrofuran for dilution, and then add the dilution dropwise into the stirred anhydrous methanol (120 mL) through a glass tube plugged with cotton. After standing, filter with a funnel to obtain a polymer that is dried to constant weight. Characterization data: yellow solid, yield 55.4%. GPC results show: weight average molecular weight (M w ) is 18800 and the molecular weight distribution (PDI) is 3.07. 1 H NMR (400MHz, CDCl3), δ (TMS, ppm): 8.02, 7.92, 7.58, 7.51, 7.42, 7.29, 7.10, 6.91, 6.76, 6.71, 4.08, 2.5, 1.86, 1.75.
[0121] The polymer prepared in this example also has good solubility and thermal stability; since it contains tetraphenylethylene groups with aggregation-induced light activity, the polymer also has aggregation-induced light properties and can be used for the detection of nitroaromatic explosives, as in Example 1.
[0122] Embodiment 14
[0123] This embodiment provides a method for preparing polyarylpyridine, which specifically comprises the following steps:
[0124]
[0125] (1) Synthesis of diaryl ethyl ketone monomers:
[0126] Weigh 1,4-dibromo-tetraphenylene (2.46 g, 5 mmol), potassium carbonate (2.07 g, 15 mmol), tetrakistriphenylphosphine palladium (0.13 g, 0.15 mmol), 4-acetylphenylboronic acid (3.28 g, 20 mmol) in a 250 mL dry two-necked bottle, vacuumize and fill with nitrogen three times, add freshly distilled THF (102 mL), water (10.2 mL), react in a 70 ° C constant temperature oil bath for 6 hours, TLC plate confirms that the raw materials have reacted completely, end the reaction and cool to room temperature, extract with dichloromethane, dry the combined organic phase with anhydrous magnesium sulfate, and concentrate the filtered filtrate by vacuum distillation, purify by silica gel column chromatography, and use a mixed solvent of petroleum ether and ethyl acetate (15:1) as the eluent. After drying, a gray solid is obtained, which is the first monomer binary acetophenone monomer. The yield is 50.4% (1.43 g). 1 H NMR (400MHz, CDCl3), δ (TMS, ppm): 7.99 (d, J = 8.0Hz, 4H), 7.65 (d, J = 8.0Hz, 4H), 7.42 (d, J = 7.9Hz, 4H), 7.23–6.96 (m, 12H), 2.62 (s, 4H).
[0127] (2) The second monomer is a diacetylenic ketone monomer, which is the same as in Example 1.
[0128] (3) The third component, ammonium acetate, is the same as in Example 1.
[0129] (4) Preparation of polyarylpyridine:
[0130] Add the first monomer, diacetophenone (56.9 mg, 0.10 mmol), the second monomer, diacetophenone monomer (88.2 mg, 0.15 mmol), potassium tert-butoxide (22.4 mg, 0.2 mmol), and DMSO (1.0 mL) to a 10 mL polymerization tube with a side arm. After reacting in a 60°C constant temperature oil bath for 0.5 h, add ammonium acetate (38.5 mg, 0.5 mmol), and continue to react in a 90°C constant temperature oil bath for 11.5 h. After the polymerization is completed, add 3 mL of tetrahydrofuran for dilution, and then add the dilution dropwise into the stirred anhydrous methanol (120 mL) through a glass tube plugged with cotton. After standing, filter with a funnel to obtain a polymer that is dried to constant weight. Characterization data: yellow solid, yield 84.1%. GPC results show: weight average molecular weight (M w ) is 11600 and the molecular weight distribution (PDI) is 3.30. 1 HNMR (400MHz, CDCl3), δ (TMS, ppm): δ8.03,7.90,7.74,7.58,7.53,7.47,7.19,7.22,7.13,7.07,6.84,6.76,2.52.
[0131] The polymer prepared in this example also has good solubility and thermal stability; since it contains tetraphenylethylene groups with aggregation-induced light activity, the polymer also has aggregation-induced light properties and can be used for the detection of nitroaromatic explosives, as in Example 1.
[0132] Embodiment 15
[0133] This embodiment provides a method for preparing polyarylpyridine, which specifically comprises the following steps:
[0134]
[0135] The specific steps include:
[0136] (1) The first monomer is a binary acetophenone monomer, which is the same as in Example 13.
[0137] (2) Synthesis of dibasic acetylenic ketone monomers
[0138] The second monomer, dibasic acetylene ketone monomer, was synthesized by referring to the preparation method of the published literature (Macromol. Rapid Commun. 2012, 33(16), 1356-1361).
[0139] PdCl2(PPh3) (281 mg, 0.4×10 -3 mol), CuI (152 mg, 0.8 x 10 -3mol), PPh3 (105 mg, 0.40 × 10 -3 mol), THF (60 mL) and triethylamine (20 mL). Then, 1,4-diynylbenzene (10 x 10 -3 The mixture was cooled to 0°C in an ice-water bath, and then benzoyl chloride (2.783 mL, 24×10 -3 mol,). After stirring at room temperature for 12 hours, the mixture was poured into ice water. The aqueous solution was extracted three times with 50 mL of dichloromethane. The organic phases were combined and then dried over anhydrous magnesium sulfate overnight. After filtration and solvent evaporation, the crude product was purified by silica gel column using a petroleum ether / chloroform mixture (1:1, v:v) as eluent. A gray powder (3.145 g) was obtained with a yield of 94.2%. 1 H NMR (400MHz, CDCl3), δ (TMS, ppm): 8.25–8.17 (m, 4H), 7.73 (s, 4H), 7.69–7.61 (m, 2H), 7.57–7.49 (m, 4H).
[0140] (3) The third component, ammonium acetate, is the same as in Example 1.
[0141] (4) Preparation of polyarylpyridine:
[0142] Add the first monomer, diacetophenone (35.4 mg, 0.10 mmol), the second monomer, diacetyl ketone monomer (50.1 mg, 0.15 mmol), potassium tert-butoxide (22.4 mg, 0.2 mmol), and DMSO (1.0 mL) to a 10 mL polymerization tube with a side arm. After reacting in a 60°C constant temperature oil bath for 0.5 h, add ammonium acetate (38.5 mg, 0.5 mmol), and continue to react in a 90°C constant temperature oil bath for 11.5 h. After the polymerization is completed, add 3 mL of tetrahydrofuran for dilution, and then add the dilution dropwise to the stirred anhydrous methanol (120 mL) through a glass tube plugged with cotton. After standing, filter with a funnel to obtain a polymer that is dried to constant weight. Characterization data: brown solid, yield 61.4%. GPC results show: weight average molecular weight (M w ) is 6700 and the molecular weight distribution (PDI) is 2.13. 1 H NMR (400MHz, CDCl3), δ (TMS, ppm): 8.23, 7.86, 7.81, 7.68, 7.64, 7.50, 7.45, 7.35, 7.26, 7.01, 6.96, 6.89, 6.64, 4.00, 3.93, 2.571.85, 1.27.
[0143] Example 16
[0144] This embodiment provides a method for preparing polyarylpyridine, which specifically comprises the following steps:
[0145]
[0146] The specific steps include:
[0147] (1) The first monomer is a binary acetophenone monomer, which is the same as in Example 14.
[0148] (2) The synthesis of the second monomer, dibasic acetylene ketone monomer, is the same as in Example 14.
[0149] (3) The third component, ammonium acetate, is the same as in Example 1.
[0150] (4) Preparation of polyarylpyridine:
[0151] Add the first monomer, diacetophenone (56.9 mg, 0.10 mmol), the second monomer, diacetyl ketone monomer (50.1 mg, 0.15 mmol), potassium tert-butoxide (22.4 mg, 0.2 mmol), and DMSO (1.0 mL) to a 10 mL polymerization tube with a side arm. After reacting in a 60°C constant temperature oil bath for 0.5 h, add ammonium acetate (38.5 mg, 0.5 mmol), and continue to react in a 90°C constant temperature oil bath for 11.5 h. After the polymerization is completed, add 3 mL of tetrahydrofuran for dilution, and then add the dilution dropwise into the stirred anhydrous methanol (120 mL) through a glass tube plugged with cotton. After standing, filter with a funnel to obtain a polymer that is dried to constant weight. Characterization data: brown solid, yield 57.8%. GPC results show: weight average molecular weight (M w ) is 7400 and the molecular weight distribution (PDI) is 2.70. 1 H NMR (400MHz, CDCl3), δ (TMS, ppm): 8.26, 8.03, 7.76, 7.66, 7.53, 7.49, 7.24, 7.15, 2.53.
[0152] Obviously, the above embodiments are merely examples for clear explanation and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the protection scope of the invention.
Claims
1. A polyarylpyridine, characterized in that The polyarylpyridine structural formula is as follows: , Formula I, wherein n is 2 to 200; R1 and R2 are selected from the following structures shown in Formula 1, Formula 10 or Formula 15: , m is an integer of 1 to 18, and * is a substitution position.
2. A method for preparing polyarylpyridine according to claim 1, characterized in that: The following steps are involved: Diaryl ketone monomer With diaryl alkynyl ketone monomer , ammonium acetate as raw materials, and the polyaryl pyridine is obtained by solution polymerization in a reaction solvent.
3. A method for preparing polyarylpyridine according to claim 1, characterized in that: The following steps are involved: Diaryl ketone monomer With diaryl alkynyl ketone monomer , ammonium iodide as raw materials, and the polyaryl pyridine is obtained by solution polymerization in a reaction solvent.
4. The preparation method according to claim 2 or 3, characterized in that: The polymerization reaction is carried out in an air atmosphere and mediated by potassium tert-butoxide as a catalyst.
5. The preparation method according to claim 2 or 3, characterized in that: The polymerization reaction conditions are as follows: the reaction temperature is 30 to 120° C., and the reaction time is 3 to 15 hours.
6. The preparation method according to claim 2 or 3, characterized in that: The reaction solvent is selected from one or more of N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide and toluene.
7. The preparation method according to claim 2 or 3, characterized in that: The molar ratio of the divalent aryl ethyl ketone monomer to the divalent aryl alkynyl ketone monomer is 1:1 to 1.
3.
8. The preparation method according to claim 2 or 3, characterized in that: The concentration of the diaryl ethyl ketone monomer is 0.02-1 mol / L.
9. The preparation method according to claim 2 or 3, characterized in that: The concentration of the divalent aromatic alkynyl ketone monomer is 0.02-1 mol / L.
10. A fluorescence sensor, characterized in that: The sensor comprises the polyarylpyridine described in claim 1 or the polyarylpyridine prepared by the preparation method described in any one of claims 2-9.
11. Use of the fluorescent sensor according to claim 10 in the detection of polynitroaromatic explosives.