High temperature resistant composite polymer tackifier and preparation method thereof
By combining terpolymers and sodium carboxymethylcellulose in aqueous solution, optimizing the molar ratio of polymerized monomers and potassium persulfate, the problem of insufficient high-temperature resistance in high-temperature oil fields is solved, and the problem of insufficient high-temperature resistance in high-temperature oil fields is achieved. The high viscosity and high temperature resistance of composite polymer solutions are improved.
Patent Information
- Application Number
- CN202310729196.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-19
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-06-19
AI Technical Summary
Sodium carboxymethylcellulose is used as a thickener in high-temperature oil fields with limited application, and its high-temperature resistance is poor, and the existing composite polymers are limited in improvement.
A terpolymer and sodium carboxymethylcellulose were combined in aqueous solution. By optimizing the molar ratio of polymer monomers and the use of potassium persulfate, a composite polymer solution with synergistic tackification and good high temperature resistance was prepared.
The composite polymer solution has been maintained at a high viscosity within the range of 20 to 80°C, which significantly improves high temperature resistance and is suitable for high-temperature oil fields.
Smart Images

Figure QLYQS_1 
Figure BDA0004293799000000011 
Figure BDA0004293799000000021
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of petrochemical industry, and in particular relates to a high temperature resistant composite polymer tackifier and a preparation method thereof. Background Art
[0002] As a thickener, sodium carboxymethyl cellulose has the advantages of strong thickening ability and small dosage, and can be used as an oil field displacement agent in oil extraction. However, sodium carboxymethyl cellulose solution has poor high temperature resistance, and its viscosity is easily affected by the reservoir temperature, which limits its application in high-temperature oil fields. To this end, researchers compounded polymers such as hydroxyethyl cellulose with sodium carboxymethyl cellulose in a certain proportion to prepare a composite solution, but the improvement in high temperature resistance was limited. Summary of the invention
[0003] One of the purposes of the present invention is to provide a composite polymer solution having a synergistic viscosity-increasing effect and good high temperature resistance.
[0004] To achieve the object, the present invention adopts the following technical scheme to achieve the object of the present invention: the composite polymer thickener solution is prepared by mixing the terpolymer and sodium carboxymethyl cellulose in an aqueous solution.
[0005] The general structural formula of the terpolymer is shown in Formula I.
[0006]
[0007] Among them, z:x:y is 2~5:0.5~3:1, and n=9.
[0008] The reaction formula for preparing the compound of formula I is shown below.
[0009]
[0010] The preparation method of the compound of formula I is carried out according to the following steps: using acrylamide, N-isopropyl methacrylamide and methoxy polyethylene glycol acrylate as polymerization monomers, potassium persulfate as initiator, heating to 80°C in an aqueous solution under nitrogen protection for reaction for 24 hours. After the reaction is completed, the reaction solution is cooled to room temperature, dialyzed in ultrapure water for 3 days, and freeze-dried to obtain a terpolymer solid.
[0011] Wherein, the molar ratio of acrylamide, N-isopropyl methacrylamide and methoxy polyethylene glycol acrylate is 2 to 4:1 to 4:2, preferably 4:4:2;
[0012] The mass of potassium persulfate is 0.6-1% of the total mass of polymerization monomers;
[0013] The molecular weight of methoxy polyethylene glycol acrylate is about 480 Da.
[0014] The mass ratio of the terpolymer to sodium carboxymethyl cellulose is 1-4:0.3.
[0015] The advantages of the present invention are:
[0016] In the composite polymer solution provided by the present invention, the terpolymer and sodium carboxymethyl cellulose have a synergistic viscosity-increasing effect, and good high-temperature resistance can be achieved by optimizing the molar ratio of each polymerized monomer in the terpolymer. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 H NMR spectra of the copolymers prepared in Examples 1, 2, 4, 5, 7 and Comparative Example 1. DETAILED DESCRIPTION
[0018] The method of the present invention is further described below in conjunction with specific embodiments.
[0019] Example 1 Preparation of poly(N-isopropylmethacrylamide-methoxypolyethylene glycol acrylate) (3.0:1)
[0020] 2.54 g of N-isopropyl methacrylamide and 2.4 g of methoxy polyethylene glycol acrylate (molecular weight 480) were dissolved in 80 mL of ultrapure water, 30 mg of potassium persulfate was added, nitrogen was introduced by bubbling method to expel air for 30 min, the reaction solution was heated to 80° C. under nitrogen atmosphere, stirred for reaction for 24 hours, and then the reaction solution was cooled to room temperature, dialyzed in ultrapure water (molecular weight cutoff 3500 Da) for 3 days, and freeze-dried to obtain a white solid.
[0021] The prepared binary copolymers were characterized by hydrogen nuclear magnetic resonance spectroscopy. Figure 1 . The molar ratio of the polymerized units N-isopropylmethacrylamide and methoxypolyethylene glycol acrylate in the copolymer was calculated to be 3.0:1 by the integral ratio of the methyl hydrogen signal of N-isopropylmethacrylamide (chemical shift 1.1) and the polyethylene glycol signal of methoxypolyethylene glycol acrylate (chemical shift 3.5-4.5). The number average molecular weight of the copolymer was 11751 and the multi-fraction index was 1.12 by gel permeation chromatography, indicating that the molecular weight of the copolymer was relatively uniform.
[0022] Example 2 Preparation of poly(N-isopropylmethacrylamide-methoxypolyethylene glycol acrylate) (2.1:1)
[0023] 2.54 g of N-isopropyl methacrylamide and 4.8 g of methoxy polyethylene glycol acrylate (molecular weight 480) were dissolved in 80 mL of ultrapure water, 60 mg of potassium persulfate was added, nitrogen was introduced by bubbling method to expel air for 30 min, the reaction solution was heated to 80° C. under nitrogen atmosphere, stirred for reaction for 24 hours, and then the reaction solution was cooled to room temperature, dialyzed in ultrapure water (molecular weight cutoff 3500 Da) for 3 days, and freeze-dried to obtain a white solid.
[0024] The prepared binary copolymers were characterized by hydrogen nuclear magnetic resonance spectroscopy. Figure 1 . The molar ratio of the polymerized units N-isopropyl methacrylamide and methoxy polyethylene glycol acrylate in the copolymer was calculated to be 2.1:1 by integrating the methyl hydrogen signal of N-isopropyl methacrylamide (chemical shift 1.1) and the polyethylene glycol signal of methoxy polyethylene glycol acrylate (chemical shift 3.5-4.5). The number average molecular weight of the copolymer was 10549 and the multi-fraction index was 1.13 by gel permeation chromatography, indicating that the molecular weight of the copolymer was relatively uniform.
[0025] Example 3 Preparation of Poly(N-isopropylmethacrylamide-methoxypolyethylene glycol acrylate)
[0026] 2.54 g of N-isopropyl methacrylamide and 7.2 g of methoxy polyethylene glycol acrylate (molecular weight 480) were dissolved in 80 mL of ultrapure water, 60 mg of potassium persulfate was added, nitrogen was introduced by bubbling method to exhaust air for 30 min, and the reaction solution was heated to 80° C. and stirred for reaction for 24 hours under nitrogen atmosphere, and the reaction solution was cross-linked and gelled.
[0027] Example 4 Preparation of poly(acrylamide-N-isopropylmethacrylamide-methoxypolyethylene glycol acrylate) (3.3:0.7:1)
[0028] 0.71 g of acrylamide, 1.27 g of N-isopropyl methacrylamide and 4.8 g of methoxy polyethylene glycol acrylate were dissolved in 80 mL of ultrapure water, 60 mg of potassium persulfate was added, nitrogen was introduced by bubbling method to exhaust the air for 30 min, the reaction solution was heated to 80° C. under nitrogen atmosphere, stirred for reaction for 24 hours, then the reaction solution was cooled to room temperature, dialyzed in ultrapure water (molecular weight cutoff 3500 Da) for 3 days, and freeze-dried to obtain a white solid.
[0029] The prepared binary copolymers were characterized by hydrogen nuclear magnetic resonance spectroscopy. Figure 1. The molar ratio of acrylamide, N-isopropylmethacrylamide and methoxypolyethylene glycol acrylate in the copolymer was calculated to be 3.3:0.7:1 by the integral ratio of the methyl hydrogen signal of N-isopropylmethacrylamide (chemical shift 1.0), the polyethylene glycol signal of methoxypolyethylene glycol acrylate (chemical shift 3.4-4.4) and the hydrogen signal of the polymer backbone (chemical shift 1.5 and 2.1). The number average molecular weight of the copolymer was 15116 and the multi-fraction index was 1.01 by gel permeation chromatography, indicating that the molecular weight of the copolymer was relatively uniform.
[0030] Example 5 Preparation of poly(acrylamide-N-isopropylmethacrylamide-methoxypolyethylene glycol acrylate) (2.9:0.6:1)
[0031] 1.07 g of acrylamide, 0.64 g of N-isopropyl methacrylamide and 4.8 g of methoxy polyethylene glycol acrylate were dissolved in 80 mL of ultrapure water, 60 mg of potassium persulfate was added, nitrogen was introduced by bubbling method to exhaust the air for 30 min, the reaction solution was heated to 80° C. under nitrogen atmosphere, stirred for reaction for 24 hours, and then the reaction solution was cooled to room temperature, dialyzed in ultrapure water (molecular weight cutoff 3500 Da) for 3 days, and freeze-dried to obtain a white solid.
[0032] The prepared binary copolymers were characterized by hydrogen nuclear magnetic resonance spectroscopy. Figure 1 . The molar ratio of acrylamide, N-isopropylmethacrylamide and methoxypolyethylene glycol acrylate in the copolymer was calculated to be 2.9:0.6:1 by the integral ratio of the methyl hydrogen signal of N-isopropylmethacrylamide (chemical shift 1.0) and the polyethylene glycol signal of methoxypolyethylene glycol acrylate (chemical shift 3.4-4.4) and the hydrogen signal of the polymer backbone (chemical shift 1.6 and 2.1). The number average molecular weight of the copolymer was 14825 and the multi-fraction index was 1.01 by gel permeation chromatography, indicating that the molecular weight of the copolymer was relatively uniform.
[0033] Example 6 Preparation of Poly(Acrylamide-N-Isopropyl Methacrylamide-Methoxy Polyethylene Glycol Acrylate)
[0034] 1.24 g acrylamide, 0.32 g N-isopropyl methacrylamide and 4.8 g methoxy polyethylene glycol acrylate were dissolved in 80 mL ultrapure water, 60 mg potassium persulfate was added, nitrogen was introduced by bubbling method to exhaust air for 30 min, and the reaction solution was heated to 80° C. under nitrogen atmosphere and stirred for reaction for 24 hours, and the reaction solution was cross-linked and gelled.
[0035] Example 7 Preparation of poly(acrylamide-N-isopropylmethacrylamide-methoxypolyethylene glycol acrylate) (4.7:2.3:1)
[0036] 0.71 g of acrylamide, 1.27 g of N-isopropyl methacrylamide and 2.4 g of methoxy polyethylene glycol acrylate were dissolved in 80 mL of ultrapure water, 30 mg of potassium persulfate was added, nitrogen was introduced by bubbling method to expel air for 30 min, the reaction solution was heated to 80° C. under nitrogen atmosphere, stirred for reaction for 24 hours, and then the reaction solution was cooled to room temperature, dialyzed in ultrapure water (molecular weight cutoff 3500 Da) for 3 days, and freeze-dried to obtain a white solid.
[0037] The prepared binary copolymers were characterized by hydrogen nuclear magnetic resonance spectroscopy. Figure 1 . The molar ratio of acrylamide, N-isopropylmethacrylamide and methoxypolyethylene glycol acrylate in the copolymer was calculated to be 4.7:2.3:1 by the integral ratio of the methyl hydrogen signal of N-isopropylmethacrylamide (chemical shift 1.0), the polyethylene glycol signal of methoxypolyethylene glycol acrylate (chemical shift 3.4-4.4) and the hydrogen signal of the polymer backbone (chemical shift 1.6 and 2.1). The number average molecular weight of the copolymer was 13782 and the multi-fraction index was 1.10 by gel permeation chromatography, indicating that the molecular weight of the copolymer was relatively uniform.
[0038] Example 8 Preparation of Poly(Acrylamide-N-Isopropyl Methacrylamide-Methoxy Polyethylene Glycol Acrylate)
[0039] 1.42 g of acrylamide, 1.27 g of N-isopropyl methacrylamide and 2.4 g of methoxy polyethylene glycol acrylate were dissolved in 80 mL of ultrapure water, 30 mg of potassium persulfate was added, nitrogen was introduced by bubbling method to exhaust air for 30 min, and the reaction solution was heated to 80° C. under nitrogen atmosphere and stirred for reaction for 24 hours, and the reaction solution was cross-linked and gelled.
[0040] Example 9 Preparation of poly(acrylamide-methoxypolyethylene glycol acrylate)
[0041] 1.42 g of acrylamide and 2.4 g of methoxy polyethylene glycol acrylate were dissolved in 80 mL of ultrapure water, 30 mg of potassium persulfate was added, nitrogen was introduced by bubbling method to expel air for 30 min, the reaction solution was heated to 80° C. under nitrogen atmosphere and stirred for reaction for 24 hours, and the reaction solution was cross-linked and gelled.
[0042] Example 10 Preparation of poly(acrylamide-methoxypolyethylene glycol acrylate)
[0043] 0.71 g acrylamide and 2.4 g methoxy polyethylene glycol acrylate were dissolved in 80 mL ultrapure water, 30 mg potassium persulfate was added, nitrogen was introduced by bubbling method to expel air for 30 min, the reaction solution was heated to 80° C. under nitrogen atmosphere and stirred for reaction for 24 hours, and the reaction solution was cross-linked and gelled.
[0044] Comparative Example 1 Poly(N-isopropylmethacrylamide-sodium acrylate)
[0045] 2.54 g of N-isopropylmethacrylamide and 0.94 g of sodium acrylate were dissolved in 80 mL of ultrapure water, 30 mg of potassium persulfate was added, nitrogen was introduced by bubbling method to expel air for 30 min, the reaction solution was heated to 80° C. under nitrogen atmosphere, stirred for reaction for 24 hours, then the reaction solution was cooled to room temperature, dialyzed in ultrapure water (molecular weight cutoff 3500 Da) for 3 days, and freeze-dried to obtain a white solid.
[0046] The prepared binary copolymers were characterized by hydrogen nuclear magnetic resonance spectroscopy. Figure 1 . The molar ratio of the polymer units N-isopropylmethacrylamide and sodium acrylate units in the copolymer was calculated to be 2.4:1 by the integral ratio of the hydrogen signal of the polymer main chain (chemical shift 1.7) and the methyl hydrogen signal of N-isopropylmethacrylamide (chemical shift 1.0). The number average molecular weight of the copolymer was 14392 and the multi-fraction index was 1.03 by gel permeation chromatography, indicating that the molecular weight of the copolymer was relatively uniform.
[0047] Comparative Example 2 Preparation of Poly(Acrylamide-N-isopropylmethacrylamide-Sodium Acrylate) (4.5:2.4:1)
[0048] 0.71 g of acrylamide, 1.27 g of N-isopropylmethacrylamide and 0.47 g of sodium acrylate were dissolved in 80 mL of ultrapure water, 30 mg of potassium persulfate was added, nitrogen was introduced by bubbling method to expel air for 30 min, the reaction solution was heated to 80° C. under nitrogen atmosphere, stirred for reaction for 24 hours, then the reaction solution was cooled to room temperature, dialyzed in ultrapure water (molecular weight cutoff 3500 Da) for 3 days, and freeze-dried to obtain a white solid.
[0049] Comparative Example 3 Preparation of Poly(Acrylamide-N-isopropylmethacrylamide-Hydroxybutyl Acrylate) (4.8:2.5:1)
[0050] 0.71 g of acrylamide, 1.27 g of N-isopropylmethacrylamide and 0.72 g of hydroxybutyl acrylate were dissolved in 80 mL of ultrapure water, 30 mg of potassium persulfate was added, nitrogen was introduced by bubbling method to expel air for 30 min, the reaction solution was heated to 80° C. under nitrogen atmosphere, stirred for reaction for 24 hours, and then the reaction solution was cooled to room temperature, dialyzed in ultrapure water (molecular weight cutoff 3500 Da) for 3 days, and freeze-dried to obtain a white solid.
[0051] Example 11 Preparation of 2% copolymer solution
[0052] The copolymers prepared in Examples 1, 2, 4, 5, 7 and Comparative Examples 1, 2 and 3 were dissolved in ultrapure water to prepare aqueous solutions with a mass concentration of 2% for each copolymer.
[0053] Example 12 Preparation of 0.3% sodium carboxymethylcellulose solution
[0054] Sodium carboxymethyl cellulose was dissolved in ultrapure water to prepare a 0.3% sodium carboxymethyl cellulose aqueous solution.
[0055] Example 13 Preparation of composite polymer solutions containing 0.3% sodium carboxymethyl cellulose and copolymers of different concentrations
[0056] The copolymers prepared in Examples 1, 2, 4, 5, 7 and Comparative Examples 1, 2 and 3 were dissolved in ultrapure water, and sodium carboxymethyl cellulose was added to dissolve the copolymers to prepare aqueous solutions containing 0.3% sodium carboxymethyl cellulose and 1% of the copolymer, aqueous solutions containing 0.3% sodium carboxymethyl cellulose and 2% of the copolymer, and aqueous solutions containing 0.3% sodium carboxymethyl cellulose and 3% of the copolymer.
[0057] Example 14 Determination of viscosity-temperature characteristics
[0058] The solutions prepared in Examples 11 to 13 were taken and the viscosity of the solutions was measured with a digital rotational viscometer at a shear rate of 100 s -1 .
[0059] Table 1. Viscosity of 2% copolymer solution at different temperatures
[0060]
[0061] As shown in Table 1, the poly(N-isopropylmethacrylamide-methoxypolyethylene glycol acrylate) prepared in Examples 1 and 2, the poly(acrylamide-N-isopropylmethacrylamide-methoxypolyethylene glycol acrylate) prepared in Examples 4, 5, and 7, the poly(N-isopropylmethacrylamide-sodium acrylate) prepared in Comparative Example 1, the poly(acrylamide-N-isopropylmethacrylamide-sodium acrylate) prepared in Comparative Example 2, and the poly(acrylamide-N-isopropylmethacrylamide-hydroxybutyl acrylate) prepared in Comparative Example 3 (all with a mass concentration of 2%) have low viscosities, and the viscosity decreases with increasing temperature. As shown in Table 2, the aqueous solution of sodium carboxymethylcellulose (mass concentration of 0.3%) has a high viscosity, but the solution viscosity decreases significantly with increasing temperature.
[0062] Table 2. Viscosity of composite polymer solution (0.3% sodium carboxymethylcellulose concentration, 1% polymer concentration) at different temperatures
[0063]
[0064] The viscosity of the composite solution containing 1% copolymer and 0.3% sodium carboxymethyl cellulose is shown in Table 2. When the composite solution is prepared by using the poly (N-isopropyl methacrylamide-methoxy polyethylene glycol acrylate) (3.0:1) prepared in Example 1 and sodium carboxymethyl cellulose, the viscosity of the composite solution is only slightly higher than that of the sodium carboxymethyl cellulose solution, and the high temperature resistance cannot be effectively improved; when the composite solution is prepared by using the poly (N-isopropyl methacrylamide-methoxy polyethylene glycol acrylate) (2.1:1) prepared in Example 2 and sodium carboxymethyl cellulose, the viscosity of the composite solution is significantly higher than that of the sodium carboxymethyl cellulose solution, and when the temperature is raised to 70°C, the viscosity of the composite solution does not decrease but increases, indicating that the N-isopropyl methacrylamide in the poly (N-isopropyl methacrylamide-methoxy polyethylene glycol acrylate) prepared in Example 2 is The amine unit can undergo a phase change at high temperature, from hydrophilic to hydrophobic, and bridge and crosslink the polymer molecules through hydrophobic association, thereby increasing the viscosity of the composite solution. When the temperature is further increased to 80°C, the viscosity of the composite solution decreases due to the increase in the molecular thermal motion speed. In general, the composite solution maintains a relatively high viscosity in the range of 20 to 80°C and has good high temperature resistance. Therefore, when the molar ratio of N-isopropyl methacrylamide unit to methoxy polyethylene glycol acrylate unit in poly(N-isopropyl methacrylamide-methoxy polyethylene glycol acrylate) is 2.1, the prepared composite solution has good high temperature resistance; when the poly(N-isopropyl methacrylamide-sodium acrylate) (2.4:1) and sodium carboxymethyl cellulose to prepare a composite solution, the viscosity of the composite solution is significantly lower than that of the sodium carboxymethyl cellulose solution, which is mainly due to the sodium acrylate unit playing a charge shielding role here, so that the electrostatic repulsion between the carboxyl anions in the sodium carboxymethyl cellulose is weakened, the polymer coil is curled, the volume is reduced, and the viscosity is reduced; when the poly (acrylamide-N-isopropylmethacrylamide-methoxypolyethylene glycol acrylate) prepared in Examples 4, 5, and 7 is used to prepare a composite solution with sodium carboxymethyl cellulose, the viscosity of the composite solution is significantly increased, which is mainly due to the strong hydrogen bonding between acrylamide and sodium carboxymethyl cellulose. As the temperature increases, the viscosity of Examples 4, 5, and 7 increases. The viscosity of the composite solution prepared by Example 7 and sodium carboxymethyl cellulose decreased significantly, mainly because the high temperature destroyed the hydrogen bond interaction. When the temperature of the composite solution prepared by Example 7 and sodium carboxymethyl cellulose was raised to 70°C, the viscosity did not decrease but increased, indicating that at this time, the N-isopropylmethacrylamide unit in Example 7 underwent a phase change at high temperature, from hydrophilic to hydrophobic, and the polymer molecules were bridged and cross-linked by hydrophobic association, which improved the viscosity of the composite solution and outweighed the viscosity reduction effect caused by the destruction of hydrogen bonds. In general, the composite solution maintained a relatively high viscosity in the range of 20 to 80°C, especially when the temperature was greater than or equal to 60°C, the viscosity of the composite solution was significantly higher than that of other groups, and it had the best high temperature resistance in the test groups. In addition, when the molar ratio of acrylamide unit, N-isopropyl methacrylamide unit and methoxy polyethylene glycol acrylate unit in poly(acrylamide-N-isopropyl methacrylamide-methoxy polyethylene glycol acrylate) is 4.7:2.3:1, the prepared composite solution has high high temperature resistance, and the unit molar ratio of N-isopropyl methacrylamide unit and methoxy polyethylene glycol acrylate is very close to the molar ratio of N-isopropyl methacrylamide unit and methoxy polyethylene glycol acrylate unit in poly(acrylamide-N-isopropyl methacrylamide-methoxy polyethylene glycol acrylate) prepared in Example 2, which further indicates that the control of N-isopropyl methacrylamide unit and methoxy polyethylene glycol acrylate in the copolymer is better than that of methoxy polyethylene glycol acrylate. When the molar ratio of ethylene glycol acrylate units is about 2:1, the high temperature resistance of the composite solution can be effectively improved; when the poly(acrylamide-N-isopropylmethacrylamide-sodium acrylate) (4.5:2.4:1) prepared in Comparative Example 2 is used to prepare a composite solution with sodium carboxymethyl cellulose, at low temperatures, the viscosity of the composite solution is slightly higher than that of the sodium carboxymethyl cellulose solution, and when the temperature is higher than 40°C, the viscosity of the composite solution is lower than that of the sodium carboxymethyl cellulose solution. This is because the charge shielding effect of the sodium acrylate unit overcomes the hydrogen bond interaction between the acrylamide unit and the sodium carboxymethyl cellulose at high temperatures; when the poly(acrylamide-N-isopropylmethacrylamide-hydroxybutyl acrylate) (4.8:2.4:1) prepared in Comparative Example 3 is used to prepare a composite solution, the viscosity of the composite solution is slightly higher than that of the sodium carboxymethyl cellulose solution, and when the temperature is higher than 40°C, the viscosity of the composite solution is lower than that of the sodium carboxymethyl cellulose solution.After preparing a composite solution with sodium carboxymethyl cellulose, the viscosity of the composite solution increased significantly, but its viscosity-increasing effect was not as good as the composite solution formed by poly(acrylamide-N-isopropylmethacrylamide-methoxypolyethylene glycol acrylate) and sodium carboxymethyl cellulose prepared in Examples 4, 5, and 7, and its high temperature resistance was not as good as the composite solution formed by sodium carboxymethyl cellulose in Example 7, indicating that the viscosity-increasing and high temperature resistance of the hydroxybutyl acrylate unit in the terpolymer were not as good as the methoxypolyethylene glycol acrylate unit.
[0065] Table 3. Viscosity of composite polymer solution (0.3% sodium carboxymethylcellulose concentration, 2% polymer concentration) at different temperatures.
[0066]
[0067] As shown in Table 3, when the concentration of the copolymer is increased to 2%, the viscosity of the composite solutions formed by Examples 1, 2, 4, 5, 7, and Comparative Example 3 with sodium carboxymethyl cellulose is increased, while the viscosity of the composite solution formed by Comparative Example 1 with sodium carboxymethyl cellulose is reduced, and the viscosity of the composite solution formed by Comparative Example 2 with sodium carboxymethyl cellulose is also reduced at high temperatures, which is mainly due to the charge shielding effect of the sodium acrylate unit.
[0068] Table 4. Viscosity of composite polymer solution (0.3% sodium carboxymethylcellulose concentration, 3% polymer concentration) at different temperatures
[0069]
[0070] As shown in Table 4, when the concentration of the copolymer is increased from 2% to 3%, the viscosity of the composite solution formed by Examples 1, 2, 4, 5, 7, and Comparative Example 3 and sodium carboxymethyl cellulose is only slightly improved, while the viscosity of the composite solution formed by Comparative Example 1 and sodium carboxymethyl cellulose continues to decrease, and the viscosity of the composite solution formed by Comparative Example 2 and sodium carboxymethyl cellulose also continues to decrease at high temperatures, which is also due to the charge shielding effect of the sodium acrylate unit in the copolymer. Although continuing to increase the concentration of the copolymer in Examples 1, 2, 4, 5, 7, and Comparative Example 3 can continuously increase the viscosity of the composite solution, it is more appropriate to control the mass ratio of the copolymer to sodium carboxymethyl cellulose within the range of 1 to 4:0.3 from the perspectives of cost, viscosity-increasing effect, and high temperature resistance.
Claims
1. A high temperature resistant composite polymer tackifier as an oil field oil displacement agent, characterized in that: The high temperature resistant composite polymer thickener is prepared by mixing and compounding a terpolymer and sodium carboxymethyl cellulose in an aqueous solution; The general structural formula of the terpolymer is shown in Formula I , Among them, z:x:y is 2~5:0.5~3:1, n=9; The mass ratio of the terpolymer to sodium carboxymethyl cellulose is 1-4:0.3; The preparation method of the terpolymer is as follows: using acrylamide, N-isopropyl methacrylamide and methoxy polyethylene glycol acrylate as polymerization monomers, using potassium persulfate as an initiator, heating and reacting in an aqueous solution under nitrogen protection, cooling the reaction solution to room temperature after the reaction is completed, purifying by dialysis, and freeze-drying to obtain a terpolymer solid.
2. The high temperature resistant composite polymer tackifier as an oil field oil displacement agent according to claim 1, characterized in that: The molar ratio of acrylamide, N-isopropyl methacrylamide and methoxy polyethylene glycol acrylate is 2-4:1-4:
2.
3. The high temperature resistant composite polymer tackifier as an oil field oil displacement agent according to claim 1, characterized in that: The feeding amount of potassium persulfate is 0.6-1% of the total feeding mass of polymerization monomers.
4. The high temperature resistant composite polymer tackifier as an oil field oil displacement agent according to claim 1, characterized in that: The molecular weight of methoxy polyethylene glycol acrylate is 480 Da.
5. The high temperature resistant composite polymer tackifier as an oil field oil displacement agent according to claim 1, characterized in that: The heating reaction temperature was 80°C and the reaction time was 24 hours.