Sodium bismuth titanate-based high entropy dielectric energy storage ceramic material and its preparation method and application
Through the preparation of sodium bismuth titanate-based high-entropy dielectric energy storage ceramic materials, the problem that existing materials are difficult to achieve both large ΔP and high breakdown field strength is solved, and high-efficiency energy storage density and stable performance are achieved, which is suitable for high-end capacitors.
Patent Information
- Application Number
- CN202310768347.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-28
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-06-28
AI Technical Summary
Existing sodium bismuth titanate ceramic materials are difficult to achieve both large ΔP and high breakdown field strength (Eb), and cannot meet the needs of high-end dielectric capacitors.
The composition formula of sodium bismuth titanate-based high-entropy medium energy storage ceramic material is (Bi0.5Na0.5)0.8Sr0.07Ba0.07Ca0.06Ti0.75(Nb0.05Mg0.05T a0.05Zr0.05Sn0.05)O3, ceramic materials with excellent energy storage properties are prepared through specific preparation processes including baking, batching, pre-burning, ball milling, tableting, debinding, sintering and surface metallization.
It has achieved a maximum breakdown field strength of 359~370kV/cm, an energy storage density of 4.16~4.33J/cm3, and an energy storage efficiency of 89.7~90.1%. It also has excellent temperature stability, frequency stability and fatigue characteristics, and is suitable for pulse capacitors. and other high-power devices.
Smart Images

Figure CN116854469B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of ceramic materials, and in particular relates to a sodium bismuth titanate-based high-entropy dielectric energy storage ceramic material and a preparation method and application thereof. Background Art
[0002] With the development of materials science and technology as well as 5G and 6G mobile communications, electronic components are becoming increasingly miniaturized, lightweight, and intelligent, and there is an urgent need for high-end dielectric capacitors with high energy storage density and low loss. As an important system of dielectric capacitor materials, sodium bismuth titanate ceramics are considered to be one of the most commercially promising lead-free and environmentally friendly materials due to their wide band gap (large breakdown electric field), no volatile K element (easy to prepare), and low volume density (lightweight). However, based on traditional doping and defect engineering strategies, it is rare to simultaneously achieve large ΔP (Pmax-Pr) and high breakdown field strength (Eb) in sodium bismuth titanate ceramic materials, making it difficult to meet practical applications. Summary of the invention
[0003] The technical problem to be solved by the present invention is to provide a sodium bismuth titanate-based high entropy dielectric energy storage ceramic material and a preparation method and application thereof in view of the deficiencies of the above-mentioned prior art. The sodium bismuth titanate-based high entropy dielectric energy storage ceramic material has excellent energy storage performance, a simple preparation process, good repeatability, low cost, and is suitable for industrialization.
[0004] In order to solve the above technical problems, the technical solution adopted by the present invention is: a sodium bismuth titanate-based high entropy dielectric energy storage ceramic material, the composition formula of the sodium bismuth titanate-based high entropy dielectric energy storage ceramic material is:
[0005] (Bi 0.5 Na 0.5 ) 0.8 Sr 0.07 Ba 0.07 Ca 0.06 Ti 0.75 (Nb 0.05 Mg 0.05 Ta 0.05 Zr 0.05 Sn 0.05 )O3.
[0006] This embodiment also provides a method for preparing the above-mentioned sodium bismuth titanate-based high entropy dielectric energy storage ceramic material, which is:
[0007] S1. Drying materials: drying the Na2CO3 raw material, Bi2O3 raw material, CaCO3 raw material, BaCO3 raw material and SrCO3 raw material at a temperature of 300°C for 6 hours respectively;
[0008] The Nb2O5 raw material, the TiO2 raw material, the Ta2O5 raw material, the ZrO2 raw material, the MgO raw material and the SnO2 raw material were dried at a temperature of 900°C for 4h respectively;
[0009] The purity of the Na2CO3 raw material is 99.8%, the purity of the Bi2O3 raw material is 99%, the purity of the CaCO3 raw material is 99%, the purity of the BaCO3 raw material is 99%, the purity of the SrCO3 raw material is 99%, the purity of the Nb2O5 raw material is 99.5%, the purity of the TiO2 raw material is 98%, the purity of the Ta2O5 raw material is 99.99%, the purity of the ZrO2 raw material is 99%, the purity of the MgO raw material is 98.5%, and the purity of the SnO2 raw material is 99.5%;
[0010] S2, ingredients: the dried Na2CO3 raw material, Bi2O3 raw material, CaCO3 raw material, BaCO3 raw material, SrCO3 raw material, Nb2O5 raw material, TiO2 raw material, Ta2O5 raw material, ZrO2 raw material, MgO raw material and SnO2 raw material in S1 are mixed according to (Bi 0.5 Na 0.5 ) 0.8 Sr 0.07 Ba 0.07 Ca 0.06 Ti 0.75 (Nb 0.05 Mg 0.05 Ta 0.05 Zr 0.05 Sn 0.05 )O3 in a stoichiometric ratio are weighed and mixed uniformly to obtain a premix, agate balls and anhydrous ethanol are added, and the mixture is ball-milled in a planetary ball mill at a speed of 300 r / min to 400 r / min for 6 h to 10 h. After separating the agate balls, the mixture is dried at a temperature of 70° C. to 120° C. for 10 h to 24 h, and after grinding, it is sieved through a 120-mesh sieve to obtain a raw material mixture;
[0011] S3, pre-calcining: heating the raw material mixture obtained in S2 from room temperature to 850°C to 950°C at a heating rate of 3°C / min to 5°C / min, then pre-calcining at a constant temperature for 2h to 4h, naturally cooling to room temperature, and grinding to obtain pre-calcined powder;
[0012] S4, secondary ball milling: add agate balls and anhydrous ethanol to the pre-calcined powder obtained in S3, ball mill for 6h to 10h, separate the agate balls, dry at a temperature of 70°C to 120°C for 10h to 24h, grind and pass through a 180-mesh sieve to obtain ball-milled pre-calcined powder;
[0013] S5, tableting: adding a 6% polyvinyl alcohol aqueous solution to the pre-burned powder after ball milling obtained in S4, granulating and passing through a 40-mesh sieve to obtain a spherical powder material in the shape of quicksand, and maintaining the pressure for 10s to 60s under a uniaxial pressure condition of 100MPa to 200MPa to obtain a disc-shaped ceramic body;
[0014] S6, debinding: heating the disc-shaped ceramic body obtained in S5 to 500°C to 600°C at a heating rate of 1°C / min to 3°C / min and keeping the temperature for 1h to 3h, and then naturally cooling to room temperature to obtain a disc-shaped ceramic body from which the binder has been completely removed;
[0015] S7, sintering: sintering the disc-shaped ceramic body obtained in S5 after the binder is removed to obtain a sintered ceramic body; the sintering conditions are: firstly heating from room temperature to 1160°C to 1220°C at a heating rate of 3°C / min to 5°C / min, sintering at a constant temperature for 2h to 3h, and then cooling to room temperature at a cooling rate of 5°C / min;
[0016] S8, polishing: grinding the upper and lower surfaces of the sintered ceramic body obtained in S7 with 600-mesh sandpaper, and then polishing with 2000-mesh sandpaper and corundum to a thickness of 0.3 mm to 0.5 mm, placing in deionized water, ultrasonically cleaning and drying to obtain a polished ceramic body;
[0017] S9, surface metallization: The upper and lower surfaces of the polished ceramic body obtained in S8 are uniformly coated with silver paste with a thickness of 0.01 mm to 0.03 mm, and then placed in a resistance furnace, and the temperature is raised to 850°C at a heating rate of 3°C / min to 6°C / min, kept at this temperature for 10 minutes, and naturally cooled to room temperature to obtain sodium bismuth titanate-based high entropy dielectric energy storage ceramic material.
[0018] Preferably, the dosage ratio of the premix, agate balls and anhydrous ethanol in S2 is 0.30 g: 1 g: 0.45 mL.
[0019] Preferably, the usage ratio of the pre-burnt powder, agate balls and anhydrous ethanol in S4 is 0.28g:1g:0.40mL.
[0020] Preferably, the mass ratio of the 6% polyvinyl alcohol aqueous solution and the pre-calcined powder after ball milling in S5 is (5% to 10%):1.
[0021] Preferably, the ultrasonic cleaning time in S8 is 10 min to 20 min.
[0022] Preferably, the sodium bismuth titanate-based high entropy dielectric energy storage ceramic material (Bi 0.5 Na 0.5 ) 0.8 Sr 0.07Ba 0.07 Ca 0.06 Ti 0.75 (Nb 0.05 Mg 0.05 Ta 0.05 Zr 0.05 Sn 0.05 )O3, its breakdown field strength is 359~370kV / cm, and its energy storage density is W rec 4.16~4.33J / cm 3 , the energy storage efficiency η is 89.7~90.1%, and it has excellent temperature stability (W rec The change value is less than 7% in the temperature range of 25-200℃), frequency stability performance (W rec Variation value <3% in the range of 1-200Hz) and excellent fatigue properties (W rec In 10 6 The variation value within the cycle range is <3%).
[0023] The present invention also provides an application of the sodium bismuth titanate-based high entropy dielectric energy storage ceramic material prepared by the above method, wherein the sodium bismuth titanate-based high entropy dielectric energy storage ceramic material is used for the preparation of a pulse capacitor.
[0024] Compared with the prior art, the present invention has the following advantages:
[0025] The high entropy ceramics prepared by the present invention can obtain the maximum energy storage density (breakdown field strength E b Reach 359~370kV / cm, energy storage density W rec Can reach 4.16~4.33J / cm 3 , energy storage efficiency η is 89.7~90.1%), excellent temperature stability (W rec The change value is less than 7% in the temperature range of 25-200℃), frequency stability performance (W rec Variation value <3% in the range of 1-200Hz) and excellent fatigue properties (W rec In 10 6 The change value within the cycle range is <3%), which is highly practical and easy to mass-produce. It is a lead-free high-entropy dielectric energy storage ceramic with excellent performance and can be used in high-power devices such as pulse capacitors.
[0026] The present invention is further described in detail below with reference to the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 1 is the XRD diagram of the ceramic body after polishing in S8 of Examples 1-4 of the present invention.
[0028] Figure 2It is a SEM scanning image of the ceramic body in S7 of Examples 1-4 of the present invention.
[0029] Figure 3 This is a PE characteristic diagram of the sodium bismuth titanate-based high entropy dielectric energy storage ceramic material of Example 2 of the present invention.
[0030] Figure 4 This is a picture of the temperature stability of the energy storage performance of the sodium bismuth titanate-based high entropy dielectric energy storage ceramic material of Example 2 of the present invention.
[0031] Figure 5 This is a frequency stability picture of the energy storage performance of the sodium bismuth titanate-based high entropy dielectric energy storage ceramic material of Example 2 of the present invention.
[0032] Figure 6 This is a test diagram of the energy storage performance fatigue performance of the sodium bismuth titanate-based high entropy dielectric energy storage ceramic material of Example 2 of the present invention. DETAILED DESCRIPTION
[0033] Example 1
[0034] The sodium bismuth titanate-based high entropy dielectric energy storage ceramic material of this embodiment has a composition formula of:
[0035] (Bi 0.5 Na 0.5 ) 0.8 Sr 0.07 Ba 0.07 Ca 0.06 Ti 0.75 (Nb 0.05 Mg 0.05 Ta 0.05 Zr 0.05 Sn 0.05 )O3.
[0036] This embodiment also provides a method for preparing the above-mentioned sodium bismuth titanate-based high entropy dielectric energy storage ceramic material, which is:
[0037] S1. Drying materials: drying the Na2CO3 raw material, Bi2O3 raw material, CaCO3 raw material, BaCO3 raw material and SrCO3 raw material at a temperature of 300°C for 6 hours respectively;
[0038] The Nb2O5 raw material, the TiO2 raw material, the Ta2O5 raw material, the ZrO2 raw material, the MgO raw material and the SnO2 raw material were dried at a temperature of 900°C for 4h respectively;
[0039] The purity of the Na2CO3 raw material is 99.8%, the purity of the Bi2O3 raw material is 99%, the purity of the CaCO3 raw material is 99%, the purity of the BaCO3 raw material is 99%, the purity of the SrCO3 raw material is 99%, the purity of the Nb2O5 raw material is 99.5%, the purity of the TiO2 raw material is 98%, the purity of the Ta2O5 raw material is 99.99%, the purity of the ZrO2 raw material is 99%, the purity of the MgO raw material is 98.5%, and the purity of the SnO2 raw material is 99.5%; all the above raw materials were purchased from Sinopharm Chemical Reagent Co., Ltd.;
[0040] S2, ingredients: the dried Na2CO3 raw material, Bi2O3 raw material, CaCO3 raw material, BaCO3 raw material, SrCO3 raw material, Nb2O5 raw material, TiO2 raw material, Ta2O5 raw material, ZrO2 raw material, MgO raw material and SnO2 raw material in S1 are mixed according to (Bi 0.5 Na 0.5 ) 0.8 Sr 0.07 Ba 0.07 Ca 0.06 Ti 0.75 (Nb 0.05 Mg 0.05 Ta 0.05 Zr 0.05 Sn 0.05 )O3 in a stoichiometric ratio are weighed and mixed uniformly to obtain a premix, agate balls and anhydrous ethanol are added, and the mixture is ball-milled in a planetary ball mill at a speed of 400r / min for 6h. After the agate balls are separated, the mixture is dried at a temperature of 70°C for 24h, and after grinding, it is sieved through a 120-mesh sieve to obtain a raw material mixture; the dosage ratio of the premix, agate balls and anhydrous ethanol is 0.30g:1g:0.45mL;
[0041] S3, pre-calcining: heating the raw material mixture obtained in S2 from room temperature to 950°C at a heating rate of 5°C / min, then pre-calcining at a constant temperature for 2h, naturally cooling to room temperature, and grinding to obtain pre-calcined powder;
[0042] S4, secondary ball milling: add agate balls and anhydrous ethanol to the pre-calcined powder obtained in S3, ball mill for 6 hours, separate the agate balls, dry at 70°C for 24 hours, grind and pass through a 180-mesh sieve to obtain the pre-calcined powder after ball milling; the amount ratio of the pre-calcined powder, agate balls and anhydrous ethanol is 0.28g:1g:0.40mL;
[0043] S5, tableting: adding a 6% polyvinyl alcohol aqueous solution to the pre-burned powder after ball milling obtained in S4, granulating and passing through a 40-mesh sieve to obtain a spherical powder material in the form of quicksand, maintaining the pressure for 60 seconds under a uniaxial pressure of 100 MPa to obtain a disc-shaped ceramic body; the mass ratio of the 6% polyvinyl alcohol aqueous solution to the pre-burned powder after ball milling is 10%:1;
[0044] S6, debinding: heating the disc-shaped ceramic body obtained in S5 to 600°C at a heating rate of 3°C / min and keeping the temperature for 1 hour to decompose and discharge the PVA, and then naturally cooling to room temperature to obtain a disc-shaped ceramic body from which the binder has been completely removed;
[0045] S7, sintering: sintering the disc-shaped ceramic body obtained in S5 after the binder is removed to obtain a sintered ceramic body; the sintering conditions are: firstly heating from room temperature to 1160°C at a heating rate of 3°C / min, sintering at a constant temperature for 3h, and then cooling to room temperature at a cooling rate of 5°C / min;
[0046] S8, polishing: grinding the upper and lower surfaces of the sintered ceramic body obtained in S7 with 600-mesh sandpaper, and then polishing with 2000-mesh sandpaper and corundum to a thickness of 0.3 mm, placing in deionized water, ultrasonically cleaning for 10 minutes, and drying to obtain a polished ceramic body;
[0047] The polished ceramic body was tested by XRD using a German Bruker D8 Advanced diffractometer, and the ceramic sample surface was tested by SEM scanning using a Japanese Hitachi S-4800 scanning electron microscope. Figures 1-2 , the prepared (Bi 0.5 Na 0.5 ) 0.8 Sr 0.07 Ba 0.07 Ca 0.06 Ti 0.75 (Nb 0.05 Mg 0.05 Ta 0.05 Zr 0.05 Sn 0.05 )O3 high entropy dielectric energy storage ceramic material is a pure perovskite structure with an average grain size of ~2.6μm and dense particle distribution;
[0048] S9, surface metallization: The upper and lower surfaces of the polished ceramic body obtained in S8 are uniformly coated with silver paste with a thickness of 0.01 mm, and then placed in a resistance furnace, and the temperature is raised to 850°C at a heating rate of 3°C / min, kept at this temperature for 10 minutes, and naturally cooled to room temperature to obtain sodium bismuth titanate-based high entropy dielectric energy storage ceramic material.
[0049] The bismuth titanate sodium-based high entropy dielectric energy storage ceramic material (Bi 0.5 Na 0.5 ) 0.8 Sr 0.07 Ba 0.07 Ca 0.06 Ti 0.75 (Nb 0.05 Mg 0.05 Ta 0.05 Zr 0.05 Sn 0.05 )O3 breakdown field strength, PE characteristics and energy storage performance were tested, and the results are shown in Table 1. rec The change value is less than 6.5% in the temperature range of 25-200℃, W rec Variation value <2.7% in the range of 1-200Hz, W rec In 10 6 The change in the cycle range was <2.9%.
[0050] Table 1 Performance test of Example 1
[0051]
[0052] Example 2
[0053] The sodium bismuth titanate-based high entropy dielectric energy storage ceramic material of this embodiment has a composition formula of:
[0054] (Bi 0.5 Na 0.5 ) 0.8 Sr 0.07 Ba 0.07 Ca 0.06 Ti 0.75 (Nb 0.05 Mg 0.05 Ta 0.05 Zr 0.05 Sn 0.05 )O3.
[0055] This embodiment also provides a method for preparing the above-mentioned sodium bismuth titanate-based high entropy dielectric energy storage ceramic material, which is:
[0056] S1. Drying materials: drying the Na2CO3 raw material, Bi2O3 raw material, CaCO3 raw material, BaCO3 raw material and SrCO3 raw material at a temperature of 300°C for 6 hours respectively;
[0057] The Nb2O5 raw material, the TiO2 raw material, the Ta2O5 raw material, the ZrO2 raw material, the MgO raw material and the SnO2 raw material were dried at a temperature of 900°C for 4h respectively;
[0058] The purity of the Na2CO3 raw material is 99.8%, the purity of the Bi2O3 raw material is 99%, the purity of the CaCO3 raw material is 99%, the purity of the BaCO3 raw material is 99%, the purity of the SrCO3 raw material is 99%, the purity of the Nb2O5 raw material is 99.5%, the purity of the TiO2 raw material is 98%, the purity of the Ta2O5 raw material is 99.99%, the purity of the ZrO2 raw material is 99%, the purity of the MgO raw material is 98.5%, and the purity of the SnO2 raw material is 99.5%; all the above raw materials were purchased from Sinopharm Chemical Reagent Co., Ltd.;
[0059] S2, ingredients: the dried Na2CO3 raw material, Bi2O3 raw material, CaCO3 raw material, BaCO3 raw material, SrCO3 raw material, Nb2O5 raw material, TiO2 raw material, Ta2O5 raw material, ZrO2 raw material, MgO raw material and SnO2 raw material in S1 are mixed according to (Bi 0.5 Na 0.5 ) 0.8 Sr 0.07 Ba 0.07 Ca 0.06 Ti 0.75 (Nb 0.05 Mg 0.05 Ta 0.05 Zr 0.05 Sn 0.05 )O3 in a stoichiometric ratio are weighed and mixed uniformly to obtain a premix, agate balls and anhydrous ethanol are added, and the mixture is ball-milled at a speed of 350r / min for 8h in a planetary ball mill. After the agate balls are separated, the mixture is dried at a temperature of 100°C for 18h, and after grinding, it is sieved through a 120-mesh sieve to obtain a raw material mixture; the dosage ratio of the premix, agate balls and anhydrous ethanol is 0.30g:1g:0.45mL;
[0060] S3, pre-calcining: heating the raw material mixture obtained in S2 from room temperature to 850°C at a heating rate of 5°C / min, then pre-calcining at a constant temperature for 2h, naturally cooling to room temperature, and grinding to obtain pre-calcined powder;
[0061] S4, secondary ball milling: add agate balls and anhydrous ethanol to the pre-calcined powder obtained in S3, ball mill for 8 hours, separate the agate balls, dry at 100°C for 18 hours, grind and pass through a 180-mesh sieve to obtain the pre-calcined powder after ball milling; the amount ratio of the pre-calcined powder, agate balls and anhydrous ethanol is 0.28g:1g:0.40mL;
[0062] S5, tableting: adding a 6% polyvinyl alcohol aqueous solution to the pre-burned powder after ball milling obtained in S4, granulating and passing through a 40-mesh sieve to obtain a spherical powder material in the shape of quicksand, maintaining the pressure for 60 seconds under a uniaxial pressure of 200 MPa to obtain a disc-shaped ceramic body; the mass ratio of the 6% polyvinyl alcohol aqueous solution to the pre-burned powder after ball milling is 8%:1;
[0063] S6, debinding: heating the disc-shaped ceramic body obtained in S5 to 550° C. at a heating rate of 3° C. / min and keeping the temperature for 3 hours to decompose and discharge the PVA, and then naturally cooling to room temperature to obtain a disc-shaped ceramic body from which the binder has been completely removed;
[0064] S7, sintering: sintering the disc-shaped ceramic body obtained in S5 after the binder is removed to obtain a sintered ceramic body; the sintering conditions are: firstly heating from room temperature to 1180°C at a heating rate of 5°C / min, sintering at a constant temperature for 2h, and then cooling to room temperature at a cooling rate of 5°C / min;
[0065] S8, polishing: grinding the upper and lower surfaces of the sintered ceramic body obtained in S7 with 600-mesh sandpaper, and then polishing with 2000-mesh sandpaper and corundum to a thickness of 0.35 mm, placing in deionized water, ultrasonically cleaning for 15 minutes, and drying to obtain a polished ceramic body;
[0066] The polished ceramic body of this embodiment was subjected to XRD test using a German Bruker D8 Advanced diffractometer, and the ceramic sample surface was subjected to SEM scanning test using a Japanese Hitachi S-4800 scanning electron microscope. The results are shown in Figures 1-2 , the prepared (Bi 0.5 Na 0.5 ) 0.8 Sr 0.07 Ba 0.07 Ca 0.06 Ti 0.75 (Nb 0.05 Mg 0.05 Ta 0.05 Zr 0.05 Sn 0.05 )O3 high entropy dielectric energy storage ceramic material is a pure perovskite structure with an average grain size of ~2.1μm and dense particle distribution.
[0067] S9, surface metallization: The upper and lower surfaces of the polished ceramic body obtained in S8 are uniformly coated with silver paste with a thickness of 0.02 mm, and then placed in a resistance furnace, and the temperature is raised to 850°C at a heating rate of 5°C / min, kept at this temperature for 10 minutes, and naturally cooled to room temperature to obtain sodium bismuth titanate-based high entropy dielectric energy storage ceramic material.
[0068] The bismuth titanate sodium-based high entropy dielectric energy storage ceramic material (Bi 0.5 Na 0.5 ) 0.8 Sr 0.07 Ba 0.07 Ca 0.06 Ti 0.75 (Nb 0.05 Mg 0.05 Ta 0.05 Zr 0.05 Sn 0.05 )O3 breakdown field strength, PE characteristics and energy storage performance were tested, and the results are shown in Table 2. PE curve, energy storage performance stability and fatigue performance curve are shown in Table 2. Figure 3-6 As shown, it has excellent temperature stability (W rec The change value is less than 6.6% in the temperature range of 25-200℃), frequency stability (W rec Variation value <3% in the range of 1-200Hz) and excellent fatigue properties (W rec In 10 6 The change in cycle range is <2.8%)
[0069] Table 2 Performance test of Example 2
[0070] Breakdown field strength Maximum polarization intensity Remanent polarization Effective energy storage density Energy storage efficiency 370kV / cm <![CDATA[27.8μC / cm 2 ]]> <![CDATA[0.94μC / cm 2 ]]> <![CDATA[4.33J / cm 3 ]]> 89.7%
[0071] The sodium bismuth titanate-based high entropy dielectric energy storage ceramic material prepared by the method of this embodiment is used for the preparation of high-power devices of pulse capacitors. The sodium bismuth titanate-based high entropy dielectric energy storage ceramic prepared in this embodiment is resistant to electromagnetic interference, has a short charge and discharge time, a long storage time, will not deteriorate and age, and has a high breakdown field strength, a large energy storage density and a relatively long life (>10 6 ), which is conducive to the development of miniaturization and lightweight of energy systems, and plays a very important role in national defense, scientific experiments, industry, agriculture, and medicine.
[0072] Example 3
[0073] The sodium bismuth titanate-based high entropy dielectric energy storage ceramic material of this embodiment has a composition formula of:
[0074] (Bi 0.5 Na 0.5 ) 0.8 Sr 0.07 Ba 0.07 Ca 0.06 Ti 0.75 (Nb0.05 Mg 0.05 Ta 0.05 Zr 0.05 Sn 0.05 )O3.
[0075] This embodiment also provides a method for preparing the above-mentioned sodium bismuth titanate-based high entropy dielectric energy storage ceramic material, which is:
[0076] S1. Drying materials: drying the Na2CO3 raw material, Bi2O3 raw material, CaCO3 raw material, BaCO3 raw material and SrCO3 raw material at a temperature of 300°C for 6 hours respectively;
[0077] The Nb2O5 raw material, the TiO2 raw material, the Ta2O5 raw material, the ZrO2 raw material, the MgO raw material and the SnO2 raw material were dried at a temperature of 900°C for 4h respectively;
[0078] The purity of the Na2CO3 raw material is 99.8%, the purity of the Bi2O3 raw material is 99%, the purity of the CaCO3 raw material is 99%, the purity of the BaCO3 raw material is 99%, the purity of the SrCO3 raw material is 99%, the purity of the Nb2O5 raw material is 99.5%, the purity of the TiO2 raw material is 98%, the purity of the Ta2O5 raw material is 99.99%, the purity of the ZrO2 raw material is 99%, the purity of the MgO raw material is 98.5%, and the purity of the SnO2 raw material is 99.5%; all the above raw materials were purchased from Sinopharm Chemical Reagent Co., Ltd.;
[0079] S2, ingredients: the dried Na2CO3 raw material, Bi2O3 raw material, CaCO3 raw material, BaCO3 raw material, SrCO3 raw material, Nb2O5 raw material, TiO2 raw material, Ta2O5 raw material, ZrO2 raw material, MgO raw material and SnO2 raw material in S1 are mixed according to (Bi 0.5 Na 0.5 ) 0.8 Sr 0.07 Ba 0.07 Ca 0.06 Ti 0.75 (Nb 0.05 Mg 0.05 Ta 0.05 Zr 0.05 Sn 0.05)O3 in a stoichiometric ratio are weighed and mixed uniformly to obtain a premix, agate balls and anhydrous ethanol are added, and the mixture is ball-milled at a speed of 330r / min in a planetary ball mill for 7h. After the agate balls are separated, the mixture is dried at a temperature of 90°C for 20h, and after grinding, it is sieved through a 120-mesh sieve to obtain a raw material mixture; the dosage ratio of the premix, agate balls and anhydrous ethanol is 0.30g:1g:0.45mL;
[0080] S3, pre-calcination: the raw material mixture obtained in S2 is heated from room temperature to 900°C at a heating rate of 4°C / min, then pre-calcined at a constant temperature for 3 hours, naturally cooled to room temperature, and ground to obtain pre-calcined powder;
[0081] S4, secondary ball milling: add agate balls and anhydrous ethanol to the pre-calcined powder obtained in S3, ball mill for 7 hours, separate the agate balls, dry at 90°C for 20 hours, grind and pass through a 180-mesh sieve to obtain the pre-calcined powder after ball milling; the amount ratio of the pre-calcined powder, agate balls and anhydrous ethanol is 0.28g:1g:0.40mL;
[0082] S5, tableting: adding a 6% polyvinyl alcohol aqueous solution to the pre-burned powder after ball milling obtained in S4, granulating and passing through a 40-mesh sieve to obtain a spherical powder material in the shape of quicksand, maintaining the pressure for 30 seconds under a uniaxial pressure of 150 MPa to obtain a disc-shaped ceramic body; the mass ratio of the 6% polyvinyl alcohol aqueous solution to the pre-burned powder after ball milling is 7%:1;
[0083] S6, debinding: heating the disc-shaped ceramic body obtained in S5 to 575° C. at a heating rate of 2° C. / min and keeping the temperature for 2 hours, and then naturally cooling to room temperature to obtain a disc-shaped ceramic body from which the binder has been completely removed;
[0084] S7, sintering: sintering the disc-shaped ceramic body obtained in S5 after the binder is removed to obtain a sintered ceramic body; the sintering conditions are: firstly heating from room temperature to 1200°C at a heating rate of 4°C / min, sintering at a constant temperature for 2.5h, and then cooling to room temperature at a cooling rate of 5°C / min;
[0085] S8, polishing: grinding the upper and lower surfaces of the sintered ceramic body obtained in S7 with 600-mesh sandpaper, and then polishing with 2000-mesh sandpaper and corundum to a thickness of 0.4 mm, placing in deionized water, ultrasonically cleaning for 20 minutes, and drying to obtain a polished ceramic body;
[0086] The polished ceramic body of this embodiment was subjected to XRD test using a German Bruker D8 Advanced diffractometer, and the ceramic sample surface was subjected to SEM scanning test using a Japanese Hitachi S-4800 scanning electron microscope. The results are shown in Figures 1-2 , the prepared (Bi 0.5Na 0.5 ) 0.8 Sr 0.07 Ba 0.07 Ca 0.06 Ti 0.75 (Nb 0.05 Mg 0.05 Ta 0.05 Zr 0.05 Sn 0.05 )O3 high entropy dielectric energy storage ceramic material is a pure perovskite structure with an average grain size of ~3.0μm and dense particle distribution.
[0087] S9, surface metallization: The upper and lower surfaces of the polished ceramic body obtained in S8 are uniformly coated with silver paste with a thickness of 0.02 mm, and then placed in a resistance furnace, and the temperature is raised to 850°C at a heating rate of 4°C / min, kept at this temperature for 10 minutes, and naturally cooled to room temperature to obtain sodium bismuth titanate-based high entropy dielectric energy storage ceramic material.
[0088] The sodium bismuth titanate-based high entropy dielectric energy storage ceramic material (Bi 0.5 Na 0.5 ) 0.8 Sr 0.07 Ba 0.07 Ca 0.06 Ti 0.75 (Nb 0.05 Mg 0.05 Ta 0.05 Zr 0.05 Sn 0.05 )O3 breakdown field strength, PE characteristics and energy storage performance results are shown in Table 3. rec The change value is less than 6.9% in the temperature range of 25-200℃, W rec Variation value <2.9% in the range of 1-200Hz, W rec In 10 6 The change in the cycle range was <2.9%.
[0089] Table 3 Performance test of Example 3
[0090] Breakdown field strength Maximum polarization intensity Remanent polarization Effective energy storage density Energy storage efficiency 365kV / cm <![CDATA[27.5μC / cm 2 ]]> <![CDATA[0.98μC / cm 2 ]]> <![CDATA[4.22J / cm 3 ]]> 89.9%
[0091] Example 4
[0092] The sodium bismuth titanate-based high entropy dielectric energy storage ceramic material of this embodiment has a composition formula of:
[0093] (Bi 0.5 Na 0.5 ) 0.8 Sr 0.07 Ba 0.07 Ca0.06 Ti 0.75 (Nb 0.05 Mg 0.05 Ta 0.05 Zr 0.05 Sn 0.05 )O3.
[0094] This embodiment also provides a method for preparing the above-mentioned sodium bismuth titanate-based high entropy dielectric energy storage ceramic material, which is:
[0095] S1. Drying materials: drying the Na2CO3 raw material, Bi2O3 raw material, CaCO3 raw material, BaCO3 raw material and SrCO3 raw material at a temperature of 300°C for 6 hours respectively;
[0096] The Nb2O5 raw material, the TiO2 raw material, the Ta2O5 raw material, the ZrO2 raw material, the MgO raw material and the SnO2 raw material were dried at a temperature of 900°C for 4h respectively;
[0097] The purity of the Na2CO3 raw material is 99.8%, the purity of the Bi2O3 raw material is 99%, the purity of the CaCO3 raw material is 99%, the purity of the BaCO3 raw material is 99%, the purity of the SrCO3 raw material is 99%, the purity of the Nb2O5 raw material is 99.5%, the purity of the TiO2 raw material is 98%, the purity of the Ta2O5 raw material is 99.99%, the purity of the ZrO2 raw material is 99%, the purity of the MgO raw material is 98.5%, and the purity of the SnO2 raw material is 99.5%; all the above raw materials were purchased from Sinopharm Chemical Reagent Co., Ltd.;
[0098] S2, ingredients: the dried Na2CO3 raw material, Bi2O3 raw material, CaCO3 raw material, BaCO3 raw material, SrCO3 raw material, Nb2O5 raw material, TiO2 raw material, Ta2O5 raw material, ZrO2 raw material, MgO raw material and SnO2 raw material in S1 are mixed according to (Bi 0.5 Na 0.5 ) 0.8 Sr 0.07 Ba 0.07 Ca 0.06 Ti 0.75 (Nb 0.05 Mg 0.05 Ta 0.05 Zr 0.05 Sn 0.05)O3 in a stoichiometric ratio are weighed and mixed uniformly to obtain a premix, agate balls and anhydrous ethanol are added, and the mixture is ball-milled at a speed of 300r / min in a planetary ball mill for 10h. After the agate balls are separated, the mixture is dried at a temperature of 120°C for 10h, and after grinding, it is sieved through a 120-mesh sieve to obtain a raw material mixture; the dosage ratio of the premix, agate balls and anhydrous ethanol is 0.30g:1g:0.45mL;
[0099] S3, pre-calcination: the raw material mixture obtained in S2 is heated from room temperature to 850°C at a heating rate of 3°C / min, then pre-calcined at a constant temperature for 4 hours, naturally cooled to room temperature, and ground to obtain pre-calcined powder;
[0100] S4, secondary ball milling: add agate balls and anhydrous ethanol to the pre-calcined powder obtained in S3, ball mill for 10 hours, separate the agate balls, dry at 120°C for 10 hours, grind and pass through a 180-mesh sieve to obtain the pre-calcined powder after ball milling; the amount ratio of the pre-calcined powder, agate balls and anhydrous ethanol is 0.28g:1g:0.40mL;
[0101] S5, tableting: adding a 6% polyvinyl alcohol aqueous solution to the pre-burned powder after ball milling obtained in S4, granulating and passing through a 40-mesh sieve to obtain a spherical powder material in the shape of quicksand, maintaining the pressure for 10 seconds under a uniaxial pressure of 200 MPa to obtain a disc-shaped ceramic body; the mass ratio of the 6% polyvinyl alcohol aqueous solution to the pre-burned powder after ball milling is 5%:1;
[0102] S6, debinding: heating the disc-shaped ceramic body obtained in S5 to 500° C. at a heating rate of 1° C. / min and keeping the temperature for 3 hours, and then naturally cooling to room temperature to obtain a disc-shaped ceramic body from which the binder has been completely removed;
[0103] S7, sintering: sintering the disc-shaped ceramic body obtained in S5 after the binder is removed to obtain a sintered ceramic body; the sintering conditions are: firstly heating from room temperature to 1220°C at a heating rate of 5°C / min, sintering at a constant temperature for 2h, and then cooling to room temperature at a cooling rate of 5°C / min;
[0104] S8, polishing: grinding the upper and lower surfaces of the sintered ceramic body obtained in S7 with 600-mesh sandpaper, and then polishing with 2000-mesh sandpaper and corundum to a thickness of 0.5 mm, placing in deionized water, ultrasonically cleaning for 20 minutes, and drying to obtain a polished ceramic body;
[0105] The polished ceramic body of this embodiment was subjected to XRD test using a German Bruker D8 Advanced diffractometer, and the ceramic sample surface was subjected to SEM scanning test using a Japanese Hitachi S-4800 scanning electron microscope. The results are shown in Figures 1-2 , the prepared (Bi 0.5Na 0.5 ) 0.8 Sr 0.07 Ba 0.07 Ca 0.06 Ti 0.75 (Nb 0.05 Mg 0.05 Ta 0.05 Zr 0.05 Sn 0.05 )O3 high entropy dielectric energy storage ceramic material is a pure perovskite structure with an average grain size of ~3.5μm and dense particle distribution.
[0106] S9, surface metallization: The upper and lower surfaces of the polished ceramic body obtained in S8 are uniformly coated with silver paste with a thickness of 0.03 mm, and then placed in a resistance furnace, and the temperature is raised to 850°C at a heating rate of 6°C / min, kept at this temperature for 10 minutes, and naturally cooled to room temperature to obtain sodium bismuth titanate-based high entropy dielectric energy storage ceramic material.
[0107] The sodium bismuth titanate-based high entropy dielectric energy storage ceramic material (Bi 0.5 Na 0.5 ) 0.8 Sr 0.07 Ba 0.07 Ca 0.06 Ti 0.75 (Nb 0.05 Mg 0.05 Ta 0.05 Zr 0.05 Sn 0.05 )O3 breakdown field strength, PE characteristics and energy storage performance results are shown in Table 4. rec The change value is less than 7% in the temperature range of 25-200℃, W rec Variation value <3% in the range of 1-200Hz, W rec In 10 6 The variation value within the cycle range is <3%.
[0108] Table 4 Performance test of Example 4
[0109]
[0110]
[0111] The sodium bismuth titanate-based high entropy dielectric energy storage ceramic material prepared by the method of this embodiment is used for the preparation of pulse capacitors.
[0112] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent change made to the above embodiment according to the technical essence of the invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. A sodium bismuth titanate-based high entropy dielectric energy storage ceramic material, It is characterized in that The composition formula of the sodium bismuth titanate-based high entropy dielectric energy storage ceramic material is: (Bi 0.5 So 0.5 ) 0.8 Sr 0.07 Ba 0.07 Approx 0.06 Tea 0.75 (Nb 0.05 Mg 0.05 Dad 0.05 Zr 0.05 Mr 0.05 )O 3 ; The sodium bismuth titanate-based high entropy dielectric energy storage ceramic material is used for the preparation of pulse capacitors; The sodium bismuth titanate-based high entropy dielectric energy storage ceramic material (Bi 0.5 Na 0.5 ) 0.8 Sr 0.07 Ba 0.07 Ca 0.06 Ti 0.75 (Nb 0.05 Mg 0.05 Ta 0.05 Zr 0.05 Sn 0.05 ) 3 The breakdown field strength is 359~370 kV / cm, and the energy storage density is W rec 4.16~4.33J / cm 3 , energy storage efficiency is 89.7~90.1%, temperature stability W rec The change value is less than 7% in the temperature range of 25-200 ℃, and the frequency stability performance is W rec The variation value in the range of 1-200 Hz is < 3%, and the fatigue properties W rec In 10 6 The change value within the cycle range is < 3%; The preparation method of the sodium bismuth titanate-based high entropy dielectric energy storage ceramic material is as follows: S1. Baking materials: respectively 2 CO 3 Raw materials, Bi 2 O 3 Raw materials, CaCO 3 Raw materials, BaCO 3 Raw materials and SrCO 3 The raw materials were dried at 300 °C for 6 h; Nb 2 O 5 Raw materials, TiO 2 Raw materials, Ta 2 O 5 Raw materials, ZrO 2 Raw materials, MgO raw materials and SnO 2 The raw materials were dried at 900 °C for 4 h; The Na 2 CO 3 The purity of the raw material is 99.8%. 2 O 3 The purity of the raw material is 99%, and the CaCO 3 The purity of the raw material is 99%. 3 The purity of the raw material is 99%. 3 The purity of the raw material is 99%, and the Nb 2 O 5 The purity of the raw material is 99.5%. 2 The purity of the raw material is 98%, and the Ta 2 O 5 The purity of the raw material is 99.99%. 2 The purity of the raw materials is 99%, the purity of the MgO raw materials is 98.5%, and the purity of the SnO 2 The purity of the raw material is 99.5%; S2, ingredients: dry the Na in S1 2 CO 3 Raw materials, Bi 2 O 3 Raw materials, CaCO 3 Raw materials, BaCO 3 Raw materials, SrCO 3 Raw materials, Nb 2 O 5 Raw materials, TiO 2 Raw materials, Ta 2 O 5 Raw materials, ZrO 2 Raw materials, MgO raw materials and SnO 2 Raw materials according to (Bi 0.5 Na 0.5 ) 0.8 Sr 0.07 Ba 0.07 Ca 0.06 Ti 0.75 (Nb 0.05 Mg 0.05 Ta 0.05 Zr 0.05 Sn 0.05 ) 3 The stoichiometric ratio of the premix is weighed and mixed uniformly to obtain a premix, agate balls and anhydrous ethanol are added, and the mixture is ball-milled in a planetary ball mill at a speed of 300 r / min to 400 r / min for 6 h to 10 h. After separating the agate balls, the mixture is dried at a temperature of 70°C to 120°C for 10 h to 24 h, and passed through a 120-mesh sieve after grinding to obtain a raw material mixture; the amount ratio of the premix, agate balls and anhydrous ethanol in S2 is 0.30 g:1 g:0.45 mL; S3, pre-calcination: the raw material mixture obtained in S2 is heated from room temperature to 850°C to 950°C at a heating rate of 3°C / min to 5°C / min, and then pre-calcined at a constant temperature for 2h to 4h, naturally cooled to room temperature, and ground to obtain pre-calcined powder; S4, secondary ball milling: add agate balls and anhydrous ethanol to the pre-calcined powder obtained in S3, ball mill for 6h to 10h, separate the agate balls, dry at a temperature of 70°C to 120°C for 10h to 24h, grind and pass through a 180-mesh sieve to obtain the pre-calcined powder after ball milling; the amount ratio of the pre-calcined powder, agate balls and anhydrous ethanol in S4 is 0.28g:1g:0.40mL; S5, tableting: add a 6% polyvinyl alcohol aqueous solution to the ball-milled pre-burned powder obtained in S4, granulate it and pass it through a 40-mesh sieve to obtain a spherical powder material in the shape of quicksand, and maintain the pressure for 10s to 60s under a uniaxial pressure of 100MPa to 200MPa to obtain a disc-shaped ceramic body; the mass ratio of the polyvinyl alcohol aqueous solution to the ball-milled pre-burned powder in S5 is (5% to 10%): 1; S6, debinding: heating the disc-shaped ceramic body obtained in S5 to 500°C~600°C at a heating rate of 1°C / min~3°C / min and keeping the temperature for 1h~3h, and then naturally cooling to room temperature to obtain a disc-shaped ceramic body from which debinding is completed; S7, sintering: sintering the disc-shaped ceramic body obtained in S5 after the binder is removed to obtain a sintered ceramic body; the sintering conditions are: firstly heating from room temperature to 1160°C to 1220°C at a heating rate of 3°C / min to 5°C / min, sintering at a constant temperature for 2h to 3h, and then cooling to room temperature at a cooling rate of 5°C / min; S8, polishing: grinding the upper and lower surfaces of the sintered ceramic body obtained in S7 with 600-mesh sandpaper, and then polishing with 2000-mesh sandpaper and corundum to a thickness of 0.3 mm to 0.5 mm, placing in deionized water, ultrasonically cleaning and drying to obtain a polished ceramic body; S9, surface metallization: The upper and lower surfaces of the polished ceramic body obtained in S8 are uniformly coated with silver paste with a thickness of 0.01 mm to 0.03 mm, and then placed in a resistance furnace, and the temperature is raised to 850°C at a heating rate of 3°C / min to 6°C / min, kept at this temperature for 10 minutes, and naturally cooled to room temperature to obtain sodium bismuth titanate-based high entropy dielectric energy storage ceramic material.
2. The sodium bismuth titanate-based high entropy dielectric energy storage ceramic material according to claim 1, It is characterized in that The ultrasonic cleaning time in S8 is 10 min to 20 min.
Citation Information
Patent Citations
High-entropy perovskite oxide doped ceramic, preparation method and application thereof
CN115991599A