Metal coating composition with improved oil resistance and adhesion, method for preparing the same, and metal article coated therewith
By using a composition of (meth)acrylic modified polyurethane and other components derived from dehydrated sugar alcohols, the problem of insufficient oil resistance and adhesion of existing biomass polyurethane adhesives is solved, and high efficiency on metal surfaces is achieved , environmentally friendly coating formed.
Patent Information
- Application Number
- CN202280015246.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-02-17
- Filing Date
- 2022-02-16
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2042-02-16
AI Technical Summary
The existing biomass-based polyurethane adhesives have shortcomings in oil resistance and adhesion, and lack environmental protection, making it difficult to replace petroleum-based raw materials.
Using a composition comprising (meth)acrylic modified polyurethane, (meth)acrylic monomer, epoxy resin, epoxy curing promoter and thermal polymerization initiator derived from a dehydrated sugar alcohol-alkylene oxide adduct, By specific ratios and preparation methods, a coating with excellent adhesion and oil resistance is formed.
A high adhesion and oil-resistant coating to metal surfaces is achieved, while excellent environmental protection and rapid curing speed due to the use of natural resources.
Smart Images

Figure BDA0004396613630000051 
Figure BDA0004396613630000061 
Figure BDA0004396613630000062
Abstract
Description
Technical Field
[0001] The present invention relates to a coating composition for metal having improved oil resistance and adhesion, a method for preparing the same, and a metal article coated with the same, and more particularly to a composition comprising a (meth)acrylic acid-modified polyurethane containing a polymerization unit derived from an anhydrosugar alcohol-alkylene oxide adduct, a (meth)acrylic acid monomer, and an epoxy resin, and can provide a coating having both excellent adhesion to metal and improved oil resistance. Background Art
[0002] Polyols and isocyanates, which are important components of polyurethane, are generally manufactured from petroleum-based raw materials. However, in the field of polyurethane, due to various reasons such as the accelerated consumption of petroleum resources, the need to reduce greenhouse gas emissions due to climate change, rising raw material prices, and the increased demand for renewable raw materials, a method for partially or completely replacing polyols and isocyanates prepared from petroleum-based raw materials with environmentally friendly ingredients is needed.
[0003] Polyol can be produced by renewable biomass such as plant natural oil, cellulose and lignin, and the biopolyol derived from plant natural oil has been produced on a commercial scale. The property of the biopolyol produced changes according to the type of the biomass used. Usually, castor oil and palm oil etc. are used to produce soft and hard polyurethane and synthetic polyol, and soybean oil is used to prepare polyol for soft polyurethane. But the shortcoming of the biopolyol based on biomass prepared at present is that they have high viscosity.
[0004] Isocyanates based on plant oils are aliphatic in nature, and their disadvantage is that they are less reactive than petroleum-based aromatic diisocyanates. Therefore, little research has been conducted on the preparation of diisocyanates using biomass.
[0005] Hydrogenated sugars (also called "sugar alcohols") are compounds obtained by adding hydrogen to the reducing end groups of sugars, and generally have the chemical formula HOCH2(CHOH) n CH2OH (where n is an integer from 2 to 5), according to the number of carbon atoms, hydrogenated sugars are divided into tetraols, pentanols, hexitols and heptanols (with 4, 5, 6 and 7 carbon atoms respectively). Among them, hexitols with 6 carbon atoms include sorbitol, mannitol, iditol, galactitol, etc., and sorbitol and mannitol are particularly effective substances.
[0006] Dehydrosugar alcohol is a substance formed by removing more than one water molecule from hydrogenated sugar. When one water molecule is removed, it has a tetraol form with four hydroxyl groups in the molecule. When two water molecules are removed, it has a diol form with two hydroxyl groups in the molecule. It can be prepared using hexitol derived from starch (e.g., Korean Patent No. 10-1079518, Korean Patent Gazette No. 10-2012-0066904). Since dehydrosugar alcohol is an environmentally friendly substance derived from renewable natural resources, it has long been a focus of attention, and research on its preparation method is underway. At present, among such dehydrosugar alcohols, isosorbide prepared from sorbitol has the widest industrial application range.
[0007] The use of dehydrosugar alcohol is very extensive, such as treating heart and vascular diseases, adhesives of patches, oral cleaners and other medicaments, solvents of compositions in the cosmetics industry, emulsifiers in the food industry, etc. In addition, dehydrosugar alcohol can increase the glass transition temperature of polymer substances such as polyester, PET, polycarbonate, polyurethane, epoxy resin, and has the effect of improving the strength of these substances, and dehydrosugar alcohol is an environmentally friendly material derived from natural resources, so it is also very useful in plastic industries such as bioplastics. In addition, it is known that dehydrosugar alcohol can also be used as an environmentally friendly solvent for adhesives, environmentally friendly plasticizers, biodegradable polymers, and water-soluble paints.
[0008] As mentioned above, anhydrosugar alcohols have attracted widespread attention due to their various application possibilities, and their use in actual industry has gradually increased.
[0009] In addition, Korean Patent Publication No. 10-2017-0125328 discloses the preparation of a metal-to-metal conductive adhesive using acrylic modified polyurethane and other acrylic monomers in the presence of a thermal polymerization initiator. However, the adhesive composition prepared by this method lacks oil resistance and its adhesiveness needs to be further improved. Summary of the invention
[0010] Technical issues to be solved
[0011] An object of the present invention is to provide a coating composition for metal, which can provide a coating having both adhesion to metal and improved oil resistance and excellent environmental protection by using a (meth)acrylic acid-modified polyurethane containing a polymerization unit derived from an anhydrosugar alcohol derivative, and a preparation method thereof, as well as a metal article coated with the composition.
[0012] Technical Solution
[0013] In order to achieve the above-mentioned object, the present invention provides a coating composition for metal, which comprises, based on a total of 100 parts by weight of the composition, 5.1-64.9 parts by weight of a (meth)acrylic acid modified polyurethane; 7.1-74.9 parts by weight of a (meth)acrylic acid monomer; 2.1-44.9 parts by weight of an epoxy resin; 0.051-2.49 parts by weight of an epoxy curing accelerator; and 0.00051-2.49 parts by weight of a thermal polymerization initiator, wherein the (meth)acrylic acid modified polyurethane comprises: i) a polymerization unit derived from an anhydrosugar alcohol-alkylene oxide adduct; ii) a polymerization unit derived from a polyisocyanate; and iii) a polymerization unit derived from a hydroxyalkyl (meth)acrylate.
[0014] According to another aspect of the present invention, a method for preparing a coating composition for metal is provided, comprising the following steps: based on a total of 100 parts by weight of the mixture, 5.1-64.9 parts by weight of a (meth)acrylic acid modified polyurethane, 7.1-74.9 parts by weight of a (meth)acrylic acid monomer, 2.1-44.9 parts by weight of an epoxy resin, 0.051-2.49 parts by weight of an epoxy curing accelerator and 0.00051-2.49 parts by weight of a thermal polymerization initiator are mixed, wherein the (meth)acrylic acid modified polyurethane contains: i) polymerization units derived from anhydrosugar alcohol-alkylene oxide adducts; ii) polymerization units derived from polyisocyanates; and iii) polymerization units derived from hydroxyalkyl (meth)acrylates.
[0015] According to another aspect of the present invention, a coated metal object is provided, comprising: a metal object; and a coating of the metal coating composition on the surface of the metal object of the present invention.
[0016] Beneficial Effects
[0017] The metal coating composition according to the present invention has excellent adhesion to metal and excellent oil resistance after coating, and has a fast curing speed, so that a coating with excellent oil resistance and adhesion can be quickly provided on the metal surface. Moreover, since anhydrosugar alcohol derived from natural resources is used, it is also environmentally friendly. DETAILED DESCRIPTION
[0018] Hereinafter, the present invention will be described in more detail.
[0019] The metal coating composition of the present invention comprises: (meth)acrylic acid modified polyurethane; (meth)acrylic acid monomer; epoxy resin; epoxy curing accelerator; and thermal polymerization initiator.
[0020] [(Meth)acrylic acid modified polyurethane]
[0021] The (meth)acrylic modified polyurethane contained in the coating composition for metal of the present invention comprises: i) polymerization units derived from anhydrosugar alcohol-alkylene oxide adduct; ii) polymerization units derived from polyisocyanate; and iii) polymerization units derived from hydroxyalkyl (meth)acrylate.
[0022] The anhydrosugar alcohol-alkylene oxide adduct (or, also referred to as "anhydrosugar alcohol-alkylene glycol") is an adduct obtained by reacting hydroxyl groups at both ends or one end (preferably both ends) of anhydrosugar alcohol with alkylene oxide, and means a compound in which hydrogen of hydroxyl groups at both ends or one end (preferably both ends) of anhydrosugar alcohol is substituted by hydroxyalkyl groups of an alkylene oxide in a ring-opened form.
[0023] In a specific embodiment, the alkylene oxide may be a linear alkylene oxide having 2 to 8 atoms or a branched alkylene oxide having 3 to 8 carbon atoms, and more specifically may be ethylene oxide, propylene oxide or a combination thereof.
[0024] The dehydrated sugar alcohol can be prepared by subjecting hydrogenated sugars derived from natural substances to a dehydration reaction. Hydrogenated sugars (also called "sugar alcohols") are compounds obtained by hydrogenating the reducing end groups of sugars, and generally have a chemical formula of HOCH2(CHOH): n CH2OH (where n is an integer from 2 to 5) is divided into tetraol, pentanol, hexitol and heptanol (having 4, 5, 6 and 7 carbon atoms, respectively) according to the number of carbon atoms. Among them, hexitol with 6 carbon atoms includes sorbitol, mannitol, iditol, galactitol, etc., and sorbitol and mannitol are particularly effective substances.
[0025] The anhydrosugar alcohol may be a monoanhydrosugar alcohol, a dianhydrosugar alcohol or a mixture thereof, but is not particularly limited, but a dianhydrosugar alcohol may be used.
[0026] Monoanhydrosugar alcohol is an anhydrosugar alcohol formed by removing one water molecule from the inside of hydrogenated sugar, and has a tetraol form with four hydroxyl groups in the molecule. In the present invention, the type of the monoanhydrosugar alcohol is not particularly limited, but preferably it can be monoanhydrohexitol, more specifically 1,4-anhydrohexitol, 3,6-anhydrohexitol, 2,5-anhydrohexitol, 1,5-anhydrohexitol, 2,6-anhydrohexitol or a mixture of two or more thereof.
[0027] Bis-anhydrosugar alcohols are anhydrosugar alcohols formed by removing two water molecules from the inside of hydrogenated sugars, have a diol form with two hydroxyl groups in the molecule, and can be prepared using hexitol derived from starch. Bis-anhydrosugar alcohols are environmentally friendly substances derived from renewable natural resources, so research on their production methods has long attracted attention. Among these bis-anhydrosugar alcohols, isosorbide prepared from sorbitol has the widest current industrial application range.
[0028] The type of the dianhydrosugar alcohol is not particularly limited, but preferably it can be dianhydrohexitol, more specifically 1,4:3,6-dianhydrohexitol. The 1,4:3,6-dianhydrohexitol can be isosorbide, isomannide, isoidide or a mixture of two or more thereof.
[0029] In a specific embodiment, the anhydrosugar alcohol-alkylene oxide adduct may be a compound represented by the following Chemical Formula 1 or a mixture of two or more of such compounds.
[0030] [Chemical formula 1]
[0031]
[0032] In the chemical formula 1, R 1 and R 2 Each independently represents a linear alkylene group having 2 to 8 carbon atoms or a branched alkylene group having 3 to 8 carbon atoms, m and n each independently represent an integer of 0 to 15, and m+n represents an integer of 1 to 30.
[0033] More preferably, in the chemical formula 1, R 1 and R 2 Each independently represents ethylene, propylene or isopropylene, preferably, R 1 and R 2 are the same as each other, m and n each independently represent an integer from 0 to 14, wherein m+n is an integer greater than 1, greater than 2 or greater than 3, and is an integer less than 25, less than 20, less than 15 or less than 12, for example, m+n represents an integer from 1 to 25, preferably represents an integer from 2 to 20, and more preferably represents an integer from 3 to 15.
[0034] In a specific embodiment, the anhydrosugar alcohol-alkylene oxide adduct may be an anhydrosugar alcohol-propylene oxide adduct represented by the following Chemical Formula 1-1, an anhydrosugar alcohol-ethylene oxide adduct represented by the following Chemical Formula 1-2, or a mixture thereof.
[0035] [Chemical formula 1-1]
[0036]
[0037] In the chemical formula 1-1, a and b each independently represent an integer from 0 to 15, and a+b represents an integer from 1 to 30. More preferably, in the chemical formula 1-1, a and b each independently represent an integer from 0 to 14, wherein a+b represents an integer of 1 or more, 2 or more, or 3 or more, and represents an integer of 25 or less, 20 or less, 15 or less, or 12 or less, for example, a+b represents an integer from 1 to 25, preferably an integer from 2 to 20, and more preferably an integer from 3 to 15.
[0038] [Chemical formula 1-2]
[0039]
[0040] In the chemical formula 1-2, c and d each independently represent an integer of 0 to 15, and c+d represents an integer of 1 to 30.
[0041] More preferably, in the chemical formula 1-2, c and d each independently represent an integer of 0 to 14, wherein c+d represents an integer of 1 or more, 2 or more or 3 or more, and represents an integer of 25 or less, 20 or less, 15 or less or 12 or less, for example, represents an integer of 1 to 25, preferably represents an integer of 2 to 20, and more preferably represents an integer of 3 to 15.
[0042] In a specific embodiment, the anhydrosugar alcohol-alkylene oxide adduct can be prepared by the following preparation method, which comprises the following steps: (1) treating the anhydrosugar alcohol with an acid component; and (2) subjecting the anhydrosugar alcohol treated with the acid component obtained in the step (1) to an addition reaction with alkylene oxide.
[0043] More specifically, the anhydrosugar alcohol-alkylene oxide adduct can be prepared by the following preparation method, which comprises the following steps: (1) treating anhydrosugar alcohol with an acid component; (2) subjecting the anhydrosugar alcohol treated with the acid component obtained in the step (1) to an addition reaction with alkylene oxide; and (3) subjecting the product obtained in the step (2) to an addition reaction with alkylene oxide in the presence of a base catalyst.
[0044] The acid component is not particularly limited, and an acid component selected from phosphoric acid, sulfuric acid, acetic acid, formic acid, heteropolyacid or their mixture can be used. In a specific embodiment, as the heteropolyacid, phosphotungstic acid, phosphomolybdic acid, silicotungstic acid or silicomolybdic acid etc. can be used, and as the acid component that can be used in addition, commercially available acid components such as Amberlyst 15 (Dow Chemical (Dow Chemical) Company (manufacture)) can also be used.
[0045] In a specific embodiment, in the acid treatment, 0.1-10 mol, preferably 0.1-8 mol, more preferably 0.1-5 mol of the acid component is used relative to 1 mol of the anhydrosugar alcohol, and it can be carried out under a nitrogen atmosphere at an elevated temperature (for example, 80-200° C. or 90-180° C.), and then vacuum decompression can be performed to remove moisture in the reactor, but it is not limited thereto.
[0046] The acid component used in the acid treatment promotes the ring-opening of the alkylene oxide in the addition reaction of the alkylene oxide described later.
[0047] Usually, the reaction of adding alkylene oxide to alcohol is carried out under the alkali catalyst, and in the case of dehydrated sugar alcohol, due to structural characteristics, the addition rate of alkylene oxide and the speed at which the ring structure of dehydrated sugar alcohol is opened and decomposed due to the alkali catalyst compete. Therefore, dehydrated sugar alcohol and the decomposition product of dehydrated sugar alcohol react with alkylene oxide, and the reaction product between the decomposition product of dehydrated sugar alcohol decomposed by the alkali catalyst and the alkylene oxide may become a factor that reduces the quality of the product and reduces the storage stability. However, after the dehydrated sugar alcohol is first treated with an acid component, when alkylene oxide is subjected to addition reaction, the acid component promotes the opening of alkylene oxide, and the decomposition product of dehydrated sugar alcohol caused by the alkali catalyst will not be produced, and due to the addition reaction of dehydrated sugar alcohol and alkylene oxide, dehydrated sugar alcohol-alkylene oxide adduct can be easily generated. Therefore, when the dehydrated sugar alcohol and alkylene oxide treated with acid are subjected to addition reaction, the existing problems can be solved.
[0048] In a specific embodiment, in the addition reaction of the dehydrated sugar alcohol treated with the acid component and the alkylene oxide, the alkylene oxide can be slowly added to the dehydrated sugar alcohol treated with the acid component at an elevated temperature (e.g., 100-180° C. or 120-160° C.), for example, for 1-8 hours or 2-4 hours, but not limited thereto. For the reaction molar ratio of the dehydrated sugar alcohol and the alkylene oxide, for example, per 1 mole of the dehydrated sugar alcohol, the alkylene oxide can be 1 mole or more or 2 moles and 30 moles or less, 20 moles or less, 15 moles or less or 12 moles or less, for example, 1-30 moles, preferably 2-20 moles, but not limited thereto.
[0049] In a specific embodiment, the further addition reaction of the product obtained by the addition reaction of the alkylene oxide and the additional alkylene oxide can be carried out, for example, in a high-pressure reactor that can be pressurized (for example, pressurized to 3 MPa or more), in the presence of an alkali catalyst (for example, an alkali metal hydroxide such as sodium hydroxide, potassium hydroxide or an alkaline earth metal hydroxide such as calcium hydroxide), at an elevated temperature (for example, 100-180° C. or 120-160° C.), for example, 1-8 hours or 2-4 hours, but is not limited thereto. For the reaction molar ratio of the dehydrosugar alcohol and the alkylene oxide, for example, per 1 mole of the dehydrosugar alcohol, the alkylene oxide can be more than 1 mole, more than 2 moles or more than 3 moles and less than 30 moles, less than 20 moles, less than 15 moles or less than 12 moles, for example, 1-30 moles, preferably 2-20 moles, more preferably 3-15 moles, but is not limited thereto. Before adding the alkali catalyst, the acid component used for treatment can be filtered out.
[0050] The product obtained by the addition reaction of the dehydrated sugar alcohol and alkylene oxide treated with acid (i.e., the compound in the form of alkylene oxide added to the dehydrated sugar alcohol) has a very stable structure, so even if there is an alkali catalyst, the ring structure of the dehydrated sugar alcohol is not easy to open or decompose at high temperature. Therefore, it is very conducive to making the alkylene oxide undergo further addition reaction. When the acid catalyst is continued to be used during the further addition reaction of the alkylene oxide, the acid catalyst contributes to the opening of the alkylene oxide, but the reaction speed decreases with the increase of the number of moles of the addition of the alkylene oxide. That is, the addition rate of the alkylene oxide competes with the opening rate of the alkylene oxide itself, and at this time, the addition rate of the alkylene oxide slows down, and self-condensation reaction occurs between the ring-opened alkylene oxides and generates by-products, so it may cause quality reduction. Therefore, the further addition reaction of the alkylene oxide is carried out under an alkali catalyst.
[0051] Thereafter, a step of removing the metal ions released from the alkaline catalyst used may be further performed. For this purpose, a metal ion adsorbent such as Ambosol MP20 (magnesium silicate component) may be used.
[0052] In a specific embodiment, examples of the polyisocyanate may be methylene diphenyl diisocyanate (MDI) (e.g., 2,4- or 4,4'-methylene diphenyl diisocyanate), xylylene diisocyanate (XDI), m- or p-tetramethylxylylene diisocyanate (TMXDI), toluene diisocyanate (TDI), di- or tetra-alkyl diphenylmethane diisocyanate, 3,3'-dimethyldiphenyl-4,4'-diisocyanate (TODI), phenylene diisocyanate (e.g., 1,3-phenylene diisocyanate, 1,4-phenylene diisocyanate), naphthalene diisocyanate (naphthalene diisocyanate), diisocyanate, NDI) or 4,4'-dibenzyl diisocyanate and other aromatic polyisocyanates; hydrogenated MDI (H12MDI), 1-methyl-2,4-diisocyanatocyclohexane, 1,12-diisocyanatododecane, 1,6-diisocyanato-2,2,4-trimethylhexane, 1,6-diisocyanato-2,4,4-trimethylhexane, isophorone diisocyanate (isophorone diisocyanate, IPDI), tetramethoxybutane-1,4-diisocyanate, butane-1,4-diisocyanate, hexamethylene diisocyanate (HDI) (for example, 1,6-hexamethylene diisocyanate), dimer fatty acid diisocyanate, dicyclohexylmethane diisocyanate, cyclohexane diisocyanate (for example, cyclohexane-1,4-diisocyanate) or ethylene diisocyanate and other aliphatic polyisocyanates; or combinations thereof, but not limited thereto.
[0053] In another specific embodiment, examples of the polyisocyanate may be methylene diphenyl diisocyanate (MDI), ethylene diisocyanate, 1,4-tetramethylene diisocyanate, 1,6-hexamethylene diisocyanate, 1-12-dodecane diisocyanate, cyclobutane-1,3-diisocyanate, cyclohexane-1,3-diisocyanate, cyclohexane-1,4-diisocyanate, isophorone diisocyanate, 2,4-hexahydrotoluene diisocyanate, 2,6-hexahydrotoluene diisocyanate, dicyclohexylmethane-4,4'-diisocyanate ester (HMDI), 1,3-phenylene diisocyanate, 1,4-phenylene diisocyanate, 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, toluene diisocyanate mixed with 2,4-toluene diisocyanate and 2,6-toluene diisocyanate (2,4- / 2,6-isomer ratio = 80 / 20), diphenylmethane-2,4'-diisocyanate, diphenylmethane-4,4'-diisocyanate, polydiphenylmethane diisocyanate (PMDI), naphthalene-1,5-diisocyanate or a combination thereof, but is not limited thereto.
[0054] More specifically, the polyisocyanate may be methylene diphenyl diisocyanate (MDI), toluene diisocyanate (TDI), hexamethylene diisocyanate (HDI), isophorone diisocyanate (IPDI), or a combination thereof.
[0055] In a specific embodiment, the example of the hydroxyalkyl (meth)acrylate can be a linear alkyl acrylate or branched alkyl acrylate having a hydroxyl group, a linear alkyl methacrylate or branched alkyl methacrylate having a hydroxyl group, or a combination thereof, more specifically a linear alkyl acrylate or branched C1-C8 alkyl acrylate having a hydroxyl group, a linear alkyl methacrylate or branched C1-C8 alkyl methacrylate having a hydroxyl group, or a combination thereof, and further specifically hydroxymethyl acrylate, hydroxymethyl methacrylate, hydroxyethyl acrylate, methacrylate The acrylate, hydroxypropyl methacrylate, hydroxybutyl acrylate, hydroxybutyl methacrylate, hydroxypentyl acrylate, hydroxypentyl methacrylate, 2-hydroxyethylhexyl acrylate, 2-hydroxyethylhexyl methacrylate, 2-hydroxyethylbutyl acrylate, 2-hydroxyethylbutyl methacrylate, hydroxyoctyl acrylate, hydroxyoctyl methacrylate or a combination thereof; further specifically, 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, hydroxypropyl acrylate, hydroxypropyl methacrylate, hydroxybutyl acrylate, hydroxybutyl methacrylate or a combination thereof, but is not limited thereto.
[0056] In a specific embodiment, the (meth)acrylic modified polyurethane may be represented by the following Chemical Formula 2:
[0057] [Chemical formula 2]
[0058]
[0059] In the chemical formula 2, R1 is independently an alkylene group, specifically a C2-C8 straight chain alkylene group or a C3-C8 branched chain alkylene group, more specifically a C2-C6 straight chain alkylene group or a C3-C6 branched chain alkylene group, R2 is independently an alkylene group, a cycloalkylene group or an arylene group, specifically a C2-C20 straight chain alkylene group or a C3-C20 branched chain alkylene group, a C3-C20 cycloalkylene group or a C6-C20 arylene group, and R3 is independently an alkylene group. R4 is each independently a hydrogen atom or an alkyl group, specifically a hydrogen atom or a C1-C4 straight chain alkyl group or a C3-C4 branched chain alkyl group, M is a divalent organic group derived from anhydrosugar alcohol, specifically a divalent organic group derived from isosorbide, isomannide or isoidide, and is more specifically selected from the following chemical formulas:
[0060]
[0061] m and n each independently represent an integer of 0 to 15, and m+n represents an integer of 1 to 30, more specifically an integer of 1 to 25, further specifically an integer of 1 to 20, further specifically an integer of 3 to 15, further specifically an integer of 5 to 15.
[0062] More specifically, the (meth)acrylic modified polyurethane may be represented by any one of the following chemical formulas, but is not limited thereto:
[0063]
[0064]
[0065] In the chemical formula, m, n and m+n are each independently the same as defined in the chemical formula 2.
[0066] The (meth)acrylic acid-modified polyurethane may be obtained by reacting an anhydrosugar alcohol-alkylene oxide adduct with polyisocyanate and then reacting the adduct with hydroxyalkyl (meth)acrylate.
[0067] In a specific embodiment, the (meth)acrylic acid modified polyurethane can be prepared by the following method, which includes the following steps: (1) reacting an anhydrosugar alcohol-alkylene oxide adduct with a polyisocyanate to prepare an intermediate having an isocyanate group terminal; and (2) reacting the intermediate obtained from the step (1) with a hydroxyalkyl (meth)acrylate.
[0068] According to a specific embodiment, an intermediate having an isocyanate group terminal can be prepared by reacting 1 equivalent of an anhydrosugar alcohol (e.g., isosorbide (ISB))-alkylene oxide adduct with 2 equivalents of diisocyanate, and then the isocyanate group terminal of the intermediate is reacted with 2 equivalents of hydroxyalkyl (meth)acrylate (e.g., 2-hydroxyethyl methacrylate) to prepare the (meth)acrylic modified polyurethane.
[0069] In the case of an acrylic modified polyurethane prepared by using a general alkylene oxide (e.g., ethylene oxide or polypropylene oxide, etc.) instead of an anhydrosugar alcohol-alkylene oxide adduct, there occurs a problem that the oil resistance of a coating formed from a composition including the acrylic modified polyurethane is reduced (when polypropylene oxide is used) or the adhesion of a coating formed from a composition including the acrylic modified polyurethane is reduced (when ethylene oxide is used).
[0070] According to a specific embodiment, the reaction of the anhydrosugar alcohol-alkylene oxide adduct and the polyisocyanate can be carried out in the presence of any catalyst (for example, a tin-based catalyst such as dibutyltin dilaurate (DBTDL)) at room temperature or at an elevated temperature (for example, 50-100° C., preferably 50-70° C.) for an appropriate time (for example, 0.1-5 hours, preferably 0.5-2 hours).
[0071] According to a specific embodiment, the reaction of the reaction product of the anhydrosugar alcohol-alkylene oxide adduct and the polyisocyanate (i.e., the intermediate obtained in the step (1)) and the hydroxyalkyl (meth)acrylate can be optionally carried out in the presence of a catalyst (e.g., a tin-based catalyst such as dibutyltin dilaurate (DBTDL)) at an elevated temperature (e.g., 50-100° C., preferably 50-70° C.) for a suitable time (e.g., 0.1-5 hours, preferably 0.5-2 hours).
[0072] The metal coating composition of the present invention contains 5.1-64.9 parts by weight of the (meth)acrylic acid modified polyurethane based on 100 parts by weight of the composition. When the content of the (meth)acrylic acid modified polyurethane in 100 parts by weight of the composition is less than 5.1 parts by weight, the adhesion of the coating formed by the composition containing the (meth)acrylic acid modified polyurethane is reduced, and its oil resistance is greatly reduced. On the other hand, when the content of the (meth)acrylic acid modified polyurethane exceeds 64.9 parts by weight, the adhesion of the coating formed by the composition containing the (meth)acrylic acid modified polyurethane is reduced.
[0073] More specifically, the content of the (meth)acrylic modified polyurethane in 100 parts by weight of the metal coating composition of the present invention can be, for example, 5.1 parts by weight or more, 5.5 parts by weight or more, 6 parts by weight or more, 6.5 parts by weight or more, 7 parts by weight or more, 7.5 parts by weight or more, 8 parts by weight or more, 8.5 parts by weight or more, 9 parts by weight or more, 9.5 parts by weight or more, or 10 parts by weight or more, and can be 64.9 parts by weight or less, 64.5 parts by weight or less, 64 parts by weight or less, 63.5 parts by weight or less, 63 parts by weight or less, 62.5 parts by weight or less, 62 parts by weight or less, 61.5 parts by weight or less, 61 parts by weight or less, 60.5 parts by weight or less, but is not limited thereto.
[0074] [(Meth)acrylic acid monomer]
[0075] The (meth)acrylic acid monomer contained in the metal coating composition of the present invention can improve the workability such as applicability on metal by adjusting the viscosity of the metal coating composition, increase the thermal curing speed of the metal coating composition, and improve the strength of the cured product, thereby improving the adhesion.
[0076] The (meth)acrylic acid monomer contained in the metal coating composition of the present invention may be a monomer having a (meth)acrylic acid group in the molecule, and preferably may be one or a mixture of two or more monomers having 1 to 6 (specifically 1 to 4) (meth)acrylic acid groups in the molecule.
[0077] In a specific embodiment, as the (meth)acrylic acid monomer, the monomer having one (meth)acrylic acid group may be, for example, (meth)acrylic acid, lauryl (meth)acrylate, stearyl (meth)acrylate, ethyl carbitol (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, caprolactone-modified tetrahydrofurfuryl (meth)acrylate, cyclohexyl (meth)acrylate, dicyclopentanyl (meth)acrylate, isobornyl (meth)acrylate, benzyl (meth)acrylate, phenyl (meth)acrylate, phenoxyethyl (meth)acrylate, phenoxydiglycol (meth)acrylate, phenoxytetraglycol (meth)acrylate, nonylphenoxyethyl (meth)acrylate, nonylphenoxytetraglycol (meth)acrylate, methoxydiglycol (meth)acrylate, ethoxydiglycol (meth)acrylate, butoxyethyl (meth)acrylate, butoxytriglycol (meth)acrylate, 2-ethylhexyl Polyethylene glycol (meth)acrylate, nonylphenyl polypropylene glycol (meth)acrylate, methoxydipropylene glycol (meth)acrylate, glycidyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, glycerol (meth)acrylate, polyethylene glycol (meth)acrylate, polypropylene glycol (meth)acrylate, epichlorohydrin (hereinafter referred to as ECH)-modified butyl (meth)acrylate, ECH-modified phenoxy (meth)acrylate, ethylene oxide (hereinafter referred to as EO)-modified phthalic acid (meth)acrylate, EO-modified succinic acid (meth)acrylate, caprolactone-modified 2-hydroxyethyl (meth)acrylate, N,N-dimethylaminoethyl (meth)acrylate, N,N-diethylaminoethyl (meth)acrylate, (2-methyl-2-ethyl-1,3-dioxolan-4-yl)methyl (meth)acrylate, or a mixture thereof, but the present invention is not limited thereto.
[0078] In another specific embodiment, as the (meth)acrylic monomer, the monomer having two or more (meth)acrylic groups may be, for example, 1,6-hexanediol diacrylate (HDDA), 1,4-butylene glycol diacrylate (BDDA), tripropylene glycol diacrylate (TPGDA), bisphenol A [EO] 4-30 diacrylate (bisphenol A [EO] 4-30 diacrylate, BPA [EO] 4-30 DA, EO is an ethylene oxide unit), trimethylolpropane triacrylate (TMPTA), trimethylolpropane [EO] 3-15 triacrylate (trimethylolpropane [EO] 3-15 triacrylate, TMP [EO] 3-15 TA, EO is an ethylene oxide unit), pentaerythritol triacrylate (PETA), pentaerythritol tetraacrylate (pentaerythritol triacrylate, PETA), pentaerythritol tetraacrylate (pentaerythritol tetra ... tetraacrylate (PETTA), ditrimethylolpropane tetraacrylate (DTMPTTA), dipentaerylthritol pentaacrylate (DPPA), dipentaerythritol hexaacrylate (DPHA) or a mixture thereof, but not limited thereto.
[0079] The metal coating composition of the present invention contains 7.1-74.9 parts by weight of the (meth)acrylic acid monomer based on 100 parts by weight of the composition. When the content of the (meth)acrylic acid monomer in 100 parts by weight of the composition is less than 7.1 parts by weight, the adhesion of the coating formed by the composition containing the (meth)acrylic acid monomer is greatly reduced, and the oil resistance is reduced. On the other hand, when the content of the (meth)acrylic acid monomer exceeds 74.9 parts by weight, the oil resistance of the coating formed by the composition containing the (meth)acrylic acid monomer is greatly reduced.
[0080] More specifically, the content of the (meth)acrylic acid monomer in 100 parts by weight of the metal coating composition of the present invention can be, for example, 7.1 parts by weight or more, 7.5 parts by weight or more, 8 parts by weight or more, 8.5 parts by weight or more, 9 parts by weight or more, 9.5 parts by weight or more, or 10 parts by weight or more, and can be 74.9 parts by weight or less, 74.5 parts by weight or less, 74 parts by weight or less, 73.5 parts by weight or less, 73 parts by weight or less, 72.5 parts by weight or less, 72 parts by weight or less, 71.5 parts by weight or less, 71 parts by weight or less, 70.5 parts by weight or less, but is not limited thereto.
[0081] [Epoxy resin]
[0082] The epoxy resin contained in the metal coating composition of the present invention is used to improve adhesion by increasing the strength of a cured product of the metal coating composition.
[0083] The epoxy resin is a resin having an epoxy group in its molecule, and preferably may be one or a mixture of two or more resins having two or more epoxy groups in its molecule.
[0084] In a specific embodiment, the epoxy resin can be, for example, a bisphenol-based epoxy resin, a phenol novolac-based epoxy resin, a cresol novolac-based epoxy resin, a multifunctional epoxy resin, an amino-based epoxy resin, a heterocyclic epoxy resin, a substituted epoxy resin, a naphthol-based epoxy resin, or a mixture thereof, but is not limited thereto.
[0085] In the metal coating composition of the present invention, the content of the epoxy resin is 2.1-44.9 parts by weight based on a total of 100 parts by weight of the composition. When the content of the epoxy resin in a total of 100 parts by weight of the composition is less than 2.1 parts by weight, the adhesion of the coating formed by the composition containing the epoxy resin is reduced, and on the other hand, when the content of the epoxy resin exceeds 44.9 parts by weight, the adhesion of the coating formed by the composition containing the epoxy resin is reduced, and the oil resistance is reduced.
[0086] More specifically, the content of the epoxy resin in 100 parts by weight of the metal coating composition of the present invention can be, for example, more than 2.1 parts by weight, more than 2.5 parts by weight, more than 3 parts by weight, more than 3.5 parts by weight, more than 4 parts by weight, more than 4.5 parts by weight or more than 5 parts by weight, and can be less than 44.9 parts by weight, less than 44.5 parts by weight, less than 44 parts by weight, less than 43.5 parts by weight, less than 43 parts by weight, less than 42.5 parts by weight, less than 42 parts by weight, less than 41.5 parts by weight, less than 41 parts by weight, less than 40.5 parts by weight, less than 40 parts by weight or less than 39 parts by weight, but is not limited to this.
[0087] [Epoxy curing accelerator]
[0088] The epoxy curing accelerator contained in the metal coating composition of the present invention is used to increase the curing speed of the epoxy resin.
[0089] In a specific embodiment, the epoxy curing accelerator can be, for example, a substituted imidazole (e.g., 1-methylimidazole, 2-methylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 1-cyanoethylimidazole), an imidazoline (e.g., 2-phenylimidazoline), a tertiary amine (e.g., N,N-dimethylbenzylamine), 2,4,6-tris(dimethylaminomethyl)phenol (DMP30), bisphenol A, bisphenol F, nonylphenol, p-tert-butylphenol, novolac type phenolic resin, salicylic acid, p-toluenesulfonic acid, 1,4-diazabicyclo[2.2.2]octane (DABCO), 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU), S-triazine (e.g., Lupragen N600), bis(2-dimethylaminoethyl)ether (e.g., Lupragen N206), pentamethyldiethylenetriamine (e.g., Lupragen N301), trimethylaminoethylethanolamine (e.g., Lupragen N400), tetramethyl-1,6-hexanediamine (e.g., Lupragen N500), aminoethylmorpholine, aminopropylmorpholine, aminoethylethyleneurea, ketimines (e.g., Epi-Kure 3502) (reaction product of ethylenediamine and methyl isobutyl ketone), urons (e.g., 3-(4-chlorophenyl)-1,1-dimethylurea (monuron), 3-(3,4-dichlorophenyl)-1,1-dimethylurea (diuron), 3-phenyl-1,1-dimethylurea (phenuron), and 3-(3-chloro-4-methylphenyl)-1,1-dimethylurea (chlorotoluron)), tolyl-2,4-bis-N,N-dimethylurea (e.g., Amicure UR2T), dicyandiamide (DICY), Mannich bases or secondary amines (e.g., dialkylamines such as di(2-ethylhexyl)amine, dibutylamine, dipropylamine, tricosylamine), N,N'-diisopropylisophoronediamine (e.g., XTJ-584), N,N'-diisobutyl-4,4'-diaminodicyclohexylmethane (eg, ClearLink 1000), N-(hydroxyethyl)aniline and di(2-methoxyethyl)amine or a combination thereof, but is not limited thereto.
[0090] The metal coating composition of the present invention contains 0.051-2.49 parts by weight of the epoxy curing accelerator based on 100 parts by weight of the composition. When the content of the epoxy resin in the total 100 parts by weight of the composition is less than 0.051 parts by weight, the composition containing the epoxy resin cannot be cured and cannot form a coating. On the other hand, when the content of the epoxy resin exceeds 2.49 parts by weight, the adhesion of the coating formed by the composition containing the epoxy resin is greatly reduced, and the oil resistance is greatly reduced.
[0091] More specifically, the content of the epoxy curing accelerator in 100 parts by weight of the metal coating composition of the present invention can be, for example, 0.051 parts by weight or more, 0.055 parts by weight or more, 0.06 parts by weight or more, 0.065 parts by weight or more, 0.07 parts by weight or more, 0.075 parts by weight or more, 0.08 parts by weight or more, 0.085 parts by weight or more, 0.09 parts by weight or more, 0.095 parts by weight or more, or 0.1 parts by weight or more, and can be 2.49 parts by weight or less, 2.45 parts by weight or less, 2.4 parts by weight or less, 2.35 parts by weight or less, 2.3 parts by weight or less, 2.25 parts by weight or less, 2.2 parts by weight or less, 2.15 parts by weight or less, 2.1 parts by weight or less, 2.05 parts by weight or less, 2 parts by weight or less, 1.5 parts by weight or less, or 1 part by weight or less, but is not limited thereto.
[0092] [Thermal polymerization initiator]
[0093] The thermal polymerization initiator contained in the metal coating composition of the present invention is used to initiate polymerization of the (meth)acrylic monomer and the (meth)acrylic modified polyurethane, thereby promoting curing.
[0094] In a specific embodiment, the thermal polymerization initiator may be selected from a compound represented by the following Chemical Formula 3-1, a compound represented by the following Chemical Formula 3-2, or a mixture thereof.
[0095] [Chemical formula 3-1]
[0096]
[0097] In the chemical formula 3-1, R and R' are each independently a C2-C8 straight chain alkyl group or a C3-C8 branched chain alkyl group; a C3-C20 cycloalkyl group; a C6-C20 aryl group; or a C2-C8 straight chain methoxy-alkyl group or a C3-C8 branched chain methoxy-alkyl group, and X is -CN or -CO2R", wherein R" is a C2-C8 straight chain alkyl group or a C3-C8 branched chain alkyl group; a C3-C20 cycloalkyl group; or a C6-C20 aryl group.
[0098] [Chemical formula 3-2]
[0099]
[0100] In the chemical formula 3-2, each R is independently a C2-C8 straight-chain alkyl group or a C3-C8 branched-chain alkyl group; a C3-C20 cycloalkyl group; or a C6-C20 aryl group.
[0101] The metal coating composition of the present invention contains 0.00051-2.49 parts by weight of the thermal polymerization initiator based on 100 parts by weight of the composition. When the content of the thermal polymerization initiator in the total 100 parts by weight of the composition is less than 0.00051 parts by weight, the composition containing the thermal polymerization initiator cannot be cured and cannot form a coating. On the other hand, when the content of the thermal polymerization initiator exceeds 2.49 parts by weight, the adhesion of the coating formed by the composition containing the thermal polymerization initiator is greatly reduced, and the oil resistance is greatly reduced.
[0102] More specifically, the content of the thermal polymerization initiator in 100 parts by weight of the metal coating composition of the present invention can be, for example, 0.00051 parts by weight or more, 0.00055 parts by weight or more, 0.0006 parts by weight or more, 0.00065 parts by weight or more, 0.0007 parts by weight or more, 0.00075 parts by weight or more, 0.0008 parts by weight or more, 0.00085 parts by weight or more, 0.0009 parts by weight or more, 0.00095 parts by weight or more, 0.0010 parts by weight or more, 0.00115 parts by weight or more, 0.00125 parts by weight or more, 0.00135 parts by weight or more, 0.00145 parts by weight or more, 0.00155 parts by weight or more, 0.00165 parts by weight or more, 0.00175 parts by weight or more, 0.00185 parts by weight or more, 0.00195 parts by weight or more, 0.00205 parts by weight or more, 0.00215 parts by weight or more, 0.00225 parts by weight or more, 0.00235 parts by weight or more, 0.00245 parts by weight or more, 0.00255 parts by weight or more, 0.00265 parts by weight or more, 0.00275 parts by weight or more, 0.00285 parts by weight or more, 0.00295 parts by weight or more, 0.00305 parts by weight or more, 0.00315 parts by weight or more, 0.00325 parts by weight or more, 0.00335 parts by weight or more, 0.00 .001 parts by weight or more, 0.005 parts by weight or more, or 0.01 parts by weight or more, and may be 2.49 parts by weight or less, 2.45 parts by weight or less, 2.4 parts by weight or less, 2.35 parts by weight or less, 2.3 parts by weight or less, 2.25 parts by weight or less, 2.2 parts by weight or less, 2.15 parts by weight or less, 2.1 parts by weight or less, 2.05 parts by weight or less, 2 parts by weight or less, 1.5 parts by weight or less, 1 part by weight or less, or 0.5 parts by weight or less, but is not limited thereto.
[0103] The coating composition for metal of the present invention may further contain additives that can be generally used for coating compositions for metal, in addition to the above-mentioned components.
[0104] [Method for preparing a coating composition for metal]
[0105] According to another aspect of the present invention, a method for preparing a coating composition for metal is provided, the method comprising the following steps: based on a total of 100 parts by weight of the mixture, 5.1-64.9 parts by weight of a (meth)acrylic acid modified polyurethane, 7.1-74.9 parts by weight of a (meth)acrylic acid monomer, 2.1-44.9 parts by weight of an epoxy resin, 0.051-2.49 parts by weight of an epoxy curing accelerator and 0.00051-2.49 parts by weight of a thermal polymerization initiator are mixed, wherein the (meth)acrylic acid modified polyurethane contains: i) polymerization units derived from anhydrosugar alcohol-alkylene oxide adducts; ii) polymerization units derived from polyisocyanates; and iii) polymerization units derived from hydroxyalkyl (meth)acrylates.
[0106] In the method for preparing a metal coating composition of the present invention, the specific types and usage amounts of the (meth)acrylic modified polyurethane, (meth)acrylic monomer, epoxy resin, epoxy curing accelerator and thermal polymerization initiator are as described above.
[0107] In a preferred embodiment, the mixing of the (meth)acrylic modified polyurethane, (meth)acrylic monomer, epoxy resin, epoxy curing accelerator and thermal polymerization initiator may be performed at a temperature of 60° C. or less (e.g., 10-60° C., more specifically 20-60° C.). When the temperature of the components is higher than 60° C., the polymerization reaction of the (meth)acrylic monomer may be performed during the mixing while curing may occur during the preparation of the composition, and thus it may be difficult to use as a coating composition.
[0108] [Coated metal objects]
[0109] According to another aspect of the present invention, there is provided a coated metal article, comprising: a metal article; and a coating layer of the metal coating composition of the present invention on a surface of the metal article.
[0110] In a specific embodiment, the metal article may be a mechanical component, an electrical component or an electronic component, but is not limited thereto.
[0111] The method of forming a coating layer of the coating composition for metal of the present invention on the metal article is not particularly limited, and can be performed using a general coating method and equipment.
[0112] Hereinafter, the present invention will be described in more detail by way of examples and comparative examples, but the scope of the present invention is not limited thereto.
[0113] [Example]
[0114] <Preparation of Anhydrosugar Alcohol-Alkylene Oxide Adduct>
[0115] Preparation Example A1: Preparation of 5 mole adduct of isosorbide-ethylene oxide
[0116] 146 g of isosorbide was added to a pressurized reactor, 0.15 g of phosphoric acid (85%) was added as an acid component, and then the interior of the reactor was replaced with nitrogen, heated to 100° C., and the moisture in the reactor was removed by vacuum decompression. Then, 88 g of ethylene oxide was slowly added to the reactor at one time, and they were reacted at a temperature of 100-140° C. for 2-3 hours. At this time, the reaction temperature was adjusted so that the reaction temperature did not exceed 140° C. After that, after the internal temperature of the reactor was cooled to 50° C., 0.3 g of potassium hydroxide was added to the reactor, the interior of the reactor was replaced with nitrogen, and heated to 100° C., and the moisture in the reactor was removed by vacuum decompression. Then, 132 g of ethylene oxide was slowly added twice, and reacted at 100-140° C. for 2-3 hours. When the reaction is completed, the internal temperature of the reactor is cooled to 50°C, 4.0 g of Ambosol MP20 as an adsorbent is added, and the mixture is heated again and stirred at a temperature of 100-120°C for 1-5 hours to remove metal ions. At this time, the interior of the reactor is replaced with nitrogen and / or vacuum pressure is applied. When no metal ions are detected, the internal temperature of the reactor is cooled to 60-90°C, and then 362 g of a transparent liquid phase isosorbide-ethylene oxide 5 mol adduct is obtained by removing the residual by-products.
[0117] Preparation Example A2: Preparation of 10 mole adduct of isosorbide-ethylene oxide
[0118] 551 g of a transparent liquid phase of isosorbide-ethylene oxide 10 mol adduct was obtained by the same method as in Preparation Example A1 except that the secondary addition amount of ethylene oxide was changed from 132 g to 352 g.
[0119] Preparation Example A3: Preparation of 5 mole adduct of isosorbide-propylene oxide
[0120] The same method as Preparation Example A1 was used, except that propylene oxide was used instead of ethylene oxide as the addition reaction raw material, specifically, 116 g of propylene oxide was first added instead of 88 g of ethylene oxide being added once, and 174 g of propylene oxide was added a second time instead of 132 g of ethylene oxide being added a second time, thereby obtaining 423 g of a transparent liquid isosorbide-propylene oxide 5 mol adduct.
[0121] Preparation Example A4: Preparation of 10 mol of isosorbide-propylene oxide adduct
[0122] Propylene oxide is used as the addition reaction raw material instead of ethylene oxide. Specifically, the same method as Preparation Example A1 is used, except that 116 g of propylene oxide is first added instead of 88 g of ethylene oxide, and 465 g of propylene oxide is added a second time instead of 132 g of ethylene oxide, to obtain 698 g of a transparent liquid phase isosorbide-propylene oxide 10 mol adduct.
[0123] <Preparation of (meth)acrylic acid modified polyurethane>
[0124] Preparation Example B1: Using isosorbide-ethylene oxide 5 mol adduct as polyol and polyisocyanate as polyisocyanate isophorone diisocyanate (IPDI), 2-hydroxyethyl methacrylate as hydroxyalkyl (meth)acrylate (Meth)acrylic acid modified polyurethane
[0125] 222g of isophorone diisocyanate (IPDI) and 0.1g of dibutyltin dilaurate (DBTDL) as a reaction catalyst were placed in a three-necked glass reactor equipped with a stirrer and mixed at room temperature, and 183g of the isosorbide-ethylene oxide 5 mole adduct obtained in Preparation Example A1 was slowly added to carry out a crosslinking reaction. After the addition of the isosorbide-ethylene oxide 5 mole adduct was completed, 65g of 2-hydroxyethyl methacrylate was slowly added thereto after stirring at 50°C for 1 hour for aging to carry out an acrylic acid modification reaction. After the addition of 2-hydroxyethyl methacrylate was completed, after stirring at 50°C for 1 hour for aging, the reaction product was cooled to room temperature to obtain 467g of the (meth) acrylic acid modified polyurethane of the following chemical formula A.
[0126] [Chemical formula A]
[0127]
[0128] Preparation Example B2: Using isosorbide-ethylene oxide 10 mol adduct as polyol and polyisocyanate as polyisocyanate Hexamethylene diisocyanate (HDI), 2-hydroxyethyl acrylate as hydroxyalkyl (meth)acrylate to prepare (meth)acrylate Acrylic modified polyurethane
[0129] The same method as Preparation Example B1 was used, except that 168 g of hexamethylene diisocyanate (HDI) was used instead of isophorone diisocyanate (IPDI) as the polyisocyanate, 293 g of the isosorbide-ethylene oxide 10 mol adduct obtained in Preparation Example A2 was used as the polyol instead of the isosorbide-ethylene oxide 5 mol adduct obtained in Preparation Example A1, and 58 g of 2-hydroxyethyl acrylate was used instead of 2-hydroxyethyl methacrylate as the hydroxyalkyl (meth)acrylate, thereby obtaining 515 g of a (meth)acrylic modified polyurethane of the following Chemical Formula B.
[0130] [Chemical formula B]
[0131]
[0132] Preparation Example B3: Using 5 mol of isosorbide-propylene oxide adduct as a polyol and 5 mol of isosorbide-propylene oxide adduct as a polyisocyanate Methylene diphenyl diisocyanate (MDI), 2-hydroxyethyl methacrylate as hydroxyalkyl (meth)acrylate Preparation of (meth)acrylic acid modified polyurethane
[0133] The same method as Preparation Example B1 was used, except that 250 g of methylene diphenyl diisocyanate (MDI) was used as the polyisocyanate instead of isophorone diisocyanate (IPDI), and 218 g of the isosorbide-propylene oxide 5 mol adduct obtained in Preparation Example A3 was used as the polyol instead of the isosorbide-ethylene oxide 5 mol adduct obtained in Preparation Example A1, thereby obtaining 529 g of a (meth)acrylic modified polyurethane of the following chemical formula C.
[0134] [Chemical formula C]
[0135]
[0136] Preparation Example B4: Using 10 mol of isosorbide-propylene oxide adduct as a polyol and 10 mol of isosorbide-propylene oxide adduct as a polyisocyanate isophorone diisocyanate (IPDI), 2-hydroxyethyl methacrylate as hydroxyalkyl (meth)acrylate (Meth)acrylic acid modified polyurethane
[0137] The same method as Preparation Example B1 was used, except that 363 g of the isosorbide-propylene oxide 10 mol adduct obtained in Preparation Example A4 was used instead of the isosorbide-ethylene oxide 5 mol adduct obtained in Preparation Example A1 as the polyol, to obtain 643 g of a (meth)acrylic modified polyurethane of the following Chemical Formula D.
[0138] [Chemical formula D]
[0139]
[0140] Preparation Example B5: Using isosorbide as the polyol and isophorone diisocyanate as the polyisocyanate (IPDI), 2-hydroxyethyl methacrylate as hydroxyalkyl (meth)acrylate to prepare (meth)acrylic acid modified polyurethane ester
[0141] 431 g of a (meth)acrylic modified polyurethane of the following Chemical Formula E was obtained by the same method as Preparation Example B1 except that 146 g of isosorbide was used as the polyol instead of the isosorbide-ethylene oxide 5 mol adduct obtained in Preparation Example A1.
[0142] [Chemical formula E]
[0143]
[0144] Preparation Example B6: Using polyethylene glycol (number average molecular weight: 500 g / mol) as a polyol,
[0145] Isophorone diisocyanate (IPDI) as a polyisocyanate, methacrylate as a hydroxyalkyl (meth)acrylate Preparation of (meth)acrylic acid modified polyurethane with 2-hydroxyethyl acrylate
[0146] 782 g of a (meth)acrylic modified polyurethane of the following Chemical Formula F was obtained by the same method as Preparation Example B1 except that 500 g of polyethylene glycol (number average molecular weight: 500 g / mol) was used as the polyol instead of the isosorbide-ethylene oxide 5 mol adduct obtained in Preparation Example A1.
[0147] [Chemical formula F]
[0148]
[0149] Preparation Example B7: Using polypropylene glycol (number average molecular weight: 500 g / mol) as a polyol,
[0150] Hexamethylene diisocyanate (HDI) as a polyisocyanate, acrylate as a hydroxyalkyl (meth)acrylate Preparation of (meth)acrylic acid modified polyurethane with 2-hydroxyethyl acrylate
[0151] The same method as in Preparation Example B1 was used, except that 168 g of hexamethylene diisocyanate (HDI) was used instead of isophorone diisocyanate (IPDI) as the polyisocyanate, 500 g of polypropylene glycol (number average molecular weight: 500 g / mol, manufactured by Kumho Petrochemical (manufactured)) was used instead of the isosorbide-ethylene oxide 5 mol adduct obtained in Preparation Example A1 as the polyol, and 58 g of 2-hydroxyethyl acrylate was used instead of 2-hydroxyethyl methacrylate as the hydroxyalkyl (meth)acrylate, thereby obtaining 720 g of a (meth)acrylic modified polyurethane of the following Chemical Formula G.
[0152] [Chemical formula G]
[0153]
[0154] Preparation Example B8: Using polybutylene glycol (number average molecular weight: 1000 g / mol) as the polyol and polyisocyanate as the Methylene diphenyl diisocyanate (MDI) as an ester, 2-hydroxyethyl methacrylate as a hydroxyalkyl (meth)acrylate To prepare (meth) acrylic acid modified polyurethane
[0155] The same method as Preparation Example B1 was used, except that 250 g of methylene diphenyl diisocyanate (MDI) was used as the polyisocyanate instead of isophorone diisocyanate (IPDI), and 1000 g of polytetramethylene glycol (number average molecular weight: 1000 g / mol, manufactured by Aldrich Corporation) was used as the polyol instead of the isosorbide-ethylene oxide 5 mol adduct obtained in Preparation Example A1, thereby obtaining 1308 g of a (meth)acrylic modified polyurethane of the following Chemical Formula H.
[0156] [Chemical formula H]
[0157]
[0158] <Preparation of Oil-Resistant Coating Composition for Metal>
[0159] Examples A1 to A4 and Comparative Examples A1 to Comparative Example A14: Standard preparation method
[0160] According to the weight ratio described in Table 1 below, (meth)acrylic acid modified polyurethane, (meth)acrylic acid monomer, epoxy resin, epoxy curing accelerator and thermal polymerization initiator were added to a mixing reactor controlled at 60° C. or less, and they were mixed while stirring at a temperature of 60° C. or less to prepare a liquid oil-resistant coating composition for metal. At this time, the total content of (meth)acrylic acid modified polyurethane, (meth)acrylic acid monomer, epoxy resin, epoxy curing accelerator and thermal polymerization initiator was 100 parts by weight in total.
[0161] <Ingredients>
[0162] (1) (Meth) acrylic modified polyurethane (acrylic modified PU)
[0163] - Preparation Example B1: (Meth)acrylic acid-modified polyurethane of formula A obtained in Preparation Example B1
[0164] - Preparation Example B2: (Meth)acrylic acid-modified polyurethane of formula B obtained in Preparation Example B2
[0165] - Preparation Example B3: (Meth)acrylic acid-modified polyurethane of Chemical Formula C obtained in Preparation Example B3
[0166] - Preparation Example B4: (Meth)acrylic acid-modified polyurethane of Chemical Formula D obtained in Preparation Example B4
[0167] - Preparation Example B5: (Meth)acrylic acid-modified polyurethane of Formula E obtained in Preparation Example B5
[0168] - Preparation Example B6: (Meth)acrylic acid-modified polyurethane of Formula F obtained in Preparation Example B6
[0169] - Preparation Example B7: (Meth)acrylic acid-modified polyurethane of Chemical Formula G obtained in Preparation Example B7
[0170] - Preparation Example B8: (Meth)acrylic acid-modified polyurethane of Chemical Formula H obtained in Preparation Example B8
[0171] (2) (Meth) acrylic acid monomer
[0172] -2-HEMA: 2-Hydroxyethyl methacrylate (Samchun Pure Chemical (manufactured))
[0173] -4-HBA: 4-Hydroxybutyl acrylate (Samchun Pure Chemical (manufactured))
[0174] -BA: Butyl acrylate (Samchun Pure Chemical (manufactured))
[0175] -PETTA: Pentaerythritol tetraacrylate (manufactured by Miwon Commercial)
[0176] -P-2M: 2-methacryloyloxyethyl acid phosphate (manufactured by Kyoei Chemical Co., Ltd.)
[0177] -BDDA: 1,4-Butanediol diacrylate (manufactured by Aldrich Corporation)
[0178] (3) Epoxy resin
[0179] -YD-128: Bisphenol A type epoxy resin (manufactured by Kukdo Chemical)
[0180] -YDF-170: Bisphenol F type epoxy resin (manufactured by Kukdo Chemical)
[0181] -1,4-BDGE: 1,4-Butanediol diglycidyl ether (manufactured by Kukdo Chemical)
[0182] (4) Epoxy curing accelerator
[0183] -DICY: Dicyandiamide (Evonik Corporation ((Manufactured))
[0184] -UR2T: 1,1'-(4-methyl-m-phenylene)bis(3,3-dimethylurea) (manufactured by Evonik)
[0185] (5) Thermal polymerization initiator
[0186] -V-65: 2,2'-azobis(2,4-dimethylvaleronitrile) (Fuji Film Corporation (manufactured))
[0187] -V-40: 1,1'-azobis(cyclohexane-1-carbonitrile) (manufactured by Fujifilm Corporation)
[0188] - Peroyl TCP: Bis(4-tert-butylcyclohexyl)peroxydicarbonate (Nichiyu Corporation (manufactured))
[0189] [Table 1]
[0190]
[0191] [Table 1] (Continued)
[0192]
[0193]
[0194] [Table 1] (Continued)
[0195]
[0196] <Evaluation of Physical Properties of Oil-Resistant Coating Composition for Metal>
[0197] The oil-resistant metal coating composition prepared in Examples A1 to A4 and Comparative Examples A1 to A14 was coated on two surfaces of a rolled steel plate cut into a size of 2.5 cm x 12 cm in an area of 2.5 cm x 2.0 cm, respectively, and then the two coated portions of the rolled steel plate were overlapped and fixed, and then heated and cured at 150° C. for 5 minutes to manufacture metal bonding samples. The adhesion and oil resistance of each sample were evaluated by the following physical property measurement method, and the results are shown in Table 2 below.
[0198] <Measurement Methods of Physical Properties>
[0199] (1) Adhesion
[0200] In order to evaluate the adhesion of the metal coating composition to the metal, the shear strength (Lap shear strength) (MPa) of each metal bonding sample was measured using UTM (Instron 5967 product, Instron Corporation (manufactured)). Specifically, for each metal bonding sample, the shear strength was measured 5 times in total, and then the average value was calculated. The higher the shear strength, the better the adhesion.
[0201] (2) Oil resistance
[0202] The metal bonded samples were immersed in mineral oil (manufactured by Daejung Chemical) and heated at 190°C for 200 hours, and then the shear strength of each metal bonded sample immersed by the above-mentioned (1) adhesion measurement method was measured 5 times, and the average value thereof was calculated. Thereafter, the reduction rate (%) of the shear strength after immersion relative to the shear strength before immersion of each metal bonded sample was calculated. The lower the reduction rate of the shear strength, the more excellent the oil resistance.
[0203] Reduction rate of shear strength (%) = (shear strength before immersion - shear strength after immersion) × 100 / shear strength before immersion
[0204] [Table 2]
[0205]
[0206] As shown in Table 2, in the case of the metal bonding samples of Examples A1 to A4 to which the coating composition comprising the (meth)acrylic modified polyurethane according to the present invention is applied, the shear strength is 16 MPa or more, the adhesion to the metal is excellent, and after immersion in mineral oil at 190° C. for 200 hours, the shear strength reduction rate is less than 30%, thereby maintaining excellent adhesion, and the oil resistance is also excellent.
[0207] However, in the case of the metal bonding samples of Comparative Examples A1 and A2, the adhesion is poor. In addition, in the case of the metal bonding samples of Comparative Examples A3 and A4, the shear strength is significantly reduced after immersion in high-temperature mineral oil, and the oil resistance is poor. In addition, in the case of the metal bonding sample of Comparative Example A5, both the adhesion and oil resistance are poor, and in the case of the metal bonding sample of Comparative Example A6, the adhesion is poor. In addition, in the case of the metal bonding sample of Comparative Example A7, the adhesion is very poor, and in the case of the metal bonding sample of Comparative Example A8, the oil resistance is very poor, and the natural peeling of the metal bonding sample is observed after immersion in mineral oil and heating. In addition, in the case of the metal bonding samples of Comparative Examples A9 and A10, the adhesion is poor. In addition, in the case of the metal bonding samples of Comparative Examples A11 and A13, the curing of the metal coating composition cannot be performed, so the adhesion and oil resistance cannot be evaluated, and in the case of the metal bonding samples of Comparative Examples A12 and A14, the adhesion and oil resistance are poor.
[0208] As described above, in the case of a metal coating composition containing the (meth)acrylic modified polyurethane according to the present invention in a specific content range, the metal adhesion is excellent while maintaining good adhesion in high temperature oil, and thus has excellent oil resistance.
Claims
1. A coating composition for metal, comprising, based on 100 parts by weight of the composition in total: 5.1-64.9 parts by weight of (meth)acrylic acid modified polyurethane; 7.1-74.9 parts by weight of (meth)acrylic acid monomer; 2.1-44.9 parts by weight of epoxy resin; 0.051-2.49 parts by weight of an epoxy curing accelerator; and 0.00051-2.49 parts by weight of a thermal polymerization initiator, the (meth)acrylic modified polyurethane comprising: i) a polymerization unit derived from an anhydrosugar alcohol-alkylene oxide adduct; ii) a polymerization unit derived from a polyisocyanate; and iii) a polymerization unit derived from a hydroxyalkyl (meth)acrylate.
2. The metal coating composition according to claim 1, wherein The anhydrosugar alcohol-alkylene oxide adduct is obtained by reacting hydroxyl groups at both ends or one end of anhydrosugar alcohol with alkylene oxide, wherein the alkylene oxide is a linear alkylene oxide having 2 to 8 carbon atoms or a branched alkylene oxide having 3 to 8 carbon atoms.
3. The metal coating composition according to claim 2, wherein The anhydrosugar alcohol is isosorbide, isomannide, isoidide or a mixture thereof.
4. The metal coating composition according to claim 1, wherein The polyisocyanate is methylene diphenyl diisocyanate (MDI), toluene diisocyanate (TDI), hexamethylene diisocyanate (HDI), isophorone diisocyanate (IPDI) or a combination thereof.
5. The metal coating composition according to claim 1, wherein The hydroxyalkyl (meth)acrylate is a hydroxy-C1-8 alkyl (meth)acrylate.
6. The metal coating composition according to claim 1, wherein The (meth)acrylic acid modified polyurethane is represented by the following chemical formula 2: [Chemical formula 2] In the chemical formula 2, R1 is each independently an alkylene group, R2 is each independently an alkylene group, a cycloalkylene group or an arylene group, R3 is each independently an alkylene group, R4 is each independently a hydrogen atom or an alkyl group, M is a divalent organic group derived from anhydrosugar alcohol, m and n each independently represent an integer from 0 to 15, and m+n represents an integer from 1 to 30.
7. The metal coating composition according to claim 1, wherein The (meth)acrylic modified polyurethane is prepared by a method comprising: reacting an anhydrosugar alcohol-alkylene oxide adduct and polyisocyanate to prepare an intermediate having an isocyanate group terminal; and reacting the intermediate with a hydroxyalkyl (meth)acrylate.
8. The metal coating composition according to claim 1, wherein The (meth)acrylic acid monomer is a monomer having 1 to 4 (meth)acrylic acid groups in the molecule.
9. The metal coating composition according to claim 1, wherein The epoxy resin is a resin having two or more epoxy groups in a molecule.
10. The metal coating composition according to claim 1, wherein The thermal polymerization initiator is selected from the compound represented by the following Chemical Formula 3-1, the compound represented by the following Chemical Formula 3-2, or a mixture thereof: [Chemical formula 3-1] In the chemical formula 3-1, R and R' are each independently a C2-C8 straight chain alkyl or a C3-C8 branched chain alkyl; a C3-C20 cycloalkyl; a C6-C20 aryl; or a C2-C8 straight chain methoxy-alkyl or a C3-C8 branched chain methoxy-alkyl, and X is -CN or -CO2R", wherein R" is a C2-C8 straight chain alkyl or a C3-C8 branched chain alkyl; a C3-C20 cycloalkyl; or a C6-C20 aryl; [Chemical formula 3-2] In the chemical formula 3-2, each R is independently a C2-C8 straight-chain alkyl group or a C3-C8 branched-chain alkyl group; a C3-C20 cycloalkyl group; or a C6-C20 aryl group.
11. A method for preparing a coating composition for metal, comprising the following steps: Based on 100 parts by weight of the mixture, 5.1-64.9 parts by weight of (meth)acrylic acid-modified polyurethane; 7.1-74.9 parts by weight of (meth)acrylic acid monomer; 2.1-44.9 parts by weight of epoxy resin; 0.051-2.49 parts by weight of an epoxy curing accelerator; and 0.00051-2.49 parts by weight of a thermal polymerization initiator are mixed, wherein the (meth)acrylic modified polyurethane comprises: i) a polymerization unit derived from an anhydrosugar alcohol-alkylene oxide adduct; ii) a polymerization unit derived from a polyisocyanate; and iii) a polymerization unit derived from a hydroxyalkyl (meth)acrylate.
12. The method for preparing a coating composition for metal according to claim 11, wherein: The mixing of the (meth)acrylic modified polyurethane, the (meth)acrylic monomer, the epoxy resin, the epoxy curing accelerator and the thermal polymerization initiator is carried out at a temperature below 60°C.
13. A coated metal article comprising: Metal objects; And a coating of the metal coating composition according to any one of claims 1 to 10 on the surface of the metal article.