A Sm 3+ Preparation method and regulation of ion-doped reversible photochromic cadmium glass

Through Sm3+ ion doped reversible photochromic cadmium-based glass, ultraviolet light and laser technology can realize lossless reading and writing and multi-dimensional storage of information, solving the shortcomings of existing optical storage glasses in information reading and writing capabilities and storage capacity. Reduces costs and improves mechanical properties.

CN116891340BActive Publication Date: 2024-11-22KUNMING UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310853150.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-12
Publication Date
2024-11-22
Estimated Expiration
2043-07-12

AI Technical Summary

Technical Problem

The existing optical storage glass has insufficient information reading and writing capabilities and storage capacity, and traditional methods require power supply and cooling systems, which are costly.

Method used

Reversible photochromic cadmium-based glass with Sm3+ ion doping is used to induce rare earth ion doping through ultraviolet light radiation, and write information using laser induction technology, and erase and read information through blue laser bleaching, which improves the The storage capacity and reading and writing capabilities of information.

Benefits of technology

Lossless readout and multi-dimensional optical information are realized, which expands optical storage capacity, reduces costs, and does not require power supply and cooling systems, which improves the mechanical properties of glass.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116891340B_ABST
    Figure CN116891340B_ABST
Patent Text Reader

Abstract

The present invention provides a Sm 3+ The preparation method and regulation of ion-doped reversible photochromic cadmium glass are characterized in that the raw materials are composed of the following molar percentages: CdO: 50-65%; SiO2: 5-30%; B2O3: 5-25%; R2CO3: 0-10%; PbO: 3-10%; Sb2O3: 0-5%; Sm2O3: 0.05-1%, 15g of the above raw materials are weighed, ground and mixed evenly, kept warm at a temperature of 1300-1450°C for 20-40min, poured into a stainless steel mold preheated to 300-400°C, and then annealed at a temperature of 480°C for 2-5 hours. The adjustable luminescent photochromic glass provided by the present invention has high mechanical strength, transparency and wear resistance, can quickly respond to light sources in the ultraviolet band to achieve color change, and can bleach the color-changing glass by blue laser irradiation. And the rare earth ion Sm 3+ The doping can reversibly regulate the luminescence intensity based on the color-changing effect, which can be used to broaden the application of this optical glass in light storage.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of photon glass and particularly relates to a Sm 3+ Ion-doped reversible photochromic cadmium glass, preparation method thereof, and optical storage application thereof. Technical Background

[0002] Photochromic glass is a transparent glass that absorbs light in the visible light region, causing a decrease in transmittance or a change in color when exposed to ultraviolet or visible light. Photochromic glass can automatically adjust transmittance or color as needed and has a wide range of applications, including in the fields of architecture, automobiles, electronic equipment, and optical storage devices.

[0003] In recent years, with the explosive growth of information, it is urgent to develop new storage media. Optical storage glass is a high-density optical storage medium that can be used for long-term data storage, data backup and data archiving. Compared with traditional magnetic disks and optical disks, optical storage glass has higher storage density, longer life and better stability. It can store a large amount of data while ensuring the security and reliability of the data. At the same time, combined with photoluminescent optical storage glass, the written data can be read out losslessly through a fixed light source. Combined with the high chemical stability of inorganic glass, the written data can be repeatedly erased and read and reused. And optical storage glass does not require power and cooling system, which can save costs. Summary of the invention

[0004] In order to solve the problems existing in the above-mentioned prior art, the present invention provides a Sm 3+ Ion-doped reversible photochromic cadmium glass and its preparation method and application, wherein the photochromic glass uses light field control and laser-induced coloring in the glass to write information into the glass in a dimensional manner, thereby increasing the storage capacity of the information. While the information can be reversibly written, lossless reading can be achieved by regulating the luminescence intensity of rare earth ions, which is beneficial to storage applications in practice.

[0005] In order to solve the above technical problems and achieve the above technical effects, the present invention is a photochromic luminescent glass induced by ultraviolet radiation and doped with rare earth ions, which is realized by the following technical scheme, characterized in that it comprises raw material compositions in the following proportions: CdO: 50-65%, SiO2: 5-30%, B2O3: 5-25%, R2CO3: 0-10%, PbO: 3-10%, Sb2O3: 0-5%, Sm2O3: 0.05-1%.

[0006] Another object of the present invention is to provide a method for preparing ultraviolet irradiation-induced rare earth ion-doped photochromic luminescent glass, which specifically comprises the following steps:

[0007] S1: Weigh the raw materials according to the following components: CdO: 50-65%, SiO2: 5-30%, B2O3: 5-25%, R2CO3: 0-10%, PbO: 3-10%, Sb2O3: 0-5%, Sm2O3: 0.05-1%; mix the raw materials in an agate mortar and grind and mix them evenly;

[0008] S2: putting the mixed raw materials in S1 into a box furnace at a temperature of 1300-1450°C for 20-40 minutes, pouring the glass liquid onto a copper plate preheated to 300-400°C to obtain a precursor glass;

[0009] S3: placing the glass in an annealing furnace at 480°C for 2-5 hours to remove the thermal stress in the glass and keep the glass in good mechanical properties, thereby obtaining ultraviolet laser-induced rare earth ion-doped photochromic glass;

[0010] S4: grinding and polishing of glass;

[0011] S5: UV laser induced glass discoloration and pattern writing, read out in dark conditions using 405 nm light, and photobleaching of the glass by blue laser.

[0012] The beneficial effects of the present invention are:

[0013] A method for preparing photochromic luminescent glass with simple process and low cost is provided, and the glass can be used for optical storage. The UV-induced brown color-changing glass produces an obvious color-changing effect after being irradiated by sunlight or UV light for a certain period of time, from extremely transparent colorless to brown, indicating that the laser-induced glass coloring technology is applied to the field of optical storage. The laser-induced coloring in the blue 473nm laser bleached glass indicates that the stored information can be rewritten and erased.

[0014] The present invention prepares a photochromic glass, which can induce glass coloring through ultraviolet light, write information using ultraviolet laser, and erase information through blue laser. Compared with traditional glass, the information reading and writing ability is stronger and the optical storage capacity is larger. At the same time, the entire glass material uses transparent glass as the storage medium, and multi-dimensional optical information can be written, further expanding the optical storage capacity. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] The accompanying drawings are used to illustrate the specific embodiments of the present experiment and constitute a part of the application, but do not constitute a limitation of the embodiments of the present invention.

[0016] Figure 1 The glass prepared by the present invention has a UV laser power of 0.47W / cm 2 Below, a photograph of discolored glass after saturated irradiation;

[0017] Figure 2 The glass prepared by the present invention is prepared at a laser power of 0.47W / cm 2 Photo of glass after irradiation for 3 minutes, and glass bleached to its initial state by 473nm blue laser;

[0018] Figure 3 The glass of the present invention has a laser power of 1.53W / cm 2 , photos of patterns written by 365nm UV laser;

[0019] Figure 4 It is a comparative description of the transmittance of the glass of the present invention before and after ultraviolet laser irradiation, and the transmittance difference can reach up to 60%;

[0020] Figure 5 The comparative description is of the photoluminescence spectrum of the glass of the present invention before and after ultraviolet laser irradiation under the excitation of 405nm light, and the luminescence controllable rate can reach up to 67%.

[0021] Specific implementation cases

[0022] The content of the present invention is further described below in conjunction with specific embodiments and drawings, but the present invention is not limited to the following embodiments.

[0023] Example 1

[0024] A UV-induced brown color-changing luminescent controllable glass and a preparation method thereof, as follows:

[0025] S1: Design glass composition, by molar percentage, CdO: 62%, SiO2: 12%, B2O3: 15%, Li2CO3: 5%, PbO: 5%, Sb2O3: 0.5%, Sm2O3: 0.5%, weigh 15g into an agate mortar, grind for 10 minutes until the mixture is uniform, move the glass powder into a high-temperature box furnace at 1400℃, keep it warm for 30 minutes, and obtain precursor glass;

[0026] S2: Move the glass to 480℃ and keep it warm for 2 hours, mainly to remove the thermal stress in the glass and keep the glass in good mechanical properties;

[0027] S3: Control the UV laser power density to 1.53W / cm 2 By controlling the irradiation time, the glass shows a gradient change in the degree of coloring.

[0028] The transparent glass prepared in Example 1 was 2 After irradiating the glass for 3 minutes, the following pictures are obtained: Figure 1As shown, the irradiated glass exhibited obvious photochromic phenomenon. Using a computer program, laser-induced coloring was used, indicating that optical information can be written into the glass by laser.

[0029] Example 2

[0030] A UV-induced brown color-changing luminescent controllable glass and a preparation method thereof, as follows:

[0031] S1: Design the glass composition, by molar percentage, CdO: 65%, SiO2: 4.7%, B2O3: 18%, K2CO3: 8%, PbO: 4%, Sm2O3: 0.3%. Weigh 15g into an agate mortar, grind for 10 minutes until the mixture is evenly mixed, move the glass powder into a high-temperature box furnace at 1400℃, keep it warm for 30 minutes, and obtain the precursor glass;

[0032] S2: Move the glass to 450℃ and keep it warm for 2 hours, mainly to remove the thermal stress in the glass and keep the glass in good mechanical properties;

[0033] S3: Use ultraviolet laser to irradiate the glass, and after irradiation for 3 minutes, the glass will produce a significant color change effect, and then use 473nm blue light for photobleaching. The bleaching time is different, so that the colored glass gradually fades.

[0034] In this embodiment 2, the glass was first irradiated with ultraviolet laser for 3 minutes, and then completely photobleached with 473nm laser. Figure 2 As shown, the tinted brown glass can be bleached, further illustrating that optical information can be written into the glass using the photochromic effect and then erased using photobleaching so that the information can be rewritten.

[0035] Example 3

[0036] A UV-induced brown color-changing luminescent controllable glass and a preparation method thereof, as follows:

[0037] S1: Design the glass composition, by molar percentage, CdO: 60%, SiO2: 12.4%, B2O3: 15%, Na2CO3: 5%, PbO: 5%, Sb2O3: 2%, Sm2O3: 0.6%. Weigh 15g into an agate mortar, grind for 10 minutes until the mixture is evenly mixed, move the glass powder into a high-temperature box furnace at 1400℃, keep it warm for 30 minutes, and obtain the precursor glass;

[0038] S2: Move the glass to 480℃ and keep it warm for 2 hours, mainly to remove the thermal stress in the glass and keep the glass in good mechanical properties;

[0039] S3: The glass was irradiated with ultraviolet light. After saturated irradiation for 3 minutes, the transmittance spectrum of the glass before and after irradiation with 365 nm light was measured using a spectrophotometer (U-4100) equipped with an integrating sphere, and the luminescence spectrum of the glass before and after irradiation with 365 nm light was measured using a fluorescence spectrometer (F-7000) with a high-performance monochromator.

[0040] In this embodiment 3, ultraviolet light was first used to irradiate the glass for five minutes, and the transmittance spectrum of the glass before and after irradiation with 365nm ultraviolet light was measured using a spectrophotometer (U-4100) equipped with an integrating sphere. Figure 4 As shown in the figure, the transmittance spectrum of the glass after laser irradiation is within the range of 380nm-1600nm. After laser irradiation, the transmittance spectrum of the glass within the range of 380nm-1000nm decreases, which further illustrates that ultraviolet light can induce coloring of transparent glass. The glass was irradiated with ultraviolet light for five minutes, and the luminescence spectrum of the glass before and after 365nm light irradiation was measured by a fluorescence spectrometer (F-7000) with a high-performance monochromator. Figure 5 As shown in the figure, after laser irradiation, under the excitation of 405nm wavelength light, Sm 3+ The decrease in the luminescence spectrum in all visible light bands further illustrates the controllability of rare earth ion luminescence.

[0041] The glasses prepared in Examples 1-3 of the present invention have a sintering temperature of 1400°C and a heat treatment temperature of 480°C to remove thermal stress in the glasses. All glasses have high mechanical strength, and the brown color change of the glasses is induced by ultraviolet laser or ultraviolet light, and the colored glasses are bleached by blue laser, and non-destructive reading is performed using 405nm light.

[0042] Multi-dimensional optical information writing can be achieved in glass by focusing laser, and photobleaching can erase the optical information stored in the glass. The above implementation cases demonstrate the excellent optical information storage performance of laser-induced photochromic glass.

[0043] In summary, the present invention prepares a rare earth ion doped photochromic glass, which can induce glass coloring through ultraviolet light irradiation, write information using laser, and erase information through photobleaching treatment, and realize lossless reading of information through photoluminescence. Compared with traditional glass, the information reading and writing ability is stronger and the optical storage capacity is larger. At the same time, the entire glass material uses transparent glass as the storage medium, and multi-dimensional optical information can be written, further expanding the optical storage capacity.

[0044] Although the main inventive examples that affect the factors of this experiment have been described and listed, ordinary persons in the art can understand that various changes, explorations, modifications and combinations can be made to the embodiments without departing from the principles and purpose of the invention, and the scope of the invention is defined by the claims and their equivalents.

Claims

1. A Sm 3+ Ion-doped reversible photochromic cadmium glass, It is characterized in that Includes raw materials in the following proportions Composition: CdO: 62%, SiO 2 :12%, B 2 O 3 :15%,Li 2 CO 3 :5%,PbO:5%,Sb 2 O 3 :0.5%, Sm 2 O 3 : 0.5%, the sum of the molar percentages of all raw materials is 100%.

2. A Sm 3+ Ion-doped reversible photochromic cadmium glass, It is characterized in that The raw material composition includes the following proportions: CdO: 65%, SiO 2 :4.7%, B 2 O 3 :18%, K 2 CO 3 :8%,PbO:4%,Sm 2 O 3 : 0.3%, the sum of the molar percentages of all raw materials is 100%.

3. A Sm 3+ Ion-doped reversible photochromic cadmium glass, It is characterized in that Includes raw materials in the following proportions Composition: CdO: 60%, SiO 2 :12.4%, B 2 O 3 :15%,Na 2 CO 3 :5%,PbO:5%,Sb 2 O 3 :2%, Sm 2 O 3 : 0.6%, the sum of the molar percentages of all raw materials is 100%.

4. The method for preparing the reversible photochromic cadmium glass according to claim 1, It is characterized in that The specific steps include: S1: Weigh the raw materials according to the following composition: CdO: 62%, SiO 2 :12%, B 2 O 3 :15%,Li 2 CO 3 :5%,PbO:5%,Sb 2 O 3 :0.5%, Sm 2 O 3 : 0.5%, the sum of the molar percentages of all raw materials is 100%; mix the raw materials in an agate mortar, grind and mix evenly; S2: placing the mixed raw materials in S1 into a high-temperature box furnace at a temperature of 1400°C for 30 minutes, pouring the glass liquid onto a copper plate preheated to 300-400°C to obtain a precursor glass; S3: Place the glass in an annealing furnace at 480°C for 2 hours to remove thermal stress in the glass and keep the glass in good mechanical properties; S4: grinding and polishing of glass; S5: UV laser induced glass discoloration and pattern writing, read out in dark conditions using 405 nm light, and photobleaching of the glass by blue laser.

5. The method for preparing the reversible photochromic cadmium glass according to claim 2, It is characterized in that The specific steps include: S1: Weigh the raw materials according to the following composition: CdO: 65%, SiO 2 :4.7%, B 2 O 3 :18%, K 2 CO 3 :8%,PbO:4%,Sm 2 O 3 : 0.3%, the sum of the molar percentages of all raw materials is 100%; mix the raw materials in an agate mortar and grind and mix them evenly; S2: placing the mixed raw materials in S1 into a high-temperature box furnace at a temperature of 1400°C for 30 minutes, pouring the glass liquid onto a copper plate preheated to 300-400°C to obtain a precursor glass; S3: Place the glass in an annealing furnace at 450°C for 2 hours to remove thermal stress in the glass and keep the glass in good mechanical properties; S4: grinding and polishing of glass; S5: UV laser induced glass discoloration and pattern writing, read out in dark conditions using 405 nm light, and photobleaching of the glass by blue laser.

6. The method for preparing the reversible photochromic cadmium glass according to claim 3, It is characterized in that The specific steps include: S1: Weigh the raw materials according to the following composition: CdO: 60%, SiO 2 :12.4%, B 2 O 3 :15%,Na 2 CO 3 :5%,PbO:5%,Sb 2 O 3 :2%, Sm 2 O 3 : 0.6%, the sum of the molar percentages of all raw materials is 100%; mix the raw materials in an agate mortar and grind and mix them evenly; S2: placing the mixed raw materials in S1 into a high-temperature box furnace at a temperature of 1400°C for 30 minutes, pouring the glass liquid onto a copper plate preheated to 300-400°C to obtain a precursor glass; S3: Place the glass in an annealing furnace at 480°C for 2 hours to remove thermal stress in the glass and keep the glass in good mechanical properties; S4: grinding and polishing of glass; S5: UV laser induced glass discoloration and pattern writing, read out in dark conditions using 405 nm light, and photobleaching of the glass by blue laser.

7. Sm according to any one of claims 1 to 3 3+ Application of ion-doped reversible photochromic cadmium glass in the field of optical storage technology.