A metal catalyst and its preparation method and application

The MOF framework structure is retained in the MNP/MOF catalyst through controlled pyrolysis technology, which solves the problems of poor catalytic effect and high preparation cost, achieves efficient catalytic performance and cost control, and is suitable for the hydrogenation reaction of organic compounds.

CN116899570BActive Publication Date: 2024-10-29CHONGQING TECH & BUSINESS UNIV
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202310717303.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-16
Publication Date
2024-10-29
Estimated Expiration
2043-06-16

AI Technical Summary

Technical Problem

Existing MNP/MOF catalyst preparation methods have problems such as poor catalytic effect, high preparation costs, and strict requirements on raw materials. In particular, high-temperature calcination causes the collapse of MOF pore channels and framework structures, hindering the contact between reactants and metal sites, and the solution impregnation method and chemical vapor deposition methods require volatile metal precursors, are complex to operate and are not universal.

Method used

The MOF framework structure is partially decomposed through controlled pyrolysis technology to generate the MNPs active center in the porous nanostructure, and the active center is stabilized in the residual MOF framework, using nickel salts and cobalt salts with organic ligands in a solvent. Hydrothermal reaction is used to prepare NixCoy-MOF precursor, and pyrolysis is performed in an H2 or N2 atmosphere. The pyrolysis temperature and time are controlled to retain the MOF framework structure.

Benefits of technology

It achieves high-efficiency catalytic effects of metal catalysts, improves the conversion rate of reactants, reduces preparation costs, and does not rely on precious metals, so it has good industrial prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116899570B_ABST
    Figure CN116899570B_ABST
Patent Text Reader

Abstract

The present invention provides a metal catalyst and a preparation method and application thereof. The catalyst is composed of a general structural formula: Ni x Co y ‑MOF precursor pyrolysis; wherein 0≤x≤2, 0≤y≤2, and x and y are not 0 at the same time; MOF represents an organic metal framework. The present invention partially decomposes the MOF framework structure through controlled pyrolysis, so that the porous nanostructure of MOF is partially retained, thereby generating MNPs active centers in the porous MOF, and the residual MOF framework can ensure the stability of the active center, thereby producing a good catalytic effect, which can be used for catalytic hydrogenation of unsaturated bonds of organic compounds such as benzene, toluene, olefins, alkynes, aldehydes, ketones, esters, and catalytic hydrogenation of carbon dioxide.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of catalysts, and in particular to a metal catalyst and a preparation method and application thereof. Background Art

[0002] Metal-organic frameworks (MOFs) have high surface area and structural diversity, and have important application value in catalysis, gas storage / separation, drug delivery and chemical sensing. Studying the synergistic effect between metal nanoparticles (MNPs) and MOFs is of great significance in catalysis. If MNPs and MOFs can be reasonably coordinated, the MNP / MOF composite material may not only have a large specific surface area and pore volume, but also have the advantages of adjustable composition and morphology, thereby greatly improving its catalytic performance.

[0003] At present, the methods for preparing MNP / MOF include solvothermal method, solid grinding method, solution impregnation method, chemical vapor deposition method and self-template method. Pyrolysis is a simple and effective way to expose the metal active sites of MNP / MOF materials. However, the direct high-temperature calcination (above 400°C) of MOF-derived nanomaterials reported so far causes the complete decomposition of MOF at high temperature, causing the collapse of the pores and framework structure inside MOF, so that a large number of active metal sites are embedded in the bulk phase, hindering the contact between the reactants and the metal sites. Therefore, the catalytic effect of the catalyst obtained by this method is general and difficult to promote. The solid grinding method is a method in which a volatile organic metal precursor is ground, sublimated, evaporated and diffused into the MOF cavity, and then the organic metal precursor embedded in the MOF is reduced to form an MNP / MOF composite material. The solid grinding method is simple to operate, can avoid excess solvent, and can achieve complete loading of the introduced precursor. However, it has high requirements for the metal precursor, and the loaded metal precursor needs to be volatile. Therefore, this method is expensive and not universal. The solution impregnation method uses capillary pressure to infiltrate a solution containing a metal precursor into the internal cavity of the MOF, and then reduces the metal precursor to MNP. This method also has the advantage of simple operation, but the problem is that it is difficult to evenly distribute MNPs inside and outside the MOF pores, and the MNPs adsorbed on the surface are prone to migration. These problems result in the catalytic effect of the obtained catalyst being average, and also limit the application of this method. The chemical vapor deposition method diffuses a volatile metal precursor into the desolvated MOF pores under vacuum conditions at a certain temperature. This method does not require solvents to prepare MNP / MOF and can load a large amount of MNPs, but it also requires the organic metal precursor to be highly volatile at room temperature or to be easily sublimated at elevated temperatures. Summary of the invention

[0004] In view of the problems of poor catalytic effect, high preparation cost, and strict requirements on raw materials in the existing MNP / MOF and its preparation method, the present invention provides a metal catalyst and its preparation method and application. The technical concept of partially decomposing the MOF framework structure through controlled pyrolysis allows the porous nanostructure of MOF to be partially retained, thereby generating MNPs active centers in the porous MOF, and the residual MOF framework can ensure the stability of the active center, thereby producing a good catalytic effect.

[0005] To achieve the above object, the technical solution of the present invention is:

[0006] In a first aspect, the present invention provides a metal catalyst, wherein the catalyst is a metal catalyst having a general structural formula: Ni x Co y -MOF is obtained by thermal decomposition of a precursor; wherein 0≤x≤2, 0≤y≤2, and x and y are not 0 at the same time; MOF represents metal organic framework.

[0007] Preferably, the precursor is pyrolyzed in a H2 atmosphere or a N2 atmosphere to obtain the metal catalyst; further preferably, the pyrolysis temperature in the H2 atmosphere is 300 to 350°C, preferably 320 to 330°C; the pyrolysis time is 1 to 2 hours;

[0008] Further preferably, the pyrolysis temperature in N2 atmosphere is 300-600°C, preferably 450-500°C; the pyrolysis time is 1-2h.

[0009] Preferably, the method for preparing the precursor comprises: subjecting nickel salt and / or cobalt salt, an organic ligand and an alkaline regulator to a hydrothermal reaction in a solvent.

[0010] Preferably, the nickel salt is selected from: at least one of nickel nitrate, nickel acetate, nickel sulfate, nickel chloride, and nickel bromide; the cobalt salt is selected from: at least one of cobalt nitrate, cobalt acetate, cobalt chloride, cobalt bromide, and cobalt sulfate; the organic ligand is selected from: at least one of terephthalic acid, 1,3,5-benzenetricarboxylic acid, 2,5-dihydroxyterephthalic acid, 2,5-thiophenedicarboxylic acid, formic acid, and pyridine carboxylic acid; the alkaline regulator is selected from: at least one of triethylenediamine hexahydrate, sodium hydroxide, potassium hydroxide, triethylamine, triethanolamine, and polyvinylpyrrolidone; the solvent is selected from: at least one of DMF, methanol, ethanol, and deionized water.

[0011] Preferably, in the preparation method of the precursor, the molar ratio of nickel salt to cobalt salt is 0-2:0-2; the molar amount of the organic ligand is 0.9-1.1 of the sum of the molar amount of nickel in the nickel salt and the molar amount of cobalt in the cobalt salt; the amount of the alkaline regulator is 0.5-2.0 of the sum of the molar amount of nickel in the nickel salt and the molar amount of cobalt in the cobalt salt.

[0012] Preferably, in the method for preparing the precursor, the hydrothermal reaction temperature is 110 to 150° C., preferably 125 to 135° C.; the hydrothermal reaction time is 12 to 48 hours, preferably 20 to 30 hours.

[0013] Preferably, the preparation method of the precursor also includes: separating the solid product of the hydrothermal reaction, washing and drying; further preferably, after separation, the solid product of the hydrothermal reaction is washed multiple times with DMF, and then washed multiple times with ethanol; further preferably, the washed solid is vacuum dried at 60-80°C for more than 8h.

[0014] Preferably, the preparation method comprises: subjecting nickel salt and / or cobalt salt, organic ligand and alkaline regulator to a hydrothermal reaction in a solvent to obtain a metal precursor, and then subjecting the metal precursor to a pyrolysis reaction to obtain the metal catalyst.

[0015] In a second aspect, the present invention provides a metal precursor for synthesizing the above-mentioned metal catalyst, wherein the metal precursor has a general structural formula: NixCoy-MOF; wherein 0≤x≤2, 0≤y≤2, and x and y are not 0 at the same time; MOF represents an organic metal framework.

[0016] The third aspect is the use of the above-mentioned metal catalyst or the above-mentioned metal precursor in the catalytic hydrogenation reaction of unsaturated bonds in organic compounds.

[0017] The beneficial effects of the present invention are as follows:

[0018] The present invention prepares a metal catalyst with a MOF framework structure, uses nickel salt and cobalt salt as metal ions, selects suitable organic ligands, and regulates the content and distribution of metal species in the MOF structure to regulate the microstructure of the prepared MNP / MOF material, thereby ultimately achieving the purpose of regulating the microstructure of the metal catalyst after pyrolysis. Compared with traditional metals, the metal catalyst prepared by the present invention has a nano-scale porous MOF structure residual from pyrolysis with easily accessible active sites, and its framework structure can enrich the concentration of reactants near the active MNPs site, thereby improving the conversion rate of the reactants, and can be used for catalytic hydrogenation of unsaturated bonds of organic compounds such as benzene, toluene, alkene, alkyne, aldehyde, ketone, ester, and catalytic hydrogenation of carbon dioxide. In addition, the metal catalyst of the present invention does not contain precious metals, the preparation method is simple, the conditions are not harsh, the cost is controllable to a certain extent, and it has a good industrialization prospect. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 For you x Co y -TG analysis chart of MOF.

[0020] Figure 2FTIR analysis diagrams of NixCoy-MOF precursor and metal catalyst, where (a) is the FTIR analysis diagram of NixCoy-MOFs; (b) is the FTIR analysis diagram of the catalyst obtained by decomposing NixCoy-MOFs at 325°C; (c) is the FTIR analysis diagram of the catalyst obtained by decomposing Ni1Co2-MOFs at different decomposition temperatures (300°C, 325°C, 350°C).

[0021] Figure 3 Figure 2 is the XRD spectrum of NixCoy-MOF precursor and metal catalyst, where (a) is the XRD analysis diagram of NixCoy-MOFs; (b) is the XRD analysis diagram of the catalyst obtained by decomposing NixCoy-MOFs at 325°C; (c) is the local (43.6°~45.6°) XRD analysis diagram of the catalyst obtained by decomposing different NixCoy-MOFs at 325°C; (d) is the XRD analysis diagram of the catalyst obtained by Ni1Co2-MOFs at different decomposition temperatures (300°C, 325°C, 350°C).

[0022] Figure 4 N2 adsorption-desorption isotherms of metal catalysts.

[0023] Figure 5 Scanning electron microscopy (SEM) analysis of NixCoy-MOFs and metal catalysts, where the catalysts corresponding to figures a to j are Ni-MOF, Ni2Co1-MOF, Ni1Co1-MOF, Ni1Co2-MOF, Co-MOF, Ni / MOF-325, Ni2Co1 / MOF-325, Ni1Co1 / MOF-325, Ni1Co2 / MOF-325, and Co / MOF-325, respectively.

[0024] Figure 6 are XPS spectra of metal catalysts, wherein (a) shows the XPS spectra of Ni 2p in various metal catalysts; (b) shows the XPS spectra of Co 2p in various metal catalysts.

[0025] Figure 7 It is the H2-TPD curve of the metal catalyst in the range of 60 to 210°C.

[0026] Figure 8The catalytic activity and stability analysis diagrams of metal catalysts, wherein (a) shows the conversion rate of toluene hydrogenation catalyzed by the catalysts obtained by pyrolysis of NixCoy-MOF precursor in nitrogen at different temperatures; (b) shows the conversion rate of toluene hydrogenation catalyzed by the catalysts obtained by pyrolysis of NixCoy-MOF precursor in hydrogen at 325°C; (c) shows the conversion rate of toluene hydrogenation catalyzed by the catalysts obtained by pyrolysis of Ni1Co2 / MOF at different temperatures; (d) shows the stability of different metal catalysts at 160°C.

[0027] Fig. 9 This is the conversion curve of benzene hydrogenation catalyzed by metal catalyst Ni / MOF-300 with temperature.

[0028] Note: NixCoy-MOF-325 indicates the metal catalyst obtained by pyrolysis of NixCoy-MOF at 325 °C. DETAILED DESCRIPTION

[0029] In the description of the present invention, it should be noted that, if the specific conditions are not specified in the examples, the experiments were carried out according to conventional conditions or the conditions recommended by the manufacturer. The reagents or instruments used, if the manufacturer is not specified, are all conventional products that can be purchased commercially.

[0030] The present invention provides a metal catalyst, wherein the catalyst has a general structural formula: Ni x Co y -MOF is obtained by thermal decomposition of its precursor; wherein 0≤x≤2, 0≤y≤2, x and y can both be 0, 1, 2, but x and y cannot be 0 at the same time; MOF stands for metal organic framework.

[0031] In a preferred embodiment of the present invention, the method for preparing the precursor comprises: subjecting nickel salt and / or cobalt salt, an organic ligand, and an alkaline regulator to a hydrothermal reaction in a solvent.

[0032] In the present invention, the nickel salt is preferably selected from at least one of nickel nitrate, nickel acetate, nickel sulfate, nickel chloride, and nickel bromide; the cobalt salt is selected from at least one of cobalt nitrate, cobalt acetate, cobalt chloride, cobalt bromide, and cobalt sulfate; the organic ligand is selected from at least one of terephthalic acid, 1,3,5-benzenetricarboxylic acid, 2,5-dihydroxyterephthalic acid, 2,5-thiophenedicarboxylic acid, formic acid, and pyridinecarboxylic acid. These organic ligands can provide a stable MOF skeleton structure for the metal catalyst of the present invention, and terephthalic acid is preferably used in the present invention.

[0033] In the present invention, the alkaline regulator is preferably selected from at least one of triethylenediamine hexahydrate, sodium hydroxide, potassium hydroxide, triethylamine, triethanolamine, and polyvinylpyrrolidone; preferably triethylenediamine hexahydrate. The alkaline regulator is added to improve the coordination ability of metal ions and ligands. It is currently found that the aforementioned several can be used in the present invention.

[0034] In the present invention, the solvent is preferably selected from at least one of DMF, methanol, ethanol and deionized water.

[0035] In a preferred embodiment of the present invention, in the preparation method of the precursor, the molar ratio of nickel salt to cobalt salt is 0-2:0-2; the molar amount of the organic ligand is 0.9-1.1 of the sum of the molar amount of nickel in the nickel salt and the molar amount of cobalt in the cobalt salt, and it is better to control it at around 1.0; the amount of the alkaline regulator is 0.5-2.0 of the sum of the molar amount of nickel in the nickel salt and the molar amount of cobalt in the cobalt salt, and it is preferably controlled at 0.5-1.0.

[0036] In a preferred embodiment of the present invention, in the method for preparing the precursor, the hydrothermal reaction temperature is 110-150°C, preferably 125-135°C; more preferably 130°C; the hydrothermal reaction time is 12-48h, preferably 20-30h, more preferably 24h.

[0037] Preferably, in the present invention, the method for preparing the precursor further comprises: separating the solid product of the hydrothermal reaction, washing and drying; preferably, after separation, the solid product of the hydrothermal reaction is first washed multiple times with DMF, and then washed multiple times with ethanol; preferably, the washed solid is vacuum dried at 60-80°C for more than 8h, preferably dried at 70±2°C for 24h.

[0038] The metal catalyst is applied to the catalytic hydrogenation reaction of unsaturated bonds of organic compounds. Taking the Ni1Co2 / MOF-325 catalyst derived from a Ni / Co molar ratio of 1 / 2 for catalytic hydrogenation of toluene as an example, it not only retains the excellent structure and large specific surface area similar to MOF, but also has more unoccupied d orbitals in the d energy band of Co in the Co-rich alloy catalyst, which improves the adsorption and activation ability of the catalyst for H2, makes the metal active components fully contact with the H2 molecules, and is conducive to improving its toluene hydrogenation activity and reaction stability.

[0039] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments.

[0040] Example 1

[0041] 1.1 The preparation method of the metal catalyst is as follows:

[0042] Accurately weigh Ni(NO3)2·6H2O, Co(NO3)2·6H2O (mass see Table 1), 0.700g terephthalic acid (0.0042mol) and 0.464g (0.0021mol) triethylenediamine hexahydrate and dissolve in 50mL N,N-dimethylformamide (DMF), ultrasonically vibrate for 10min, magnetically stir for 20min, transfer the stirred solution to a 100mL polyethylene hydrothermal autoclave and seal it, and keep it at 130℃ for 24.0h. After natural cooling, the product was washed twice with DMF and twice with ethanol, centrifuged at 4000rpm for 7min each time, and vacuum dried at 70℃ overnight. The obtained crystalline powder is Ni x Co y -MOF precursors are recorded as Ni-MOF, Ni2Co1-MOF, Ni1Co1-MOF, Ni1Co2-MOF and Co-MOF according to the Ni / Co molar ratio. After pyrolysis in H2 atmosphere at 325°C for 1h, the metal catalysts Ni / MOF-325, Ni2Co1 / MOF-325, Ni1Co1 / MOF-325, Ni1Co2 / MOF-325 and Co / MOF-325 of the present invention are obtained.

[0043] Table 1 Ni(NO3)2·6H2O and Co(NO3)2·6H2O with different Ni / Co molar ratios

[0044]

[0045] 1.2 Characterization of catalysts

[0046] 1.2.1 Thermogravimetric analysis (TG)

[0047] The catalyst precursor was subjected to thermogravimetric analysis (TG) using a STA4493F3 synchronous thermal analyzer (Netzsch Instrument Manufacturing Co., Ltd., Germany). The test atmosphere was nitrogen, the temperature range was 25-900°C, and the heating rate was 10°C / min.

[0048] 1.2.2 X-ray diffraction (XRD)

[0049] The X-ray diffraction (XRD) of the sample was tested on XRD-6100 (Shimadzu Corporation, Japan). The ray tube was a 2.2kW Cu target, a Kα ray source, a tube voltage of 40kV, a current of 30mA, a scanning step of 0.02°, a scanning rate of 4° / min, and a scanning range of 5 to 80°.

[0050] 1.2.3 Specific surface area and pore size distribution test (BET)

[0051] The specific surface area and pore structure of the samples were measured using an ASAP2020HD88 fully automatic specific surface and micropore adsorption instrument (BET, Micromeritics, Inc., USA). Before the BET measurement, the accurately weighed samples were vacuum degassed at 150 °C for 3.0 h in a nitrogen flow and then tested at liquid nitrogen temperature (-196 °C).

[0052] 1.2.4 Fourier Transform Infrared Spectroscopy (FTIR)

[0053] The functional group composition of the samples was tested and analyzed by IRPrestige-21 Fourier transform infrared spectrometer (FTIR, Hitachi, Japan). KBr was used as the test background and the test wave number range was 500-4000cm –1 .

[0054] 1.2.5H2-TPR

[0055] A fully automatic chemisorption instrument (Belcat-II, Japan Microchem Belcat Co., Ltd.) was used for H2-programmed temperature reduction (H2-TPR). 50 mg of the catalyst precursor was weighed and placed in a quartz tube. ℃ The temperature was raised from room temperature to the set temperature at a heating rate of / min, and the hydrogen consumption was detected by a thermal conductivity detector (TCD).

[0056] 1.2.6H2 Temperature Programmed Desorption (H2-TPD)

[0057] A fully automatic chemisorption instrument (Belcat-II, Japan Microchem Belcat Co., Ltd.) was used for H2 temperature programmed desorption (H2-TPD) test. 50 mg of the precursor was weighed and transferred into a quartz tube. It was first pyrolyzed at 325 °C in a H2 atmosphere for 1.0 h, and then cooled to 50 °C in a He atmosphere. ℃ , then 6% H2 / Ar mixed gas was introduced into the catalyst bed for 30 min, and then He gas was purged at this temperature to remove physically adsorbed H2 molecules. ℃ / min from 50 ℃ When the temperature is raised to the set temperature, the hydrogen desorption amount of the sample is obtained by TCD detection.

[0058] 1.2.7 Scanning Electron Microscope (SEM)

[0059] The morphological characteristics of the samples were characterized using a SU1510 scanning electron microscope (SEM) (Hitachi, Japan) with an operating voltage of 15 kV.

[0060] 1.2.8 X-ray Photoelectron Spectroscopy (XPS)

[0061] The X-ray photoelectron spectroscopy (XPS) of Ni 2p and Co 2p was measured on an X-ray photoelectron spectrometer (Thermo Scientific K-Alpha, Thermo Fisher Scientific, USA), and all binding energy calibrations were based on the C1s peak at 284.8 eV. The operating voltage was 12 kV, the filament current was 6 mA, and Al Kα was used as the excitation source (hν = 1486.6 eV).

[0062] 1.3 Evaluation of catalytic activity of metal catalysts

[0063] The toluene hydrogenation reaction was carried out in a fixed bed reactor. Weigh 50 mg of Ni prepared in step 1.1 x Co y -MOF precursor sample was placed in the middle of the quartz tube reactor, and then the quartz reaction tube was fixed in a tube furnace. In the flowing H2 of 20mL / min, the temperature was raised to the pyrolysis temperature of the catalyst at a rate of 10℃ / min, and maintained at this temperature for 1.0h. After the pyrolysis was completed, when the temperature dropped to 80℃, the obtained metal catalyst was then subjected to in-situ hydrogenation reaction: the raw gas composed of toluene and H2 was introduced into the reactor at 20mL / min, and the toluene hydrogenation activity on the catalyst was evaluated in the range of 80-200℃. The reaction products were analyzed online using a gas chromatograph equipped with FID.

[0064] 2 Results and discussion

[0065] 2.1TG analysis

[0066] The thermal decomposition behaviors of Ni-MOF, Ni2Co1-MOF, Ni1Co1-MOF, Ni1Co2-MOF and Co-MOF in nitrogen atmosphere were investigated using a synchronous thermal analyzer.

[0067] Depend on Figure 1 It can be seen that Ni x Co yThe thermal degradation of -MOF in nitrogen atmosphere mainly includes three temperature stages: (1) When the temperature is 25-370℃, each precursor has a small mass loss, which is attributed to the release of solvent DMF molecules and absorbed water molecules encapsulated in the skeleton, as well as the decomposition of some MOFs skeleton structures; (2) When the temperature is 370-500℃, there is a significant mass loss in this stage, which is caused by the large-scale decomposition of ligands in MOFs; (3) When the temperature is 500-800℃, Ni-MOF, Ni1Co1-MOF, Ni1Co2-MOF and Ni2Co1-MOF all have a small mass loss, while the mass of Co-MOF increases slightly, which may be because in this temperature range, Co-MOF further decomposes and releases a large amount of gas phase products, resulting in a sudden increase in local pressure. The above results show that the pyrolysis temperature range of Ni-MOF, Ni2Co1-MOF, Ni1Co1-MOF, Ni1Co2-MOF and Co-MOF in an inert atmosphere is 370-500°C, and the MOFs skeleton structure will be completely decomposed at a temperature above 500°C. Therefore, controlled pyrolysis in nitrogen at 370-500°C may partially decompose the structure of MOFs, thereby retaining part of the MOFs framework structure.

[0068] 2.2 FTIR study

[0069] We used FTIR analysis to study the Ni x Co y - Functional groups of MOF precursors and catalysts.

[0070] Figure 2 (a) Ni with different Ni / Co molar ratios x Co y - FTIR spectrum of MOF precursor, located at 3603cm -1 and 3430cm -1 The band at is assigned to Ni x Co y -OH in the MOF precursor, which is caused by the coordinated water in MOFs, indicating that water molecules exist in Ni x Co y -MOF structure. 2927, 1502, 815 and 753 cm -1 The peak at 1572cm is the characteristic peak of the para-aromatic CH stretching band. -1 and 1383cm -1 The strong bands at – ) shows asymmetric and symmetric stretching modes, indicating that the -COO – Through the bidentate ligand mode with Ni 2+ and Co 2+Coordination (coordination between metal ions and linker molecules is successful). In addition, at 608cm -1 and 698cm -1 The peak at is attributed to the characteristic peak of Ni-O or Co-O, indicating that Ni or Co atoms react with -COO of terephthalic acid. – The metal oxygen bond was successfully formed. Therefore, Ni and Co species have been successfully introduced into the framework of MOFs to form Ni x Co y -MOF structure.

[0071] Figure 2 (b) Ni x Co y Ni-MOF was pyrolyzed at 325℃ under H2 flow for 1.0h x Co y FTIR spectrum of / MOF-325 catalyst. Compared with Ni / MOF, Ni2Co1 / MOF, and Ni1Co1 / MOF (2(a)), Figure 2 In (b), the characteristic peaks of the MOFs structure on Ni / MOF-325, Ni2Co1 / MOF-325, and Ni1Co1 / MOF-325 catalysts almost disappeared, significantly weakened, or even disappeared, indicating that the MOFs framework structure in Ni / MOF-325 and Ni2Co1 / MOF-325 catalysts has been decomposed under H2 flow at 325°C. Similarly, compared with the Ni1Co1 / MOF precursor, the characteristic peaks of the MOFs structure on the Ni1Co1 / MOF-325 catalyst were significantly weakened, indicating that its MOFs framework structure was destroyed. In addition, the FTIR spectra of Co / MOF-325 and Ni1Co2 / MOF-325 are similar to those of Co / MOF and Ni1Co2 / MOF precursors, indicating that the Co / MOF-325 and Ni1Co2 / MOF-325 catalysts have well retained the MOFs framework structure.

[0072] Figure 2 (c) is the FTIR spectra of the catalysts obtained after Ni1Co2-MOF was treated at different pyrolysis temperatures. Compared with Ni1Co2 / MOF-300 and Ni1Co2 / MOF-325, the characteristic peaks of the MOFs structure on Ni1Co2 / MOF-350 almost disappeared, indicating that its MOFs framework structure was seriously disintegrated, while the MOFs framework structure of Ni1Co2 / MOF-300 and Ni1Co2 / MOF-325 was relatively intact. Therefore, the pyrolysis temperature is also one of the important factors affecting the MOFs framework structure of the catalyst.

[0073] 2.3 XRD study

[0074] Figure 3(a) is the XRD spectra of Ni-MOF, Ni2Co1-MOF, Ni1Co1-MOF, Ni1Co2-MOF and Co-MOF. They have similar XRD crystal phase diffraction peaks because their lattice constants and crystal structures are similar, indicating that Ni and Co metal ions have almost no effect on the crystal structure of synthesized MOFs. Among them, the diffraction peak of Co-MOF is weak, indicating that the crystallinity of the corresponding phase is poor, which may be because Co atoms promote the growth of MOF materials in amorphous form.

[0075] Figure 3 (b) is the XRD spectra of Ni / MOF-325, Ni2Co1 / MOF-325, Ni1Co1 / MOF-325, Ni1Co2 / MOF-325 and Co / MOF-325 catalysts obtained by pyrolysis of the above MOFs materials at 325℃ and H2 flow for 1.0h. No characteristic diffraction peaks of Ni / MOF and Ni2Co1 / MOF were observed in the spectra of Ni / MOF-325 and Ni2Co1 / MOF-325, indicating that Ni / MOF and Ni2Co1 / MOF were completely decomposed under 325℃ and H2 flow. Compared with Ni1Co1-MOF, the intensity of MOFs characteristic diffraction peaks in Ni1Co1 / MOF-325 was significantly reduced, while Ni1Co2 / MOF-325 basically maintained the MOF characteristic diffraction peak intensity consistent with Ni1Co2-MOF. This indicates that Ni1Co2 / MOF-325, after pyrolysis of Ni1Co2-MOF at 325°C under H2 flow, maintains the framework structure of MOFs materials well, further indicating that the introduction of Co into Ni-based MOFs to form NiCo-based MOFs materials can enhance their high temperature resistance in H2 atmosphere. Figure 3 In (b), it can be clearly observed that the Ni / MOF-325 catalyst has diffraction peaks at 2θ = 44.5°, 51.8°, and 76.4°, which are respectively attributed to the {111}, {200}, and {220} crystal planes of face-centered cubic metal Ni. These are Ni NPs generated by the complete decomposition of Ni / MOF. The Ni2Co1 / MOF-325, Ni1Co1 / MOF-325, and Ni1Co2 / MOF-325 catalysts also have diffraction peaks at 2θ = 44.4°, 51.6°, and 76.2°, as shown in Figure 2. Figure 3 (c) Figure 3(b) Local enlarged view), respectively, {111}, {200}, {220} crystal planes of face-centered cubic Ni-Co alloy. Among the five samples, the XRD spectrum of Ni / MOF-325 shows sharp metallic Ni diffraction peaks, indicating high crystallinity of metallic Ni, which explains that the pyrolysis of Ni / MOF in H2 atmosphere at 325℃ causes the MOFs structure to collapse sharply and form huge Ni agglomerates. The metal particle sizes in Ni / MOF-325, Ni2Co1 / MOF-325, Ni1Co1 / MOF-325 and Ni1Co2 / MOF-325 are calculated from the half-peak width of the {111} diffraction peak by the Scherrer equation: 25.5, 15.2, 12.3 and 10.2nm, respectively. Obviously, the introduction of Co into Ni-based MOFs significantly reduces the metal particle size of the catalyst after pyrolysis, which is attributed to the stronger high temperature resistance of Co-MOF in H2 atmosphere (see the activity test section), preventing the decomposition of the MOF framework structure and the aggregation of metal species during high-temperature pyrolysis, and improving the dispersion of metal particles produced by pyrolysis in the MOFs carrier.

[0076] Figure 3 (d) shows the XRD spectra of Ni1Co2 / MOF-300, Ni1Co2 / MOF-325 and Ni1Co2 / MOF-350 catalysts obtained by pyrolysis of Ni1Co2-MOF at different temperatures (300, 325 and 350°C). In the figure, the MOFs characteristic peak intensity of Ni1Co2 / MOF-300 is significantly stronger than that of Ni1Co2 / MOF-325, while the characteristic diffraction peak of Ni1Co2 / MOF is not observed in Ni1Co2 / MOF-350, indicating that only a small amount of MOF structure may be decomposed under 300°C and H2 flow, so the generated Ni-Co alloy nanoparticles are small; while under 350°C and H2 flow, due to the high pyrolysis temperature, the MOFs framework structure is completely decomposed, resulting in the aggregation of metal species and the disappearance of the characteristic diffraction peaks of MOFs. In particular, the XRD pattern of the Ni1Co2 / MOF-325 catalyst has diffraction peaks of both MOFs and Ni-Co alloys, indicating that the controllable pyrolysis path allows the Ni1Co2 / MOF-325 catalyst to retain the MOF framework structure well, and at the same time, a large number of well-dispersed Ni-Co alloy nanoparticles (NiCo NPs) are formed in Ni1Co2 / MOF, which helps to improve its catalytic hydrogenation performance. Therefore, the appropriate pyrolysis temperature has an important influence on the phase structure of Ni-Co alloy catalysts derived from NiCo-based MOFs.

[0077] 2.4BET ​​Research

[0078] The specific surface area and pore structure of MOFs-derived catalysts Ni / MOF-325, Ni2Co1 / MOF-325, Ni1Co1 / MOF-325, Ni1Co2 / MOF-325 and Co / MOF-325 were studied using BET technology. Figure 4 As shown. Among them, Figure 4 The N2 adsorption-desorption isotherms of these catalysts are shown in Figure 2. The relative pressure range is 0.0-1.0 (P / P0) and the adsorption amount range is 0-400 (cm 3 / g STP).

[0079] like Figure 4 As shown in the figure, in the relative pressure range of 0.7 to 1.0P / P0, all isotherms show typical IV type curves with H3 type hysteresis loops, indicating the presence of mesoporous structures in these samples. The specific surface areas of Ni / MOF-325, Ni2Co1 / MOF-325, Ni1Co1 / MOF-325, Ni1Co2 / MOF-325 and Co / MOF-325 are 4.67, 5.12, 9.67, 46.55 and 23.64 m 2 / g, that is, the order of specific surface area is: Ni1Co2 / MOF-325>Co / MOF-325>Ni1Co1 / MOF-325>Ni2Co1 / MOF-325>Ni / MOF-325. This shows that at a pyrolysis temperature of 325°C, the molar ratio of Ni to Co in the catalyst has a greater influence on its specific surface area. When Ni / Co is 1 / 2, the specific surface area of ​​the corresponding Ni1Co2 / MOF-325 catalyst reaches the maximum value. The specific surface areas of Ni2Co1 / MOF-325 and Ni / MOF-325 are relatively small, which may be due to the serious decomposition of their MOF framework structures during the pyrolysis process.

[0080] Calculation of Ni using the Barrett-Joyner-Halenda (BJH) method x Co y The average pore size and total pore volume data of Ni / MOF-325 catalysts are shown in Table 2. The total pore volumes of Ni / MOF-325, Ni2Co1 / MOF-325, Ni1Co1 / MOF-325, Ni1Co2 / MOF-325, and Co / MOF-325 are 0.02, 0.01, 0.02, 0.26, and 0.17 cm, respectively. 3 / g, and the average pore sizes are 6.84, 6.83, 7.33, 22.66, and 28.61 nm, respectively. It can be seen that Ni1Co2 / MOF-325 not only has a high specific surface area, but also has a large total pore volume, which may be beneficial to improving its catalytic activity.

[0081] The BET analysis results in this section show that different Ni / Co molar ratios can adjust the specific surface area and nanopore structure of the metal catalyst.

[0082] Table 2Ni x Co y - Average pore size and total pore volume data of MOF-325

[0083]

[0084] 2.5 Scanning electron microscopy (SEM) analysis

[0085] Scanning electron microscopy was used to investigate the prepared MOFs and Ni x Co y The morphology of the MOF-325 catalyst was characterized. Figure 5 As shown in the figure, among the prepared MOFs, Ni-MOF, Ni2Co1-MOF, Ni1Co1-MOF and Ni1Co2-MOF ( Figure 5 a, b, c, d) are columnar structures with a wide size distribution, while Co-MOF ( Figure 5 In e), a block structure can be observed. Ni after H2 pyrolysis x Co y In the SEM of the / MOF-325 catalyst, it can be observed that Ni / MOF-325( Figure 5 f) and Ni2Co1 / MOF-325( Figure 5 The columnar structure of the catalyst in g) collapsed significantly, indicating that the MOFs skeleton structure was completely decomposed by H2 pyrolysis at 325℃. Ni1Co1 / MOF-325( Figure 5 h) and Ni1Co2 / MOF-325( Figure 5 The surface of the catalysts in (i) is much rougher than that of the corresponding MOFs, especially the Ni1Co2 / MOF-325 catalyst, which not only retains the framework structure of the MOF before pyrolysis, but also has obvious honeycomb pores on the surface, indicating that pyrolysis in hydrogen at 325°C can partially decompose the structure of Ni1Co2-MOF, thereby retaining part of the framework structure of MOFs while forming metal particles. In addition, Co / MOF-325( Figure 5 (j) Compared with its corresponding MOF, the catalyst surface showed neither structural collapse nor rough surface formation, which may indicate that only a small amount of Co-MOF can be decomposed in a hydrogen environment at 325°C.

[0086] 2.6XPS study

[0087] The prepared Ni x Co yThe surface composition and chemical state of Ni and Co in the / MOF-325 catalysts (Ni / MOF-325, Ni1Co1 / MOF-325, Ni2Co1 / MOF-325, Ni1Co2 / MOF-325 and Co / MOF-325) are shown in Figure 2. Figure 6 As shown, Figure 6 (a) and (b) are the XPS spectra of Ni 2p and Co 2p, respectively.

[0088] In the Ni 2p and Co 2p spectra, the 3 / 2 (856.2eV) and Ni 2p 1 / 2 (873.6eV) two main characteristic peaks and Co 2p 3 / 2 (781.5eV), Co 2p 1 / 2 (797.2eV), two main characteristic peaks can be observed at 862.2, 880.1eV and 787.8, 803.7eV respectively, which are attributed to Ni 2+ and Co 2+ The two main peaks of Ni 2p and Co 2p can be divided into three and two sub-peaks, respectively. 3 / 2 The three sub-peaks at electron binding energies of 852.9±0.9eV, 854.8±1.5eV, and 858.0±2.5eV and the Ni 2p 1 / 2 The three sub-peaks at the electron binding energies of 871.6±1.9eV, 873.5±1.4eV, and 876.3±2.2eV are respectively attributed to the Ni 0 、Ni 2+ 、Ni 3+ Species. Co 2p 3 / 2 The two sub-peaks at 780.5±0.9eV and 782.6±1.1eV and Co 2p 1 / 2 The two sub-peaks at 796.3±1.0eV and 798.2±1.0eV are respectively attributed to the Co 0 、Co 2+ Species.

[0089] Depend on Figure 6 It can be seen that there are a large number of oxidized species on the surfaces of these five catalysts, which may be oxidized substances produced by oxidation in the air after the catalyst is reduced. 0 The XPS peak intensity and peak area of ​​the species are the highest, and the Co 0The XPS peak intensity and peak area of ​​the species are low. This is because under the pyrolysis conditions of 325℃, the framework structure of Ni-MOF completely collapsed, exposing more Ni on its surface. 0 species; however, the structure of Co-MOF remains stable after pyrolysis at 325℃, resulting in 0 The species are less exposed, which is consistent with the analysis results of XRD.

[0090] For Ni1Co1 / MOF-325, Ni2Co1 / MOF-325 and Ni1Co2 / MOF-325, since Ni1Co2 / MOF-325 retains more MOF framework structure (see XRD research results), its surface Ni 0 and Co 0 The amount of species detected decreased, and the corresponding XPS peak intensity and peak area decreased; Ni in Ni1Co1 / MOF-325 and Ni2Co1 / MOF-325 0 and Co 0 The XPS peak area of ​​the species is large, which is attributed to the serious destruction of their MOFs framework structure. The Ni-Co alloy is embedded in the catalyst, but its crystallite size is large (see XRD research results), and Ni can still be detected on its surface. 0 and Co 0 The results show that the structure of the alloy catalyst prepared when the Ni / Co molar ratio is 1 / 1 and 2 / 1 is unstable, while it is relatively stable when the Ni / Co molar ratio is 1 / 2, which is beneficial to improve the catalytic hydrogenation performance of Ni1Co2 / MOF-325.

[0091] The above XPS results show that the Ni / Co molar ratio affects the composition of the precursor, which in turn affects the distribution of the Ni-Co alloy in the catalyst after pyrolysis, and further affects the catalytic activity.

[0092] 2.7H2-TPD research

[0093] The H2 adsorption and desorption performances of Ni / MOF-325, Ni2Co1 / MOF-325, Ni1Co1 / MOF-325, Ni1Co2 / MOF-325 and Co-MOF-325 catalysts were studied by H2-TPD. Figure 7 All catalysts formed a H2 desorption peak in the range of 60-210℃, which was attributed to the desorption of weakly chemically adsorbed H species on the catalyst surface. The reaction temperature of toluene hydrogenation in this work (80-200℃) was just within this desorption temperature range. Therefore, the desorbed H2 in this range provided the required active H species for the toluene hydrogenation reaction.

[0094] The H2-TPD desorption peak temperature on the catalyst can tell the strength of its H2 adsorption. The H2 desorption peak temperatures of Ni / MOF-325, Ni2Co1 / MOF-325, Ni1Co1 / MOF-325, Ni1Co2 / MOF-325 and Co / MOF-325 catalysts are 101℃, 89℃, 103℃, 121℃ and 107℃, respectively. Among them, the H2 desorption peak temperature of Ni1Co2-MOF-325 is significantly higher, indicating that it has a stronger H2 adsorption strength in this area. The area of ​​the H2-TPD desorption peak is positively correlated with the amount of H2 desorption. The order of the H2 desorption peak areas of the studied catalysts is: Ni1Co2 / MOF-325>Co / MOF-325>Ni1Co1 / MOF-325>Ni2Co1 / MOF-325≈Ni / MOF-325. Among them, the H2 desorption peak area of ​​Ni / MOF-325 and Ni2Co1 / MOF-325 is relatively small, which may be due to the complete decomposition of their MOFs framework structure (see FTIR and XRD analysis results). On the one hand, the complete decomposition of the MOFs framework structure leads to low specific surface area and pore volume of Ni / MOF-325 and Ni2Co1 / MOF-325 catalysts, which weakens the catalyst's ability to adsorb and activate H2. On the other hand, the decomposition of the MOFs structure forms larger metal agglomerates, which embeds the active metal sites in the bulk phase, which is not conducive to the contact between H2 and the active metal sites, thereby reducing the amount of H2 adsorption. Compared with Ni / MOF-325, Co / MOF-325 has a larger H2 desorption peak area, which is attributed to the surviving MOFs structure in the Co / MOF-325 catalyst. Among the catalysts studied, Ni1Co2 / MOF-325 has the largest H2 desorption peak area, mainly because the catalyst retains the framework structure of MOFs, which gives it a large surface area and pore volume, which is conducive to the adsorption and activation of H2. Secondly, the surviving MOFs structure improves the dispersion of metal particles produced by pyrolysis in the MOFs carrier, forming smaller nanometal particles, which are conducive to weak chemical adsorption of H on the metal surface.

[0095] 2.8 Catalyst activity and stability test

[0096] Under normal pressure and reaction temperature of 80-200°C, the gas phase toluene hydrogenation performance of Ni1Co2 / MOF-325, Ni1Co2 / MOF-400, Ni1Co2 / MOF-450, Ni1Co2 / MOF-500, Ni1Co2 / MOF-600 catalysts prepared by pyrolysis in nitrogen atmosphere and Ni / MOF-325, Ni2Co1 / MOF-325, Ni1Co2 / MOF-325, Ni1Co1 / MOF-325, Co / MOF-325 catalysts prepared by pyrolysis in hydrogen atmosphere were tested. The only product detected by toluene hydrogenation in the present invention is methylcyclohexane. The conversion rate of toluene of each catalyst changes with temperature as shown in the figure. Figure 8 (a) and 8(b). At the same time, the toluene hydrogenation activities of Ni1Co2 / MOF-N, Ni1Co2 / MOF-300, Ni1Co2 / MOF-325 and Ni1Co2 / MOF-350 catalysts prepared by pyrolysis in a hydrogen atmosphere were compared. Figure 8 In addition, the stability of Ni / MOF-325, Ni2Co1 / MOF-325, Ni1Co2 / MOF-325, Ni1Co1 / MOF-325 and Co / MOF-325 catalysts within 10.0 h were tested at 160 °C using toluene hydrogenation as a probe reaction. Figure 8 (d) as shown.

[0097] Depend on Figure 8 (a) It can be seen that the highest conversion rate of the catalysts obtained by pyrolysis in nitrogen is at a reaction temperature of 180°C, and the order of hydrogenation activity of each catalyst is: Ni1Co2 / MOF-500-N>Ni1Co2 / MOF-450-N>Ni1Co2 / MOF-600-N>Ni1Co2 / MOF-400-N>Ni1Co2 / MOF-325-N. Their highest conversion rates for toluene are all below 10.0%, which is far less than the hydrogenation activity of the catalysts obtained by pyrolysis in a hydrogen atmosphere. Therefore, hydrogen is selected as the pyrolysis and reduction gas flow for MNP-MOF in this paper.

[0098] like Figure 8As shown in (b), the toluene hydrogenation conversion rate on each catalyst shows a trend of increasing first and then decreasing with the increase of reaction temperature. In the high temperature region, their toluene conversion rates all decrease significantly, which may be related to the dehydrogenation of the generated methylcyclohexane at high temperature. The conversion rate of toluene hydrogenation on Co / MOF-325 catalyst is 0, the toluene hydrogenation conversion rate of Ni / MOF-325 catalyst is the highest at 180℃, which is 27.0%, while the toluene hydrogenation conversion rates of Ni2Co1 / MOF-325, Ni1Co2 / MOF-325 and Ni1Co1 / MOF-325 catalysts are the highest at 160℃, which are 81.3%, 95.7% and 87.3%, respectively. That is, the toluene conversion rate on each catalyst follows the rule: Ni1Co2 / MOF-325>Ni1Co1 / MOF-325>Ni2Co1 / MOF-325>Ni / MOF-325>Co / MOF-325. It shows that Ni1Co2 / MOF-325 catalyst has good toluene hydrogenation performance.

[0099] In order to verify that 325℃ is the optimal pyrolysis temperature, the toluene hydrogenation activities of Ni1Co2 / MOF-U, Ni1Co2 / MOF-300, Ni1Co2 / MOF-325 and Ni1Co2 / MOF-350 catalysts were compared. Figure 8 As shown in (c), the order of toluene hydrogenation activity of each catalyst within the reaction temperature range is: Ni1Co2 / MOF-325>Ni1Co2 / MOF-350>Ni1Co2 / MOF-300>Ni1Co2 / MOF-N. Among them, the conversion rate of toluene of Ni1Co2 / MOF-325 catalyst pyrolyzed at 325℃ is significantly higher than that of catalysts pyrolyzed at other temperatures within the reaction temperature range, indicating that the catalyst has excellent catalytic hydrogenation performance when the pyrolysis temperature is 325℃.

[0100] like Figure 8 As shown in (d), after each catalyst was reacted at 160℃ for 10.0h, the conversion rate of toluene on Co / MOF-325 was 0, and the extreme differences of the conversion rates of toluene for Ni1Co2 / MOF-325, Ni1Co1 / MOF-325, Ni2Co1 / MOF-325 and Ni / MOF-325 were 2.1%, 7.3%, 6.9% and 4.3%, respectively, that is, the stability order was: Ni1Co2 / MOF-325>Ni / MOF-325>Ni2Co1 / MOF-325>Ni1Co1 / MOF-325. Among them, Ni1Co2 / MOF-325 had better stability, which may be related to the structure of Ni-Co alloy on Ni1Co2 / MOF-325.

[0101] The structure and properties of the active components determine the hydrogenation performance of the catalyst. XRD, BET, FTIR, XPS and H2-TPD results show that both pyrolysis temperature and Ni / Co molar ratio can regulate the microstructure of the Ni-Co alloy, thereby improving the hydrogenation performance of the catalyst. On the one hand, taking Ni1Co2-MOF as the research object and keeping other conditions unchanged, when the pyrolysis temperature is 300℃, it is not enough to pyrolyze the MOF framework structure, lacks hydrogenation active sites, and its hydrogenation activity is relatively low; when the pyrolysis temperature is 350℃, it provides enough energy to completely decompose the MOF framework structure, and the Ni-Co alloy is exposed on the catalyst surface. The metal species on the catalyst surface are severely agglomerated, and the ability to adsorb and desorb H2 is weakened, thereby weakening its hydrogenation ability; 325℃ is its critical pyrolysis temperature. The Ni1Co2 / MOF-325 catalyst derived from pyrolysis at this temperature can not only retain most of the porous structure of MOF in Ni1Co2 / MOF for the dispersion of Ni-Co alloy and the adsorption of H2, but also expose a large number of Ni-Co alloy active sites. Therefore, the Ni1Co2 / MOF-325 catalyst exhibits excellent toluene hydrogenation activity. On the other hand, keeping the pyrolysis temperature at 325°C and other related conditions unchanged, when the Ni / Co molar ratio is 1 / 0 and 0 / 1, Ni / MOF-325 and Co / MOF-325 catalysts can be derived. Due to the collapse of the porous structure of Ni / MOF-325, the Co nanoparticles of Co / MOF-325 are wrapped in the amorphous structure and are not activated, resulting in insufficient hydrogenation activity, which is difficult to compare with the bimetallic Ni-Co alloy catalyst. When the Ni / Co molar ratio is 1 / 1, the derived Ni1Co1 / MOF-325 catalyst has a serious decomposition of the MOF framework structure compared to its precursor, providing fewer active sites for the Ni-Co alloy and reducing its stability. When the Ni / Co molar ratio is 2 / 1 When the Ni2Co1 / MOF-325 catalyst is prepared, the MOF framework structure is completely decomposed and collapsed, so that the Ni-Co alloy active components are embedded in the catalyst body phase, and the adsorption and desorption ability of H2 decreases accordingly, but its stability is slightly higher than that of the Ni1Co1 / MOF-325 catalyst; the Ni1Co2 / MOF-325 catalyst derived with a Ni / Co molar ratio of 1 / 2 not only retains the excellent structure similar to MOF and a large specific surface area, but also the Co-rich alloy catalyst has more unoccupied d orbitals in the d energy band of Co, which improves the catalyst's adsorption and activation ability for H2, allowing the Ni-Co alloy active components to fully contact with H2 molecules, which is beneficial to improving its toluene hydrogenation activity and reaction stability.

[0102] Example 2

[0103] The Ni / MOF prepared in Example 1 was pyrolyzed in a hydrogen atmosphere at 300°C for 1h (Ni / MOF-300) and further used for benzene hydrogenation investigation. The benzene hydrogenation reaction was carried out in a fixed bed reactor. Weigh 50 mg of the Ni-MOF precursor sample prepared in step 1.1 of Example 1 and place it in the middle of a quartz tube reactor. Then fix the quartz reaction tube in a tubular furnace. In a flowing H2 of 13.4 mL / min, heat the temperature to the pyrolysis temperature of the catalyst at a rate of 10°C / min and maintain it at this temperature for 1.0 h. After the pyrolysis is completed, when the temperature drops to 80°C, the obtained metal catalyst is subjected to an in-situ hydrogenation reaction: the raw gas consisting of benzene and H2 is introduced into the reactor at 13.4 mL / min, and the benzene hydrogenation activity on the catalyst is evaluated in the range of 80-200°C. The reaction products were analyzed online using a gas chromatograph equipped with an FID. The specific results are as follows: Fig. 9 As shown, the benzene hydrogenation conversion rate on the Ni / MOF-300 catalyst increases first and then decreases with the increase of reaction temperature. The decrease in the benzene hydrogenation conversion rate in the high temperature zone may be due to the further dehydrogenation of the generated cyclohexane into benzene. The results show that the metal catalyst of the present invention also has high hydrogenation activity for benzene, and the benzene conversion rate at 180°C reaches more than 80%.

[0104] In summary, the present invention prepares a metal catalyst with a MOF framework structure, the metal catalyst has a nano-scale porous MOF structure residual from pyrolysis, the MOF structure has accessible active sites, and its framework structure can enrich the concentration of reactants near the active MNPs sites, thereby improving the conversion rate of the reactants. The metal catalyst of the present invention can also be used for the catalytic hydrogenation of unsaturated bonds of organic compounds such as benzene, toluene, olefins, alkynes, aldehydes, ketones, esters, and the catalytic hydrogenation of carbon dioxide.

[0105] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A metal catalyst, characterized in that The catalyst is composed of the general structural formula: Ni x Co y -MOF is obtained by pyrolysis as a precursor; wherein 1≤x≤2, 1≤y≤2, MOF represents an organic metal framework; the precursor is pyrolyzed in a H2 atmosphere to obtain the metal catalyst; the pyrolysis temperature is 320~330℃; the pyrolysis time is 1~2h.

2. A metal catalyst according to claim 1, characterized in that: The preparation method of the precursor comprises: subjecting nickel salt, cobalt salt, organic ligand and alkaline regulator to hydrothermal reaction in a solvent.

3. A metal catalyst according to claim 2, characterized in that: The nickel salt is selected from at least one of nickel nitrate, nickel acetate, nickel sulfate, nickel chloride and nickel bromide; the cobalt salt is selected from at least one of cobalt nitrate, cobalt acetate, cobalt chloride, cobalt bromide and cobalt sulfate; the organic ligand is selected from at least one of terephthalic acid, 1,3,5-benzenetricarboxylic acid, 2,5-dihydroxyterephthalic acid, 2,5-thiophenedicarboxylic acid, formic acid and pyridine carboxylic acid; the alkaline regulator is selected from at least one of triethylenediamine hexahydrate, sodium hydroxide, potassium hydroxide, triethylamine, triethanolamine and polyvinylpyrrolidone; the solvent is selected from at least one of DMF, methanol, ethanol and deionized water.

4. A metal catalyst according to claim 2 or 3, characterized in that: In the preparation method of the precursor, the molar ratio of nickel salt to cobalt salt is 1-2:1-2; the molar amount of the organic ligand is 0.9-1.1 of the sum of the molar amount of nickel in the nickel salt and the molar amount of cobalt in the cobalt salt; and the amount of the alkaline regulator is 0.5-2.0 of the sum of the molar amount of nickel in the nickel salt and the molar amount of cobalt in the cobalt salt.

5. A metal catalyst according to claim 2, characterized in that: In the preparation method of the precursor, the hydrothermal reaction temperature is 110-150° C. and the hydrothermal reaction time is 12-48 hours.

6. A metal catalyst according to claim 5, characterized in that: The hydrothermal reaction temperature is 125~135°C; the hydrothermal reaction time is 20~30h.

7. A metal catalyst according to claim 2, characterized in that: The method for preparing the precursor further comprises: separating the solid product of the hydrothermal reaction, washing and drying it.

8. A metal catalyst according to claim 7, characterized in that: After separation, the solid product of the hydrothermal reaction is washed multiple times with DMF and then washed multiple times with ethanol.

9. A metal catalyst according to claim 8, characterized in that: The washed solid was vacuum dried at 60-80°C for more than 8 h.

10. The method for preparing the metal catalyst according to claim 1, characterized in that: The preparation method comprises: subjecting nickel salt and cobalt salt, organic ligand and alkaline regulator to hydrothermal reaction in a solvent to obtain a metal precursor, and then subjecting the metal precursor to pyrolysis reaction in a H2 atmosphere, wherein the pyrolysis temperature is 320-330°C and the pyrolysis time is 1-2h; and the metal catalyst is obtained.

11. Use of the metal catalyst according to any one of claims 1 to 9 in catalytic hydrogenation of unsaturated bonds in organic compounds.

Citation Information

Patent Citations

  • Oxygen reduction reaction catalyst

    CN107949941A

  • Catalyst for catalyzing oil hydrogenation to produce biological aviation fuel and preparation method and application thereof

    CN112473708A

  • Nickel-doped MOF-5 material as well as preparation method and application thereof

    CN113578388A

  • Porous carbon supported bimetallic catalyst and preparation and application thereof

    CN114522688A

  • Preparation method of nano metal oxide

    CN115259096A