A magnetic nano-enrichment material modified with aniline groups

By covering the porous mesh shell on magnetic iron tetroxide nanoparticles, magnetic nano-enriched materials with superparamagnetic and high specific surface area are prepared, which solves the problem of low aflatoxin enrichment efficiency in the prior art , achieves efficient and fast adsorption effect, and has high thermal stability and reusability.

CN116920802BActive Publication Date: 2024-11-22CHINESE ACAD OF INSPECTION & QUARANTINE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310960026.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-08-02
Publication Date
2024-11-22
Estimated Expiration
2043-08-02

AI Technical Summary

Technical Problem

Existing magnetic adsorption materials are inefficient and lack selectivity when enriching aflatoxin in food, making it difficult to meet the needs of efficient and rapid adsorption.

Method used

Aniline group formed by magnetic iron tetraoxide nanoparticles as nucleus, and through Schiff base reaction, N,N',N'-tetrakis(p-aminophenyl)p-phenylenediamine and terephthalaldehyde A porous mesh shell composed of repeating units was coated to prepare a magnetic nano-enriched material with superparamagnetic, large specific surface area and porous structure.

Benefits of technology

It realizes efficient, rapid adsorption and enrichment of aflatoxins, has stronger adsorption capacity and shorter analyte diffusion distance, is suitable for magnetic solid phase extraction of complex samples, and has high thermal stability and reusability. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FDA0005066910600000011
    Figure FDA0005066910600000011
  • Figure GDA0004449803630000021
    Figure GDA0004449803630000021
  • Figure GDA0004449803630000071
    Figure GDA0004449803630000071
Patent Text Reader

Abstract

A magnetic nano-enrichment material modified with aniline groups comprises: a core body, which is a ferroferric oxide nanoparticle; and a shell, which is coated on the surface of the core body, and is composed of repeating aniline group units shown in formula I obtained by dehydrating N,N,N',N'-tetra(p-aminophenyl)-p-phenylenediamine and terephthalaldehyde through Schiff base reaction; the magnetic nano-enrichment material has superparamagnetism, excellent chemical and thermal stability, large specific surface area, strong adsorption capacity, fast adsorption speed, and can be reused; the preparation method comprises: (1) contacting magnetic ferroferric oxide nanoparticles with N,N,N',N'-tetra(p-aminophenyl)-p-phenylenediamine and ultrasonically treating them, and then performing a first stirring to obtain a first mixture; (2) contacting the first mixture with terephthalaldehyde and a catalyst and performing a second stirring to obtain the magnetic nano-enrichment material; the prepared magnetic nano-enrichment material can be used to adsorb multiple aflatoxins.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of nanomaterials, and in particular, relates to a preparation method and application of a magnetic nano-enriched material. Background Art

[0002] Magnetic solid phase extraction is a sample pretreatment method with great potential. It has won wide attention due to its advantages such as simple operation, low solvent consumption and large adsorption capacity. Magnetic solid phase extraction has been successfully applied to the adsorption and enrichment and purification of trace / ultra-trace levels of organic pollutants in complex samples. The performance of magnetic adsorption materials is a key factor affecting the sensitivity and selectivity of magnetic solid phase extraction methods. At present, common magnetic adsorption materials mainly include inorganic coated magnetic materials, organic small molecule grafted magnetic materials, and carbon nanomaterials, molecular imprinted polymers or metal organic framework materials and other loaded magnetic materials.

[0003] Aflatoxins (AFT) are a class of mycotoxins with highly oxidized heterocyclic rings. They are mainly produced by Aspergillus flavus and Aspergillus parasiticus, the dominant fungal species under drought, warm and humid conditions. Since the discovery of this type of mycotoxin in the 1960s, it has been confirmed as a compound with carcinogenic, teratogenic and mutagenic effects, mainly damaging the liver, kidneys and other tissues of the body. Long-term exposure to AFT can lead to some serious health damage, such as gastrointestinal pain, edema, acute liver damage and even death. Therefore, magnetic materials used to enrich aflatoxins in food need to be studied. Summary of the invention

[0004] The present invention aims to at least solve the technical problems existing in the prior art. To this end, one purpose of the present invention is to provide a magnetic nano-enrichment material, which has superparamagnetism, large specific surface area and porous structure, etc. The magnetic nano-composite material is used to efficiently enrich aflatoxin in complex samples to obtain a new adsorbent with stronger and faster adsorption capacity.

[0005] The first aspect of the present invention provides a magnetic nano-enriched material, which includes: a core body and a shell, wherein the core body is composed of magnetic ferrosoferric oxide; the shell is coated on the surface of the core body, and the shell is composed of a repeating unit of an aniline group shown in formula I obtained by dehydrating N,N,N',N'-tetrakis(p-aminophenyl)-p-phenylenediamine and terephthalaldehyde through a Schiff base reaction.

[0006]

[0007] The magnetic nano-enriched material of the invention has magnetism, large specific surface area, porous structure, good dispersibility, strong adsorption capacity, fast adsorption speed and can be reused.

[0008] In addition, the magnetic nano-enriched material of the present invention may also have the following additional technical features:

[0009] The shell is a porous mesh structure. The thicker the thickness is, the more layers there are between the repeating units of the shell material, and the greater the adsorption capacity is.

[0010] The average adsorption pore size of the shell is 3-6nm, preferably 4.5nm, and the thickness is 20-50nm, with an average thickness of 30nm. Thus, it has a good adsorption effect on aflatoxin, wherein 4.5nm is the mesopore pore size, which is larger than the molecular diameter of the target object, and can form a spatial embedding effect with the target object.

[0011] The magnetic strength of the shell of the present invention is 28emu g -1 The appropriate magnetic response can achieve rapid separation of magnetic nano-enriched materials from sample matrices and shorten operation time. At the same time, magnetic nano-enriched materials have a shorter analyte diffusion distance in the sample solution, thereby improving adsorption efficiency.

[0012] The particle size of the core body of the present invention is 120-250nm.

[0013] The specific surface area of ​​the magnetic nanoparticles of the present invention is 77.88 m 2 g -1 Therefore, the specific surface area is large and the adsorption capacity is strong.

[0014] The magnetic nano-enriched material of the present invention has crystal diffraction peaks at 2θ of 30.3°, 35.7°, 43.3°, 53.7°, 57.2° and 62.9° in X-ray powder diffraction (XRD) data. This group of characteristic peaks matches Fe3O4 with a spinel structure, thereby proving the successful synthesis of Fe3O4 and that Fe3O4 still maintains its original crystal structure after being coated with a shell.

[0015] In the TGA data of the magnetic nanoparticles of the present invention, the weight of the Fe3O4 nanoparticles is changed. Figure 2What is different in e is that the thermal degradation curve of Fe3O4@TPBD-TPA has two degradation stages. The first one occurred between 50℃-500℃, with a total weight loss of 13.2%. The main reason for the first weight loss was the weight loss caused by the volatilization of bound water and small organic molecules. The second weight loss occurred between 500℃-800℃, with a total weight loss of 39.3%, which means that the C shell is destroyed, and at the same time means that the content of the synthesized Fe3O4@TPBD-TPA component is 39.3%, which further shows that Fe3O4@TPBD-TPA has thermal stability up to 500℃.

[0016] The second aspect of the present invention is to provide a method for preparing the magnetic nano-enriched material described in the first aspect of the present invention. The method comprises:

[0017] (1) contacting magnetic ferrosoferric oxide nanoparticles with N,N,N',N'-tetrakis(p-aminophenyl)-p-phenylenediamine (TPBD) and performing a first stirring to obtain a first mixture;

[0018] (2) contacting the first mixture with terephthalaldehyde (TPA) and a catalyst and performing a second stirring to obtain the aniline group-coated magnetic nano-enriched material.

[0019] The present invention uses the first mixture as a bridge, N,N,N',N'-tetrakis(p-aminophenyl)-p-phenylenediamine and terephthalaldehyde as functional monomers, and obtains an aniline covalent organic framework material with a large specific surface area and an ordered porous structure on the surface of magnetic ferrosoferric oxide nanoparticles through a Schiff base reaction.

[0020] The preparation method of the embodiment of the present invention has mild synthesis conditions, simple operation, no other by-products, and is a high atom economy reaction. In addition, the prepared aniline group-modified magnetic nano-enriched material has superparamagnetism, large specific surface area, strong adsorption capacity, and fast adsorption speed.

[0021] The mass ratio of the magnetic ferrosoferric oxide nanoparticles to the terephthalaldehyde is 1:(0.6-1.1), preferably, the mass ratio is 1:0.97.

[0022] Preferably, the molar ratio of N,N,N',N'-tetrakis(p-aminophenyl)-p-phenylenediamine to terephthalaldehyde is 1: 2. At this ratio, the two monomers can react fully, and the formed covalent organic framework material has a better core-shell structure and a relatively high yield.

[0023] In the preparation method of the present invention, the catalyst is acetic acid, so that the catalytic effect is good and the reaction rate is fast.

[0024] Preferably, the first stirring is performed in tetrahydrofuran. The present invention uses tetrahydrofuran as the reaction solvent, and the magnetic ferrosoferric oxide nanoparticles and the two monomers are well dispersed therein, thereby ensuring sufficient contact of the reaction system, and thus obtaining a better reaction effect.

[0025] Preferably, the first stirring time is 20-40 minutes, and the second stirring time is 60-140 minutes, preferably 120 minutes. Thus, the reaction is fully carried out and the yield of the product is high.

[0026] Preferably, the temperature of the first stirring and the second stirring are both 60-70°C, more preferably 65°C; the rotation speed is 400-800 rpm, more preferably 500 rpm.

[0027] The third aspect of the present invention is the use of the magnetic nano-enriched material described in the first aspect of the present invention or the magnetic nano-enriched material prepared by the preparation method of the second aspect of the present invention to adsorb aflatoxins in food; the aflatoxin is at least one of AFB1, AFB2, AFG1, and AFG2.

[0028] The magnetic nano-enrichment material of the invention has a strong aflatoxin adsorption capacity and a fast speed, and is suitable for the adsorption and extraction of aflatoxin in complex samples.

[0029] The adsorption capacity of the magnetic nano-enriched material of the present invention is 67.31-117.3 mg g -1 Therefore, the adsorption capacity of the magnetic nano-enrichment material can effectively remove aflatoxin from complex samples.

[0030] The specific surface area of ​​the magnetic nanoparticles of the present invention is 77.88 m 2 g -1 Therefore, the specific surface area is large and the adsorption capacity is strong.

[0031] The present invention has achieved the following technical effects:

[0032] (1) The magnetic nano-enriched material of the present invention has magnetic properties and a high specific surface area of ​​up to 77.88 m 2 g -1 ;

[0033] (2) The magnetic nano-enrichment material of the present invention performs magnetic solid phase microextraction on aflatoxin present in complex samples, and has a higher adsorption capacity (67.31-117.3 mg g -1 ) and a faster adsorption process (adsorption equilibrium can be reached in 2 min). BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1The scanning electron microscope and transmission electron microscope images of Fe3O4 nanoparticles and the magnetic nano-enriched material (Fe3O4@TPBD-TPA) prepared in Example 1 are shown. Figure 1 a and Figure 1 c is the scanning electron microscope and transmission electron microscope photos of Fe3O4 nanoparticles. Figure 1 b and Figure 1 d is the scanning electron microscope and transmission electron microscope photographs of the magnetic nano-enriched material (Fe3O4@TPBD-TPA).

[0035] Figure 2 To physically characterize the Fe3O4 nanoparticles and the magnetic nano-enriched material (Fe3O4@TPBD-TPA) prepared in Example 1: Figure 2 a is the XRD schematic diagram, Figure 2 b is a schematic diagram of VSM. Figure 2 c is a BET schematic diagram, Figure 2 d is the pore size distribution of Fe3O4@TPBD-TPA, Figure 2 e is the schematic diagram of TGA and Figure 2 f is the infrared spectrum of its monomer.

[0036] Figure 3 Schematic diagram of static adsorption and kinetic adsorption results of magnetic covalent organic framework for magnetic nano-enriched material (Fe3O4@TPBD-TPA) prepared in Example 1. Figure 3 a Schematic diagram of static adsorption results, Figure 3 b Schematic diagram of kinetic adsorption results. DETAILED DESCRIPTION

[0037] Below will be described in conjunction with embodiment scheme of the present invention.It will be appreciated by those skilled in the art that the following examples are only used to illustrate the present invention and should not be regarded as limiting the scope of the present invention.Unrepresented specific techniques or conditions in the embodiment, according to the technology or conditions described in the document in this area or according to the product specification sheet.Reagents used or instruments are not indicated by manufacturers, are conventional products that can be obtained by commercial purchase, for example, can be purchased from Sigma company.

[0038] Example 1 Preparation of magnetic nano-enriched material (Fe3O4@TPBD-TPA)

[0039] The preparation process of the magnetic nano-enriched material is as follows:

[0040] (a) In a 100-mL two-necked round-bottom flask, 100 mg of ferrosoferric oxide and 0.36 mmol of N,N,N',N'-tetrakis(p-aminophenyl)-p-phenylenediamine were added to 22 mL of tetrahydrofuran and ultrasonicated for 20 min.

[0041] (b) The product of step (a) is mechanically stirred at 65° C. for 40 minutes to allow part of the N,N,N',N'-tetrakis(p-aminophenyl)-p-phenylenediamine to be anchored to the surface of ferrosoferric oxide through hydrogen bonds for prepolymerization.

[0042] (c) 0.72 mmol of terephthalaldehyde was evenly dispersed in 8 mL of tetrahydrofuran, and added dropwise to the reaction system of step (b) with 500 μL of acetic acid under stirring. After the addition was completed, the reaction was carried out for 2 h to obtain a magnetic nano-enriched material (Fe3O4@TPBD-TPA).

[0043] Experimental Example 1 Characterization experiment of magnetic nano-enriched material (Fe3O4@TPBD-TPA)

[0044] This experimental example conducted a detailed characterization experiment on the magnetic nano-enriched material (Fe3O4@TPBD-TPA) obtained in Example 1 to prove the successful preparation of the magnetic nano-enriched material and its excellent physical and chemical properties. The details are as follows:

[0045] 1. Scanning electron microscopy and transmission electron microscopy were performed on ferroferric oxide and magnetic nano-enriched materials (Fe3O4@TPBD-TPA). The results are as follows Figure 1 a and Figure 1 As shown in c, the size of the spherical Fe3O4 nanoparticles is about 175 nm. In addition, compared with Fe3O4, a clear shell layer of about 30 nm of Fe3O4 and TPBD-TPA combined can be clearly observed on the Fe3O4@TPBD-TPA covering the surface of the Fe3O4 nanoparticles ( Figure 1 b and Figure 1 d), which confirms the successful synthesis of magnetic TPBD-TPA based on Fe3O4. Self-agglomeration of Fe3O4 was avoided.

[0046] 2. Analyze the crystal structure of Fe3O4 nanoparticles and Fe3O4@TPBD-TPA. The XRD patterns of Fe3O4 nanoparticles and Fe3O4@TPBD-TPA are shown in Figure 2As shown in Figure a, both Fe3O4 nanoparticles and Fe3O4@TPBD-TPA have six peaks at 30.3°, 35.7°, 43.3°, 53.7°, 57.2°, and 62.9°, which correspond to the crystal indexes of Fe3O4 nanoparticles (220), (311), (400), (422), (440), and (511). This indicates that Fe3O4@TPBD-TPA is well crystallized, and that the coverage of the Fe3O4 nanoparticles by the TPBD-TPA layer does not destroy the crystal structure of the Fe3O4 nanoparticles, and the crystallinity is high.

[0047] 3. The vibrating sample magnetization (VSM) curves of Fe3O4 nanoparticles and Fe3O4@TPBD-TPA were characterized. Figure 3 As shown in Figure b, the magnetic strength of Fe3O4 nanoparticles and Fe3O4@TPBD-TPA is compared. It can be clearly seen in the figure that the magnetization intensity of Fe3O4@TPBD-TPA is 28emu / g, while the magnetization intensity of Fe3O4 nanoparticles is 83emu / g. The magnetization intensity of Fe3O4 nanoparticles is significantly reduced after being wrapped by the TPBD-TPA layer, but Fe3O4@TPBD-TPA still has a high saturation magnetism, which meets the requirements of magnetic solid phase extraction, such as Figure 2 As shown in the inset in b, the Fe3O4@TPBD-TPA dispersed in the aqueous solution rapidly aggregated under the action of the external magnetic field within 0.5 min, making the solution immediately clear and transparent. This proves that Fe3O4@TPBD-TPA meets the basic requirements of magnetic solid phase extraction and has strong magnetic responsiveness and redispersibility.

[0048] 4. The adsorption gas required for this operation is nitrogen, and the nitrogen adsorption mode used is full pore (specific surface area plus pore size distribution, including mesopores + micropores). The degassing temperature used is 120℃, and the degassing time is 10h. Figure 2 As shown in Figure 3, the Brunauer-Emmett-Teller surface area of ​​Fe3O4@TPBD-TPA is 77.88 m 2 / g, such as Figure 2 As shown in the inset c, the surface area of ​​Fe3O4 is 15.6 m 2 / g, which proves that the surface area of ​​Fe3O4@TPBD-TPA is much higher than that of Fe3O4. The pore volume of Fe3O4@TPBD-TPA is 0.12cm 3 / g, which is also much higher than the 0.02cm of Fe3O4 nanoparticles. 3 / g, such as Figure 2As shown in Figure d, the pore size distribution shows that the average pore size of Fe3O4@TPBD-TPA is 4.5nm, and the size distribution is relatively narrow, indicating that it has mesoporous characteristics, and it has a large specific surface area and a large pore volume, which provides a more suitable environment for the adsorption of aflatoxin. Therefore, Fe3O4@TPBD-TPA is suitable for the enrichment and detection of aflatoxin.

[0049] 5. Fe3O4@TPBD-TPA and Fe3O4 were characterized by Hitachi TG / DTA 6300 instrument. The adsorption gas for this operation was nitrogen. The test range was 30℃-800℃, and the heating rate was 10℃ / min. The thermal stability of Fe3O4@TPBD-TPA and Fe3O4 nanoparticles and the mass ratio of different components were studied and compared by thermogravimetric analysis (TG). Figure 2 As shown in Figure e, when the temperature reaches 800°C, the weight of Fe3O4 nanoparticles is always about 4.87%, which is mainly attributed to the volatilization and decomposition of small organic molecules, resulting in changes in the weight of Fe3O4 nanoparticles. What is different in the figure is that the thermal degradation curve of Fe3O4@TPBD-TPA has two degradation stages. The first occurred between 50°C and 500°C, with a total weight loss of 13.2%. The main reason for the first weight loss was the weight loss caused by the volatilization of bound water and small organic molecules. The second weight loss occurred between 500°C and 800°C, with a total weight loss of 39.3%, which means that the C shell is destroyed, and at the same time means that the content of the synthesized Fe3O4@TPBD-TPA component is 39.3%, which further shows that Fe3O4@TPBD-TPA has thermal stability up to 500°C.

[0050] 6. Fourier transform infrared spectrometer was used to characterize Fe3O4@TPBD-TPA, Fe3O4, TPA and TPBD, and the characteristic peaks were used to determine whether Fe3O4@TPBD-TPA was successfully synthesized. Figure 2 As shown in f, Fe3O4@TPBD-TPA is compared with Fe3O4, with a characteristic peak of 578 cm -1 It is the stretching vibration peak of Fe-O-Fe. The characteristic peak 578cm is retained in Fe3O4@TPBD-TPA. -1 , indicating that Fe3O4@TPBD-TPA contains Fe3O4. Fe3O4@TPBD-TPA is compared with TPA and TPBD, and the characteristic peak is 3458cm -1 (NH stretching vibration peak), characteristic peak 3363cm -1 (CH stretching vibration peak in aldehyde group) disappeared, and the new characteristic peak was 1618cm -1(C=N stretching vibration peak) appeared, proving the successful synthesis of Fe3O4@TPBD-TPA.

[0051] Experimental Example 2 Adsorption experiment of aflatoxin (AFs) by magnetic nano-enrichment material (Fe3O4@TPBD-TPA)

[0052] In this experimental example, the feasibility of adsorbing four aflatoxins (AFs) in complex samples by using the magnetic nano-enrichment material (Fe3O4@TPBD-TPA) prepared in Example 1 was studied as follows:

[0053] Various studies have shown that aflatoxins are slightly soluble in water. Therefore, this study used a single standard solution of aflatoxins to generate adsorption isotherms at 10, 20, 30, 40, 50, 60, 70, 80, 90, 100, and 150 mg / L. After the single standard solution was prepared, Fe3O4@TPBD-TPA was used for adsorption testing. In the range of 10 to 80 mg / L, although the adsorption of the four aflatoxins increased significantly with increasing concentration, AFB2, AFG1, and AFG2 showed different adsorption amounts from other aflatoxins. Figure 3 As shown in a, when the concentration increased to 80 mg / L, the adsorption amounts of AFB2, AFG1 and AFG2 reached their maximum values ​​at 73.43, 67.5 and 69.3 mg / g, respectively. However, AFB1 was different from the other three aflatoxins. At 90 mg / L, the adsorption amount of AFB1 was balanced at 84.41 mg / g. The fact that these four aflatoxins reached equilibrium at different concentrations may be because AFB1 exhibited low polarity and thus had low steric hindrance. Therefore, Fe3O4@TPBD-TPA was more likely to approach AFB1 and interact with AFB1, and the adsorption equilibrium concentration of AFB1 was higher than that of the other three aflatoxins.

[0054]

[0055] Wherein, Q is the maximum adsorption capacity (mg / g), C0 is the initial concentration of the adsorption solution (μg / mL), Ce is the concentration of the target when the adsorption equilibrium is reached (μg / mL), m is the mass of Fe3O4@TPBD-TPA (mg), and v is the volume of the adsorption solution (mL).

[0056] Example 4

[0057] In this experimental example, the Langmuir and Freundlich isotherm models were used to fit the adsorption behavior of Fe3O4@TPBD-TPA. The Langmuir isotherm model assumes that on the solid surface, atoms or molecules exhibit outward residual valence forces, which capture gas molecules. Since the range of residual valence forces is proportional to the molecular diameter, the monolayer can only be adsorbed on the adsorbent surface; that is, each site can only adsorb one aflatoxin molecule. The linear Langmuir isotherm model is represented by the following formula:

[0058]

[0059] where q s It represents the theoretical saturated adsorption capacity (mg / g), C e is the equilibrium concentration (unit: g / mL), q e is the equilibrium adsorption capacity (in mg / g), K L is the Langmuir constant (unit: mL / g).

[0060] The Freundlich isotherm model can be applied to both monolayer adsorption and adsorption on inhomogeneous surfaces. As an empirical adsorption isotherm for inhomogeneous surfaces, the Freundlich adsorption equation can well describe the adsorption mechanism of inhomogeneous surfaces and is more suitable for adsorption at low concentrations. It can well explain the experimental results in a wider concentration range. The linear form of the Freundlich isotherm model is as follows:

[0061]

[0062] Among them C e is the equilibrium concentration (unit: g / mL), q e is the equilibrium adsorption capacity (unit: mg / g), k is the equilibrium constant, and n is the Freundlich constant.

[0063] Through data fitting analysis, the adsorption behavior of Fe3O4@TPBD-TPA is more consistent with the Langmuir isotherm model. For AFB1, AFB2, AFG1, and AFG2, the R2 of the Langmuir isotherm model is 0.988, 0.966, 0.997, and 0.992, respectively, and the R2 of the Freundlich isotherm model is 0.982, 0.947, 0.995, and 0.99, respectively. Obviously, the Langmuir isotherm model can better describe the adsorption behavior of Fe3O4@TPBD-TPA. The adsorption process is mainly multi-layer inhomogeneous adsorption, which is the result of the interaction of multiple forces.

[0064] Table 1 Langmuir thermodynamic and Freundlich thermodynamic parameters

[0065]

[0066] The relevant parameters of the thermodynamic model fitting results of Fe3O4@TPBD-TPA adsorption of four aflatoxins are shown in Table 1. It can be seen from the table that the Langmuir model has a good fitting effect on the adsorption process, R 2 ≥0.966, it is obvious that the Langmuir isotherm model more accurately describes the adsorption behavior of Fe3O4@TPBD-TPA, and the adsorption behavior is mainly multiphase multilayer adsorption occurring through the interaction of multiple forces.

[0067] Example 5 Experiment on the mechanism of interaction between Fe3O4@TPBD-TPA and aflatoxin

[0068] In this study, aflatoxin was adsorbed in a single standard aqueous solution of AFB1 (90 mg / L) and AFB2, AFG1, AFG2 (80 mg / L) for 5, 10, 20, 30, 40, 50, and 60 min to determine when the adsorption reached equilibrium and explore the mechanism of the interaction between Fe3O4@TPBD-TPA and aflatoxin. Figure 2 As shown in b, within the first 10 minutes, from 10 to 60 minutes, the adsorption amount of all aflatoxins increased with time, and when the adsorption equilibrium was reached, the maximum adsorption amount was between 64.4 and 84.4 mg / g.

[0069] The data was fitted by the first-order kinetic model and the second-order kinetic model. The expression of the first-order kinetic model is as follows:

[0070] where q e is the adsorption capacity at equilibrium (in mg / g), q t is the adsorption capacity at time t (in mg / g), and k1 is the adsorption rate constant of first-order kinetics (in 1 / h).

[0071] The expression of the second-order kinetic model is as follows:

[0072]

[0073] where q e is the adsorption capacity at equilibrium (in mg / g), q t is the adsorption capacity at time t (in mg / g), k2 is the adsorption rate constant of the second-order kinetics (in g / (mg·h))

[0074] Through data fitting analysis, the adsorption process of Fe3O4@TPBD-TPA is more consistent with the second-order kinetic model. As shown in Table 2, for AFB1, AFB2, AFG1, and AFG2, the R2 of the first-order kinetic model is 0.721, 0.787, 0.621, and 0.583, respectively, and the R2 of the second-order kinetic model is 2 They are 0.991, 0.989, 0.985, and 0.980, respectively. Compared with the first-order kinetic model, the coefficient of determination of the second-order kinetic model is closer to 1, indicating that the second-order kinetic model is more suitable for describing the adsorption process of Fe3O4@TPBD-TPA on aflatoxin. From the above results, it is inferred that the interaction force between Fe3O4@TPBD-TPA and aflatoxin is mainly intermolecular interaction force, including π-π stacking force, hydrogen bonding force, and hydrophobic force.

[0075] Table 2 Parameters of first-order and second-order kinetics

[0076]

[0077] In summary, the magnetic nano-enriched material of the embodiment of the present invention has superparamagnetism, large specific surface area, strong adsorption capacity and fast adsorption speed.

[0078] Although embodiments of the present invention have been shown and described, those skilled in the art will appreciate that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and the scope of the present invention is defined by the claims.

Claims

1. A magnetic nano-enriched material, characterized in that: include: The invention discloses a core body and a shell, wherein the shell is coated on the surface of the core body; the core body is magnetic ferrosoferric oxide; the shell is composed of repeating aniline group units shown in formula I obtained by dehydrating N,N,N',N'-tetrakis(p-aminophenyl)-p-phenylenediamine and terephthalaldehyde through Schiff base reaction; the average adsorption pore size of the shell is 3-6nm, and the thickness is 20-50nm; the magnetic strength of the magnetic nanoparticles is 28emu g -1 The specific surface area of ​​the shell is 77.88m 2 g -1 ; The magnetic nano-enriched material can be reused more than 10 times.

2. The magnetic nano-enriched material according to claim 1, characterized in that: The average particle size of the magnetic nanoparticles is 120-250 nm, and the shell is a porous mesh structure.

3. A method for preparing the magnetic nano-enriched material according to claim 1, comprising: (1) mixing magnetic ferrosoferric oxide nanoparticles and N,N,N',N'-tetrakis(p-aminophenyl)-p-phenylenediamine, performing ultrasonic treatment, and then performing a first stirring to obtain a first mixture; (2) contacting the first mixture with terephthalaldehyde and a catalyst and performing a second stirring to obtain the aniline group-modified magnetic nano-enriched material.

4. The preparation method according to claim 3, wherein the mass ratio of the magnetic ferroferric oxide nanoparticles to the N,N,N',N'-tetrakis(p-aminophenyl)-p-phenylenediamine is 1:(1-2), the mass ratio of the magnetic ferroferric oxide nanoparticles to the terephthalaldehyde is 1:(0.6-1.1), and the molar ratio of the N,N,N',N'-tetrakis(p-aminophenyl)-p-phenylenediamine to terephthalaldehyde is 1:

1.

5. The preparation method according to claim 4, wherein the mass ratio of the magnetic ferroferric oxide nanoparticles to the N,N,N',N'-tetrakis(p-aminophenyl)-p-phenylenediamine is 1:1.70, and the mass ratio of the magnetic ferroferric oxide nanoparticles to the terephthalaldehyde is 1:0.

97.

6. The preparation method according to claim 3, wherein the catalyst is acetic acid; The first stirring is carried out in tetrahydrofuran, and the first stirring time is 20-40 minutes; The second stirring time is 60-140 minutes; The temperature of the first stirring and the second stirring are both 60-70° C., and the rotation speed is 400-800 rpm.

7. The preparation method according to claim 6, The first stirring time is 30 minutes, The second stirring time is 120 minutes. The temperature of the first stirring and the second stirring were both 65° C., and the rotation speed was 500 rpm.

8. Use of the magnetic nano-enriched material according to claim 1 or 2 or the magnetic nano-enriched material prepared by the preparation method according to any one of claims 3 to 7 in adsorbing aflatoxin; The aflatoxin is at least one of AFB1, AFB2, AFG1, and AFG2.