A method for preparing porous microspheres
Through the cross-linked porous microspheres in the oil phase, the reaction of amino and aldehyde polymer Schiff bases is used to solve the problem that gelatin microspheres are not easy to degrade and uncontrollable in the prior art, and a rapid and effective hemostatic effect is achieved. , and adjust the pore size through ice crystal growth, suitable for a variety of biological applications.
Patent Information
- Application Number
- CN202310715943.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-16
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-06-16
AI Technical Summary
In the existing preparation methods for gelatin microspheres, small molecule crosslinking agents such as glutaraldehyde and genipine used cause the material to be difficult to degrade, the reaction is uncontrollable, and traditional crosslinking methods are difficult to achieve rapid and effective hemostasis effect.
Porous microspheres are prepared by Schiff base reaction using polymers containing amino and aldehyde groups, and cross-linking and curing in the oil phase, quickly absorb blood by capillary action, and the pore size and structure of the microspheres are adjusted through ice crystal growth.
The effect of rapid and large-scale hemostasis is achieved. The crosslinking agent is low in toxicity, and the microspheres have good biocompatibility and degradability, which can naturally degrade in the body. Microspheres of different pore sizes are obtained by adjusting the raw material ratio and ice crystal temperature. It is suitable for It is used in hemostasis, wound healing and drug carriers.
Smart Images

Figure CN116925359B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of biomedical materials, and in particular to a method for preparing porous microspheres. Background Art
[0002] Studies have shown that when a person suffers an accidental injury and loses blood, more than 30% of the total blood volume may cause death. If the bleeding can be effectively controlled in the early stage of blood loss, the survival rate of the injured can be greatly improved. Uncontrolled heavy bleeding is one of the main causes of death among the wounded, causing more than 2 million deaths each year. Therefore, rapid and efficient hemostasis is crucial to saving the lives of the wounded.
[0003] Gelatin is a soluble protein obtained by partial hydrolysis of collagen. Studies have shown that gelatin has a strong ability to absorb liquids and can concentrate serum, so it has good hemostatic properties. Pullulan is a linear microbial extracellular polysaccharide. Compared with other polymer systems, it has excellent mechanical properties, hydrophilicity, good biocompatibility and other advantages. The traditional chemical cross-linking methods of gelatin microspheres include the use of small molecule cross-linking agents such as glutaraldehyde and genipin, or the use of methacrylamide gelatin to cross-link by double bond polymerization under photoinitiation, but these methods will cause problems such as difficult material degradation and uncontrollable reactions. Summary of the invention
[0004] According to the first aspect, in one embodiment, a method for preparing porous microspheres is provided. The porous microspheres prepared by the method are obtained by reacting a polymer solution containing amino groups and a polymer solution containing aldehyde groups through a Schiff base reaction.
[0005] According to the second aspect, in one embodiment, a method for preparing the porous microspheres described in any one of the first aspect is provided.
[0006] According to the third aspect, in one embodiment, a hemostatic material is provided, comprising porous microspheres prepared by any method described in the first aspect.
[0007] According to the fourth aspect, in one embodiment, a material for promoting wound healing is provided, comprising the porous microspheres according to any one of the first aspect. The porous microspheres can promote wound healing.
[0008] According to the fifth aspect, in one embodiment, a drug carrier is provided, comprising the porous microspheres described in any one of the first aspect.
[0009] According to the sixth aspect, in one embodiment, a cell scaffold is provided, comprising the porous microspheres described in any one of the first aspect.
[0010] In one embodiment, the present invention provides a method for preparing porous microspheres that can quickly stop bleeding in large quantities.
[0011] In one embodiment, the reaction process of the present invention is mild and the cross-linking agent has low toxicity. When the porous microspheres are used for hemostasis, they can quickly absorb blood through capillary action. Because of their porous nature, they can absorb a large amount of blood, and ultimately achieve the effect of rapid and large-scale blood absorption. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] Figure 1 This is a scanning electron micrograph of the gelatin / oxidized pullulan microspheres prepared in Example 5;
[0013] Figure 2 This is a scanning electron micrograph of the gelatin / oxidized dextran microspheres prepared in Example 8;
[0014] Figure 3 is a scanning electron micrograph of the gelatin / oxidized hyaluronic acid microspheres prepared in Example 9;
[0015] Figure 4 This is an electron microscopic image of the gelatin / modified four-arm polyethylene glycol microspheres prepared in Example 10;
[0016] Figure 5 Thermogravimetric analysis of gelatin / oxidized pullulan microspheres prepared in Examples 1, 2, and 3;
[0017] Figure 6 This is a cytotoxicity analysis chart of gelatin / oxidized pullulan microspheres prepared in Example 2;
[0018] Fig. 7A This is the fluorescence imaging image of the small animal imaging of in vivo degradation in Example 2;
[0019] Figure 7B The fluorescence intensity diagram of feces and urine of small animals degraded in vivo in Example 2;
[0020] Figure 7C This is a fluorescence intensity diagram of the heart, liver, spleen, lung, and kidney of the small animal degraded in vivo in Example 2;
[0021] Fig.7D This is a fluorescence intensity diagram of the stomach and intestine of a small animal degraded in vivo in Example 2;
[0022] Figure 8 It is a statistical graph of hemolysis experiment of gelatin / oxidized pullulan microspheres prepared in Examples 1, 2 and 3;
[0023] Fig. 9 This is a diagram showing the effect of the gelatin / oxidized pullulan microspheres prepared in Example 2 in the tail docking experiment of SD rats;
[0024] Fig.10 This is a diagram showing the hemostatic effect of the gelatin / oxidized pullulan microspheres prepared in Example 2 in the SD rat liver lobe model. DETAILED DESCRIPTION
[0025] The present invention is further described in detail below by specific embodiments in conjunction with the accompanying drawings. In the following embodiments, many detailed descriptions are intended to enable the present application to be better understood. However, those skilled in the art can effortlessly recognize that some of the features can be omitted in different situations, or can be replaced by other materials and methods. In some cases, some operations related to the present application are not shown or described in the specification, in order to avoid the core part of the present application being overwhelmed by too much description, and for those skilled in the art, it is not necessary to describe these related operations in detail, and they can fully understand the related operations according to the description in the specification and the general technical knowledge in the art.
[0026] In addition, the features, operations or characteristics described in the specification can be combined in any appropriate way to form various implementations. At the same time, the steps or operations in the method description can also be interchanged or adjusted in a manner that is obvious to those skilled in the art. Therefore, the various sequences in the specification and the drawings are only for the purpose of clearly describing a certain embodiment and are not meant to be a required sequence unless otherwise specified that a certain sequence must be followed.
[0027] The serial numbers assigned to the components in this article, such as "first", "second", etc., are only used to distinguish the objects described and do not have any order or technical meaning.
[0028] According to the first aspect, in one embodiment, a porous microsphere is provided. The porous microsphere is obtained by reacting a polymer containing an amino group with a polymer containing an aldehyde group via a Schiff base reaction.
[0029] In one embodiment, the method for preparing the porous microspheres comprises: fully mixing a solution of a polymer containing an amino group and a polymer containing an aldehyde group, and then adding the solution to an oil phase to react and obtain microspheres. While the polymer containing an amino group and the polymer containing an aldehyde group undergo a Schiff base reaction to crosslink and solidify, the droplets change their morphology through some physical changes, and by selecting some conditions in which the chemical reaction is slower than the physical change, that is, the crosslinking time is much longer than the droplet dispersion time. Therefore, the morphology changes while crosslinking.
[0030] In one embodiment, the method for preparing the porous microspheres includes: quickly and fully mixing a polymer solution containing an amino group and a polymer solution containing an aldehyde group, and then dropping the obtained solution into the oil phase as soon as possible. After the reaction is completed, dehydrating, centrifuging, washing to remove the oil phase, soaking, and freeze-drying to obtain porous microspheres.
[0031] In one embodiment, the polymer solution containing amino groups and the polymer solution containing aldehyde groups are quickly and fully mixed and then added dropwise to the oil phase as quickly as possible.
[0032] In one embodiment, the polymer solution containing amino groups and the polymer solution containing aldehyde groups are quickly and fully mixed, and the mixing time may be 10 to 40 seconds, preferably 15 to 30 seconds, and more preferably 30 seconds.
[0033] In one embodiment, the time for adding the mixed solution of the polymer containing amino groups and the polymer containing aldehyde groups dropwise into the oil phase may be 60 to 130 seconds, preferably 120 seconds.
[0034] In one embodiment, the amino-containing polymer and the aldehyde-containing polymer solution are quickly and fully mixed and then dropwise added to the oil phase as quickly as possible, and then stirred continuously to allow the components to continue to react.
[0035] In one embodiment, the amino-containing polymer and the aldehyde-containing polymer solution are quickly and fully mixed and then dropwise added to the oil phase as quickly as possible, and then heated to 37-65° C., preferably 37° C., and stirred continuously.
[0036] In one embodiment, the polymer solution containing amino groups and the polymer solution containing aldehyde groups are quickly and fully mixed and then dropwise added to the oil phase as soon as possible, and the stirring time is continued for 1 to 12 hours.
[0037] In one embodiment, before the solution obtained by quickly mixing the polymer containing amino groups and the polymer containing aldehyde groups is added dropwise to the oil phase as soon as possible, the oil phase is preheated to 37-65° C.
[0038] In one embodiment, stirring is continued until the reaction is completed, and the product is sequentially cooled, dehydrated, washed, and centrifuged. The microspheres after centrifugation are soaked in deionized water, frozen to grow ice crystals, and then freeze-dried to obtain the porous microspheres.
[0039] In one embodiment, deionized water is used to soak the microspheres after centrifugation to facilitate the next step of freezing and growing ice crystals.
[0040] In one embodiment, the oil phase may include at least one of paraffin oil, peanut oil, corn oil, and olive oil.
[0041] In one embodiment, the oil phase further comprises an emulsifier.
[0042] In one embodiment, the emulsifier includes but is not limited to at least one of Span 80, Span 60, Tween 80, sucrose ester, sodium dodecylbenzene sulfonate, etc.
[0043] In one embodiment, the reaction is carried out at 37-70°C.
[0044] In one embodiment, the polymer containing amino groups and the polymer containing aldehyde groups may be natural polymers or synthetic polymers.
[0045] In one embodiment, the polymer containing amino groups includes but is not limited to at least one of silk fibroin, gelatin, collagen, chondroitin sulfate, chitosan, and amino-modified polyethylene glycol. The polymers used in the prior art have double bonds and require auxiliary conditions such as photocuring, while the polymers in the present invention do not have double bonds and do not require auxiliary conditions such as photocuring.
[0046] In one embodiment, the polymer containing aldehyde groups includes but is not limited to at least one of aldehyde-containing natural polymers and aldehyde-containing synthetic polymers.
[0047] In one embodiment, the natural polymer is oxidized by an oxidant to obtain an aldehyde-modified polymer.
[0048] In one embodiment, the oxidant includes but is not limited to at least one of sodium periodate and potassium permanganate.
[0049] In one embodiment, the natural polymer includes but is not limited to at least one of pullulan, dextran, and hyaluronic acid.
[0050] In one embodiment, the aldehyde-modified synthetic polymer includes but is not limited to at least one of aldehyde-modified straight-chain polyethylene glycol, four-arm polyethylene glycol, eight-arm polyethylene glycol, and the like.
[0051] According to the second aspect, in one embodiment, a method for preparing the porous microspheres described in any one of the first aspect is provided, comprising: quickly and fully mixing a polymer solution containing an amino group and a polymer solution containing an aldehyde group and then dropping the mixture into an oil phase; after the reaction is completed, dehydrating, centrifuging and washing to remove the oil phase, soaking in deionized water, freezing to grow ice crystals, and freeze-drying to obtain porous microspheres.
[0052] In one embodiment, the polymer solution containing amino groups and the polymer solution containing aldehyde groups are quickly and thoroughly mixed and then added dropwise to the oil phase as quickly as possible.
[0053] In one embodiment, the amino-containing polymer and the aldehyde-containing polymer solution are quickly and fully mixed and then dropwise added to the oil phase as quickly as possible, and then stirred continuously to allow the components to continue to react.
[0054] In one embodiment, the amino-containing polymer and the aldehyde-containing polymer solution are quickly and fully mixed and then dropwise added to the oil phase as quickly as possible, and then heated to 37-65° C. and stirred continuously.
[0055] In one embodiment, the polymer solution containing amino groups and the polymer solution containing aldehyde groups are quickly and fully mixed and then dropwise added to the oil phase as soon as possible, and the stirring time is continued for 1 to 12 hours.
[0056] In one embodiment, after the amino-containing polymer and the aldehyde-containing polymer solution are quickly and fully mixed and then dropwise added to the oil phase as soon as possible, the solutions of the two and the oil phase are preheated to 37-65° C. respectively.
[0057] In one embodiment, stirring is continued until the reaction is completed, and the product is sequentially cooled, dehydrated, centrifuged, and washed. The washed microspheres are soaked in deionized water, frozen to grow ice crystals, and then freeze-dried to obtain the porous microspheres.
[0058] In one embodiment, the washed microspheres are soaked in deionized water.
[0059] According to the third aspect, in one embodiment, a hemostatic material is provided, comprising porous microspheres prepared by the method described in any one of the first aspects.
[0060] According to the fourth aspect, in one embodiment, a material for promoting wound healing is provided, comprising the porous microspheres prepared as described in any one of the first aspect. According to the properties of the raw materials for preparing the porous microspheres, the prepared material can have the property of promoting wound healing.
[0061] According to the fifth aspect, in one embodiment, a drug carrier is provided, comprising the porous microspheres described in any one of the first aspect.
[0062] According to the sixth aspect, in one embodiment, a cell scaffold is provided, comprising the porous microspheres described in any one of the first aspect.
[0063] In one embodiment, a porous microsphere cross-linked by a macromolecular cross-linking agent is provided for rapid and large-scale hemostasis.
[0064] In one embodiment, the method for preparing porous microspheres comprises the following steps:
[0065] (1) Preparation of polymers with aldehyde groups
[0066] Some natural polysaccharides, such as pullulan, dextran, hyaluronic acid, etc., can be selected and oxidized with oxidants such as sodium periodate and potassium permanganate to obtain natural polymers with multiple aldehyde groups on each molecular chain; or synthetic polymers with more than two aldehyde groups in each molecule can be synthesized, for example, aldehyde-modified straight-chain polyethylene glycol, four-arm polyethylene glycol, eight-arm polyethylene glycol, etc.
[0067] (2) Preheating and preparing oil phase
[0068] Heat the liquid paraffin to 37°C, add an appropriate amount of emulsifier to form an oil phase, and mix evenly with mechanical stirring.
[0069] (3) Preheating to dissolve the dispersed phase
[0070] Heat to 37°C, prepare polymer solutions with amino groups and polymer solutions with aldehyde groups at appropriate concentrations. The polymer solutions with amino groups can be silk fibroin, gelatin, collagen, chondroitin sulfate, chitosan, amino-modified polyethylene glycol, etc.
[0071] (4) Preparation of porous microspheres
[0072] The pre-dissolved solution in step (3) is quickly and fully mixed, 25 mL is taken, and then quickly added dropwise to the oil phase prepared in step (2). After the addition is completed, stirring and heating are continued for 4 hours. After 4 hours, the solidified microspheres are washed with organic solvents such as acetone and isopropanol to remove the oil phase. After the oil phase is cleaned, the microspheres are soaked in deionized water. After soaking for 90 minutes, they are placed in a refrigerator and frozen overnight, and then freeze-dried. After freeze-drying, porous microspheres can be obtained. The present invention undergoes cross-linking during the addition process. After the addition is completed, the cross-linking is not completely completed, but continues to proceed slowly. The stirring process will further affect the material to form droplets, which are further cross-linked and solidified into microspheres. The methods such as microfluidics used in the prior art are mainly to form droplets, which are not solidified.
[0073] In one embodiment, the porous microspheres prepared by the present invention are degradable.
[0074] In one embodiment, in step (1), the oxidation degree of the oxidized polysaccharide can be adjusted according to the content of the added oxidant.
[0075] In one embodiment, in step (1), the oxidized polysaccharide used includes but is not limited to pullulan, dextran and hyaluronic acid.
[0076] In one embodiment, in step (2), the preheated and prepared oil phase includes but is not limited to paraffin oil, peanut oil, corn oil, olive oil, etc., and the types of emulsifiers include but are not limited to Span 80, Span 60, Tween 80, sucrose esters, sodium dodecylbenzene sulfonate, etc.
[0077] In one embodiment, in step (4), the mechanical stirring speed includes but is not limited to 500-1500 rpm, and the particle size of the obtained microspheres may vary depending on the stirring speed and the viscosity of the solution, including but not limited to 20-500 μm.
[0078] In one embodiment, the use of porous microspheres in hemostasis, wound healing, drug carriers, cell scaffolds, etc. is provided.
[0079] In one embodiment, the porous microspheres prepared by the method of the present invention can integrate the characteristics of two or more raw materials, and because the chemical cross-linking is denser than the simple physical mixed network, the structure is more stable, and the presence of gelatin in the raw materials can also make the microspheres degradable and biocompatible. It is expected that by adjusting the raw material ratio of the microspheres, a high degree of matching between the materials and the biological application parts can be achieved. In addition, the preparation of composite microspheres with higher strength can also obtain porous microspheres with different pore sizes by adjusting the ice crystal growth temperature, and then provide them to different cells as cell scaffolds.
[0080] In one embodiment, the present invention provides a porous microsphere of a controllable degradation, high-strength composite material and a preparation method thereof.
[0081] In one embodiment, a first object of the present invention is to provide a method for preparing microspheres using two or more polymer materials.
[0082] In one embodiment, the second object of the present invention is to provide a method for preparing gelatin microspheres cross-linked with polymers such as oxidized pullulan, oxidized dextran, and oxidized hyaluronic acid.
[0083] In one embodiment, a third object of the present invention is to prepare a method that is robust enough to prepare microspheres with a variety of pore sizes.
[0084] In one embodiment, the fourth object of the present invention is to prepare a biodegradable porous gelatin / oxidized pullulan composite microsphere for wound hemostasis.
[0085] In one embodiment, the method for preparing porous gelatin / oxidized pullulan microspheres provided by the present invention comprises the following steps:
[0086] (1) Oxidized Pullulan
[0087] 2 g of pullulan was dissolved in 100 mL of sulfuric acid solution with a pH of 4, and then 2.1-8.4 mmol of sodium periodate was added and stirred in the dark for 2-8 hours. After the reaction, it was dialyzed with a dialysis bag with a molecular weight cutoff of 1000. After dialysis for 60 hours, the solution was frozen overnight and finally freeze-dried to obtain oxidized pullulan.
[0088] (2) Preparation of the oil phase for the reaction
[0089] Pour 500 mL of paraffin oil into a 1000 mL reaction bottle, then add 1-5% of the solution of emulsifier, mechanically stir at 300-1500 rpm to mix evenly, and preheat at 37-65°C.
[0090] (3) Predissolved dispersed phase
[0091] The gelatin is heated and dissolved to prepare a 10-20% w / v aqueous solution, and the oxidized pullulan is prepared into a 2-10% w / v aqueous solution, and the solution is preheated at 37-65°C.
[0092] (4) Preparation of porous gelatin / oxidized pullulan microspheres
[0093] The preheated dispersed phase was quickly and evenly mixed with magnetic stirring for 30-90s, and 25mL of the mixed solution was added dropwise to the preheated oil phase. According to the time of viscosity change, the addition was completed within 30-180s, and the temperature was continuously heated at 37-65℃, and the mechanical stirring was continued at 300-1500rpm for 1-12h. After the reaction was completed, the ice bath was cooled for 10-30min. After cooling, 200mL of acetone was added to the system for dehydration. After dehydration for 30min, the microspheres were washed with organic solvents such as acetone and isopropanol, and then centrifuged at 1000rpm, repeated 3 times or more, and the oil on the surface of the microspheres was washed, and the microspheres were soaked in deionized water. After soaking in deionized water for 90min, they can be placed in a refrigerator at -20℃ or -80℃, waiting for ice crystal growth overnight, or directly using liquid nitrogen to promote the rapid growth of ice crystals to obtain microspheres with a certain size of ice crystals. After freeze-drying, porous microspheres with different pore sizes can be obtained.
[0094] In one embodiment, in step (1), the amount of sodium periodate used in the solution does not exceed 8.4 mmol, as too high an amount of oxidant may easily lead to over-oxidation. The optimal time range obtained from the sodium periodate oxidation time experiment is 4-6 hours.
[0095] In one embodiment, in step (2), the emulsifier may preferably be Span 80 at a concentration of 5%, and the mechanical stirring speed may be maintained at 500-800 rpm.
[0096] In one embodiment, in step (3), the preheating temperature is optimally controlled at 37° C. in the optimized experimental scheme. The mechanical stirring speed is maintained at 500-800 rpm. The concentration of the gelatin solution can be selected to be 20% w / v, and the concentration of oxidized pullulan can be selected to be 2-6% w / v.
[0097] In one embodiment, in step (4), 500-800rpm magnetic stirring can be used for rapid and uniform mixing, which lasts for about 30s, and the time of adding dropwise to the oil phase can be controlled within 60s. After the reaction is completed, 200mL of acetone is preferably used for dehydration, and the detergent is preferably acetone and isopropanol, two organic solvents. The temperature of ice crystal growth is adjusted according to the size of the required pore size. The lower the temperature, the larger the ice crystal, and the larger the pore size of the porous microsphere is obtained.
[0098] In one embodiment, the present invention provides a method for preparing porous microspheres by cross-linking two or more macromolecules, which is prepared according to any of the above methods.
[0099] In one embodiment, the present invention provides a porous gelatin / pullulan microsphere for sealing hemorrhagic wounds. The tail of a SD rat is cut off at 1 / 2, and 150 mg of porous microspheres are used, and it can be observed that the porous microspheres absorb liquid at the cut tail.
[0100] In one embodiment, the present invention provides a hemostatic sealing material that does not need to be removed and can avoid causing secondary damage. Gelatin / oxidized pullulan microspheres can be naturally degraded in the body and are a potential hemostatic material.
[0101] Example 1
[0102] (1) Oxidized Pullulan
[0103] 2 g of pullulan was dissolved in 100 mL of sulfuric acid solution with a pH of 4, and then 8.4 mmol of sodium periodate was added and stirred in the dark for 4 hours. After the reaction, the solution was dialyzed using a dialysis bag with a molecular weight cutoff of 1000. After dialysis for 60 hours, the solution was frozen overnight and freeze-dried to obtain oxidized pullulan.
[0104] (2) Preparation of the oil phase for the reaction
[0105] Pour 500 mL of paraffin oil into a 1000 mL reaction bottle, then add 16 g of Span 80 into the oil phase, stir mechanically at 530 rpm to mix evenly, and preheat at 37°C.
[0106] (3) Predissolved dispersed phase
[0107] Gelatin was heated and dissolved to prepare a 20% w / v aqueous solution, and oxidized pullulan was prepared into a 2% w / v aqueous solution, and the two were preheated at 37°C respectively.
[0108] (4) Preparation of porous gelatin / oxidized pullulan microspheres
[0109] The preheated dispersed phase was quickly and evenly mixed with magnetic stirring in equal proportion for 30s (through experimental trials, the optimal mixing time of pullulan and gelatin under this oxidation condition is 30s), and then added dropwise to the preheated oil phase to take 25mL of the mixed solution, and the addition was completed within 120s, and the mixture was continuously heated at 37°C and mechanically stirred at 530rpm for 3h. After the reaction was completed, it was cooled in an ice bath for 15min. After cooling, 200mL of acetone was added to the system for dehydration. After dehydration for 30min, the microspheres were washed with acetone and centrifuged at 1000rpm. This process was repeated for more than 3 times. After the oil on the surface of the microspheres was washed, the microspheres were soaked in deionized water. After soaking for 90min, they were placed in a refrigerator at -20°C and waited for ice crystals to grow overnight. After freeze-drying, porous microspheres GPMs-Ⅰ were obtained.
[0110] Example 2
[0111] (1) Oxidized Pullulan
[0112] 2 g of pullulan was dissolved in 100 mL of sulfuric acid solution with a pH of 4, and then 8.4 mmol of sodium periodate was added and stirred in the dark for 4 hours. After the reaction, it was dialyzed with a dialysis bag with a molecular weight cutoff of 1000. After dialysis for 60 hours, the solution was frozen overnight and finally freeze-dried to obtain oxidized pullulan.
[0113] (2) Preparation of the oil phase for the reaction
[0114] Pour 500 mL of paraffin oil into a 1000 mL reaction bottle, then add 16 g of Span 80 into the oil phase, stir mechanically at 530 rpm to mix evenly, and preheat at 37°C.
[0115] (3) Predissolved dispersed phase
[0116] Gelatin was heated and dissolved to prepare a 20% w / v aqueous solution, and oxidized pullulan was prepared into a 4% w / v aqueous solution, and the two were preheated at 37°C respectively.
[0117] (4) Preparation of porous gelatin / oxidized pullulan microspheres
[0118] The preheated dispersed phase was quickly and evenly mixed with a magnetic stirrer for 30 seconds in equal proportions, and then added dropwise to the preheated oil phase. 25 mL of the mixed solution was taken and added dropwise for 120 seconds. The mixture was continuously heated at 37 ° C and mechanically stirred at 530 rpm for 3 hours. After the reaction was completed, it was cooled in an ice bath for 15 minutes. After cooling, 200 mL of acetone was added to the system for dehydration. After dehydration for 30 minutes, the microspheres were washed with acetone and centrifuged at 1000 rpm. This process was repeated for more than 3 times. After the oil on the surface of the microspheres was washed, the microspheres were soaked in deionized water. After soaking for 90 minutes, they were placed in a refrigerator at -20 ° C and waited for ice crystals to grow overnight. After freeze-drying, porous microspheres GPMs-Ⅱ were obtained.
[0119] Example 3
[0120] (1) Oxidized Pullulan
[0121] 2 g of pullulan was dissolved in 100 mL of sulfuric acid solution with a pH of 4, and then 8.4 mmol of sodium periodate was added and stirred in the dark for 4 hours. After the reaction, it was dialyzed with a dialysis bag with a molecular weight cutoff of 1000. After dialysis for 60 hours, the solution was frozen overnight and finally freeze-dried to obtain oxidized pullulan.
[0122] (2) Preparation of the oil phase for the reaction
[0123] Pour 500 mL of paraffin oil into a 1000 mL reaction bottle, then add 16 g of Span 80 into the oil phase, stir mechanically at 530 rpm to mix evenly, and preheat at 37°C.
[0124] (3) Predissolved dispersed phase
[0125] Gelatin was heated and dissolved to prepare a 20% w / v aqueous solution, and oxidized pullulan was prepared into a 6% w / v aqueous solution, and the two were preheated at 37°C respectively.
[0126] (4) Preparation of porous gelatin / oxidized pullulan microspheres
[0127] The preheated dispersed phase was quickly and evenly mixed with magnetic stirring for 30 seconds, and then added to the preheated oil phase after mixing. 25 mL of the mixed solution was taken and added within 120 seconds. The mixture was continuously heated at 37 ° C and mechanically stirred at 530 rpm for 3 hours. After the reaction was completed, it was cooled in an ice bath for 15 minutes. After cooling, 200 mL of acetone was added to the system for dehydration. After dehydration for 30 minutes, the microspheres were washed with acetone and centrifuged at 1000 rpm. This process was repeated for more than 3 times. After the oil on the surface of the microspheres was washed, the microspheres were soaked in deionized water. After soaking for 90 minutes, they were placed in a refrigerator at -20 ° C and frozen overnight to obtain porous microspheres GPMs-Ⅲ.
[0128] Example 4
[0129] (1) Oxidized Pullulan
[0130] 2 g of pullulan was dissolved in 100 mL of sulfuric acid solution with a pH of 4, and then 8.4 mmol of sodium periodate was added and stirred in the dark for 4 hours. After the reaction, it was dialyzed with a dialysis bag with a molecular weight cutoff of 1000. After dialysis for 60 hours, the solution was frozen overnight and finally freeze-dried to obtain oxidized pullulan.
[0131] (2) Preparation of the oil phase for the reaction
[0132] Pour 500 mL of paraffin oil into a 1000 mL reaction bottle, then add 16 g of Span 80 into the oil phase, stir mechanically at 530 rpm to mix evenly, and preheat at 37°C.
[0133] (3) Predissolved dispersed phase
[0134] Gelatin was heated and dissolved to prepare a 20% w / v aqueous solution, and oxypullulan was prepared into a 4% w / v aqueous solution, and the two were preheated at 37°C respectively.
[0135] (4) Preparation of porous gelatin / oxidized pullulan microspheres
[0136] The preheated dispersed phase was quickly and evenly mixed with magnetic stirring for 30 seconds, and then added to the preheated oil phase. 25 mL of the mixed solution was added for 120 seconds, and the mixture was continuously heated at 37 ° C and mechanically stirred at 530 rpm for 3 hours. After the reaction was completed, it was cooled in an ice bath for 15 minutes. After cooling, 200 mL of acetone was added to the system for dehydration. After dehydration for 30 minutes, the microspheres were washed with acetone and centrifuged at 1000 rpm. This process was repeated for more than 3 times. After the oil on the surface of the microspheres was washed, the microspheres were soaked in deionized water. After soaking for 90 minutes, they were placed in a refrigerator at -80 ° C and waited for ice crystals to grow overnight. After freeze-drying, porous microspheres GPMs-IV were obtained.
[0137] Example 5
[0138] (1) Oxidized Pullulan
[0139] 2 g of pullulan was dissolved in 100 mL of sulfuric acid solution with a pH of 4, and then 8.4 mmol of sodium periodate was added and stirred in the dark for 4 hours. After the reaction, the solution was dialyzed using a dialysis bag with a molecular weight cutoff of 1000. After dialysis for 60 hours, the solution was frozen overnight and freeze-dried to obtain oxidized pullulan.
[0140] (2) Preparation of the oil phase for the reaction
[0141] Pour 500 mL of paraffin oil into a 1000 mL reaction bottle, then add 16 g of Span 80 into the oil phase, stir mechanically at 530 rpm to mix evenly, and preheat at 37°C.
[0142] (3) Predissolved dispersed phase
[0143] Gelatin was heated and dissolved to prepare a 20% w / v aqueous solution, and oxidized pullulan was prepared into a 4% w / v aqueous solution, and the two were preheated at 37°C respectively.
[0144] (4) Preparation of porous gelatin / oxidized pullulan microspheres
[0145] The preheated dispersed phase was quickly and evenly mixed with magnetic stirring for 30 seconds, and then added to the preheated oil phase after mixing. 25 mL of the mixed solution was taken and added for 120 seconds. The mixture was continuously heated at 37 ° C and mechanically stirred at 530 rpm for 3 hours. After the reaction was completed, it was cooled in an ice bath for 15 minutes. After cooling, 200 mL of acetone was added to the system. After dehydration for 30 minutes, the microspheres were washed with acetone and centrifuged at 1000 rpm. This process was repeated for more than 3 times. After the oil on the surface of the microspheres was washed, the microspheres were soaked in deionized water. After soaking for 90 minutes, they were placed in liquid nitrogen. After 5 minutes, the ice crystals were completely grown, and then freeze-dried. Finally, the porous microspheres GPMs-V were obtained.
[0146] Example 6
[0147] (1) Oxidized Pullulan
[0148] 2 g of pullulan was dissolved in 100 mL of sulfuric acid solution with a pH of 4, and then 4.2 mmol of sodium periodate was added and stirred in the dark for 4 hours. After the reaction, it was dialyzed for 60 hours using a dialysis bag with a molecular weight cutoff of 1000. The solution was frozen overnight and finally freeze-dried to obtain oxidized pullulan.
[0149] (2) Preparation of the oil phase for the reaction
[0150] Pour 500 mL of paraffin oil into a 1000 mL reaction bottle, then add 16 g of Span 80 to the oil phase, stir mechanically at 530 rpm to mix evenly, and preheat at 37 °C.
[0151] (3) Predissolved dispersed phase
[0152] Gelatin was heated and dissolved to prepare a 20% w / v aqueous solution, and oxidized pullulan was prepared into a 4% w / v aqueous solution, and the two were preheated at 37°C respectively.
[0153] (4) Preparation of porous gelatin / oxidized pullulan microspheres
[0154] The preheated dispersed phase was quickly and evenly mixed with magnetic stirring for 30 seconds in equal proportions, and then added dropwise to the preheated oil phase after mixing. 25 mL of the mixed solution was taken and added dropwise for 120 seconds, and the mixture was continuously heated at 37 ° C and mechanically stirred at 530 rpm for 3 hours. After the reaction was completed, the mixture was cooled in an ice bath for 15 minutes. After cooling, 200 mL of acetone was added to the system. After dehydration for 30 minutes, the microspheres were washed with acetone and centrifuged at 1000 rpm. This process was repeated for more than 3 times. After the oil on the surface of the microspheres was washed, the microspheres were soaked in deionized water. After soaking for 90 minutes, the microspheres were placed in a refrigerator at -20 ° C and waited for ice crystals to grow overnight, and then freeze-dried. After freeze-drying, porous microspheres GPMs-VI were obtained.
[0155] Example 7
[0156] (1) Oxidized Pullulan
[0157] 2 g of pullulan was dissolved in 100 mL of sulfuric acid solution with a pH of 4, and then 2.1 mmol of sodium periodate was added and stirred in the dark for 4 hours. After the reaction, it was dialyzed with a dialysis bag with a molecular weight cutoff of 1000. After dialysis for 60 hours, the solution was frozen overnight and finally freeze-dried to obtain oxidized pullulan.
[0158] (2) Preparation of the oil phase for the reaction
[0159] Pour 500 mL of paraffin oil into a 1000 mL reaction bottle, then add 16 g of Span 80 into the oil phase, stir mechanically at 530 rpm to mix evenly, and preheat at 37°C.
[0160] (3) Predissolved dispersed phase
[0161] Gelatin was heated and dissolved to prepare a 20% w / v aqueous solution, and oxidized pullulan was prepared into a 4% w / v aqueous solution, and the two were preheated at 37°C respectively.
[0162] (4) Preparation of porous gelatin / oxidized pullulan microspheres
[0163] The preheated dispersed phase was quickly and evenly mixed with magnetic stirring for 30 seconds, and then added to the preheated oil phase after mixing. 25 mL of the mixed solution was taken and added for 120 seconds. The mixture was continuously heated at 37 ° C and mechanically stirred at 530 rpm for 3 hours. After the reaction was completed, it was cooled in an ice bath for 15 minutes. After cooling, 200 mL of acetone was added to the system for dehydration. After dehydration for 30 minutes, the microspheres were washed with acetone and centrifuged at 1000 rpm. This process was repeated for more than 3 times. After the oil on the surface of the microspheres was washed, the microspheres were soaked in deionized water. After soaking for 90 minutes, they were placed in a refrigerator at -20 ° C and waited for ice crystals to grow overnight. After freeze-drying, porous microspheres GPMs-VII were obtained.
[0164] Example 8
[0165] (1) Oxidized dextran
[0166] 10 g of dextran was dissolved in 100 mL of deionized water, and then 2.1 mmol of sodium periodate was added and stirred in the dark for 4 hours. After the reaction, it was dialyzed with a dialysis bag with a molecular weight cutoff of 3500. After dialysis for 60 hours, the solution was frozen overnight and finally freeze-dried to obtain oxidized dextran.
[0167] (2) Preparation of the oil phase for the reaction
[0168] Pour 500 mL of paraffin oil into a 1000 mL reaction bottle, then add 16 g of Span 80 into the oil phase, stir mechanically at 530 rpm to mix evenly, and preheat at 37°C.
[0169] (3) Predissolved dispersed phase
[0170] Gelatin was heated and dissolved to prepare a 20% w / v aqueous solution, and oxidized dextran was prepared into a 4% w / v aqueous solution, and the two were preheated at 37°C respectively.
[0171] (4) Preparation of porous gelatin / oxidized dextran microspheres
[0172] The preheated dispersed phase was quickly and evenly mixed with a magnetic stirrer for 30 seconds in equal proportions, and then added dropwise to the preheated oil phase after mixing. 25 mL of the mixed solution was taken and added dropwise for 120 seconds, and the mixture was continuously heated at 37 ° C and mechanically stirred at 530 rpm for 3 hours. After the reaction was completed, it was cooled in an ice bath for 15 minutes. After cooling, 200 mL of acetone was added to the system for dehydration. After dehydration for 30 minutes, the microspheres were washed with acetone and centrifuged at 1000 rpm. This process was repeated for more than 3 times. After the oil on the surface of the microspheres was washed, the microspheres were soaked in deionized water. After soaking for 90 minutes, they were placed in liquid nitrogen. After the ice crystals grew completely, they were freeze-dried to obtain the porous microspheres GPMs-VIII.
[0173] Example 9
[0174] (1) Oxidized hyaluronic acid
[0175] Dissolve 10 g of hyaluronic acid in 100 mL of deionized water, then add 13 g of sodium periodate and stir in the dark, react for 4 hours, and after the reaction is completed, dialyze with a dialysis bag with a molecular weight cutoff of 3500. After dialysis for 60 hours, freeze the solution overnight and finally freeze-dry it to obtain oxidized hyaluronic acid.
[0176] (2) Preparation of the oil phase for the reaction
[0177] Pour 100 mL of paraffin oil into a 250 mL reaction bottle, then add 3 g of Span 80 into the oil phase, stir mechanically at 530 rpm to mix evenly, and preheat at 37 °C.
[0178] (3) Predissolved dispersed phase
[0179] Gelatin was heated and dissolved to prepare a 20% w / v aqueous solution, and oxidized hyaluronic acid was prepared into a 4% w / v aqueous solution, and the two were preheated at 37°C respectively.
[0180] (4) Preparation of porous gelatin / oxidized hyaluronic acid microspheres
[0181] The preheated dispersed phase was quickly and evenly mixed with magnetic stirring for 15 seconds, and then added to the preheated oil phase after mixing. 5 mL of the mixed solution was taken out and added after 30 seconds. The mixture was continuously heated at 37 ° C and mechanically stirred at 530 rpm for 16 hours. After the reaction was completed, it was cooled in an ice bath for 15 minutes. After cooling, 50 mL of acetone was added to the system for dehydration. After dehydration for 30 minutes, the microspheres were washed with acetone and centrifuged at 1000 rpm. This process was repeated for more than 3 times. After the oil on the surface of the microspheres was washed, the microspheres were soaked in deionized water. After soaking for 90 minutes, they were placed in liquid nitrogen, and the ice crystals were completely grown. They were freeze-dried to finally obtain porous microspheres GPMs-IX.
[0182] Example 10
[0183] (1) Amino-modified polyethylene glycol
[0184] A 4-arm polyethylene glycol can be selected for amino modification, or the modified amino polyethylene glycol can be directly purchased. In this embodiment, an amino 4-arm polyethylene glycol with a molecular weight of 10k is selected.
[0185] (2) Preparation of the oil phase for the reaction
[0186] Pour 100 mL of paraffin oil into a 250 mL reaction bottle, then add 3 g of Span 80 into the oil phase, stir mechanically at 530 rpm to mix evenly, and preheat at 37 °C.
[0187] (3) Predissolved dispersed phase
[0188] Gelatin was heated to 37°C to prepare a 20% w / v aqueous solution, and amino polyethylene glycol was prepared into a 4% w / v aqueous solution, and both were preheated at 37°C.
[0189] (4) Preparation of porous gelatin / polyethylene glycol microspheres
[0190] The preheated dispersed phase was quickly and evenly mixed with magnetic stirring for 15 seconds, and then added to the preheated oil phase as soon as possible after mixing. 5 mL of the mixed solution was taken and added for 30 seconds. The mixture was continuously heated at 37 ° C and mechanically stirred at 530 rpm for 16 hours. After the reaction was completed, it was cooled in an ice bath for 15 minutes. After cooling, 50 mL of acetone was added to the system for dehydration. After dehydration for 30 minutes, the microspheres were washed with acetone and centrifuged at 1000 rpm. This process was repeated for more than 3 times. After the oil on the surface of the microspheres was washed, the microspheres were soaked in deionized water. After soaking for 90 minutes, they were placed in liquid nitrogen. After the ice crystals grew completely, the porous microspheres GPMs-X were obtained after freeze-drying.
[0191] (I) Microsphere structure characterization
[0192] (1) Scanning electron microscopy morphology characterization
[0193] In order to detect the morphology of the porous microspheres, the porous gelatin / oxidized pullulan microspheres prepared in Example 5 were subjected to morphological analysis, and the obtained scanning electron microscope photographs are shown in FIG. Figure 1 As shown in the figure, the microspheres have a relatively large pore size, and the pore size of the microspheres obtained after freeze-drying is about 10 μm. Figure 1 It can be seen that the microspheres have a pore structure and are stable without collapse.
[0194] In order to detect the morphology of the porous microspheres, the porous gelatin / oxidized dextran microspheres prepared in Example 8 were subjected to morphological analysis, and the obtained scanning electron microscope photographs are shown in FIG. Figure 2 As shown, the microspheres have a porous structure and are stable without collapse.
[0195] In order to detect the morphology of the porous microspheres, the porous gelatin / oxidized hyaluronic acid microspheres prepared in Example 9 were subjected to morphological analysis, and the obtained scanning electron microscope photographs are shown in FIG. Figure 3 As shown. It can be seen that the microspheres have a porous structure and the structure has not collapsed. Compared with the first two microspheres ( Figure 1 , 2 ), Figure 3 The particle size of the microspheres shown is relatively large, which may be due to the high viscosity of hyaluronic acid, which makes it less dispersible under the same shear force. Its pore structure is not as stable as the first two, which may be because the strength of hyaluronic acid itself is not as high as pullulan and dextran.
[0196] The three types of microspheres use the same ratio of gelatin and oxidized polysaccharide, the same oil phase, emulsifier type and content, and reaction speed, but the obtained microspheres have different particle sizes. The same pore-forming conditions, i.e., liquid nitrogen pore-forming, result in different pore sizes of the obtained microspheres, indicating that different combinations of raw materials will produce microspheres with different particle sizes and pore sizes due to their different properties such as viscosity.
[0197] Figure 4 The electron microscope image of the porous microspheres prepared in Example 10 shows that gelatin and modified polyethylene glycol can also be used to prepare microspheres using this method.
[0198] (2) Thermogravimetric analysis
[0199] The microspheres GPMs-I, GPMs-II and GPMs-III obtained in Examples 1, 2 and 3 were subjected to thermogravimetric analysis. The temperature was raised from 100°C to 800°C at a rate of 5°C / min. The obtained thermogravimetric curves are shown in FIG. Figure 5 As shown, the weight loss rate of the microspheres was less than that of their raw materials gelatin and oxidized pullulan.
[0200] (3) Porosity test
[0201] The porosity of porous microspheres GPMs (I, II, and III) was measured using the liquid displacement method (ethanol, at room temperature). First, an empty hydrometer (M) was filled with ethanol (total weight M1). Second, the porous microspheres (GPMs) were completely immersed in the hydrometer filled with ethanol. The hydrometer was vacuumed for 3 minutes, the pores of the microspheres were filled with ethanol, and then the hydrometer was refilled with ethanol (total weight M2). Finally, the remaining ethanol in the hydrometer was drained, and the remaining weight (hydrometer, microspheres, and ethanol in the pores of the microspheres) was M3. The porosity (P) of the porous microspheres was calculated as follows:
[0202] V s =(M1-M2+M3-M) / ρ ethanol
[0203] P(%)=V p / V s =(M3-MM s ) / (M1-M2+M3-M)
[0204] The experimental results show that the porous microspheres GPMs-I, GPMs-II and GPMs-III all exceed 90%, which also proves that the microspheres have a porous structure.
[0205] (II) Microsphere Biosafety Test
[0206] (1) Cytotoxicity assay
[0207] The cell viability of the microspheres GPMs-Ⅱ obtained in Example 2 was studied using the CCK-8 toxicity quantification method. Mouse fibroblasts were seeded in a 96-well plate with a cell density of 3,000 cells per well and incubated in an incubator at 37°C and 5% CO2 for 24 hours. GPMs-Ⅱ was soaked in complete culture medium at three concentrations of 5g / mL, 10g / mL and 20g / mL for 24 hours, and Yunnan Baiyao (YB) was selected as a commercial control group at a concentration of 10g / mL. Cells cultured in complete culture medium were used as blank controls (Control). The sample solution was removed at 24h, 48h, and 72h, and 10μL of CCK-8 reagent was added to the culture medium and cultured for 1.5h. Finally, the absorbance of the sample solution was detected at 450nm using an enzyme reader, as shown in Figure 6 In the three concentrations of material extracts, high, medium and low, the results of the cck-8 experiment showed that there was no cell toxicity. Compared with the high cytotoxicity of Yunnan Baiyao, GPMs showed its advantage in low cytotoxicity.
[0208] (2) In vivo degradation experiment
[0209] The material GPMs-II was prepared by labeling gelatin with Cy 5.5. 1 mg was implanted subcutaneously in C57 mice. Fluorescence imaging was performed on the mice at fixed time intervals to observe the changes in fluorescence intensity. The results are as follows: Fig. 7A It can be seen that with the increase of implantation time, the fluorescence signal is significantly weakened. After 1 day of implantation, the fluorescence signal is significantly weakened, and the weakening is more obvious after 4 days. After 15 days, the fluorescence signal disappears. The feces and urine of the above mice were collected and the fluorescence intensity of their feces and urine was observed. The changes in the intensity of the fluorescence signal of their metabolic pathways and excrement can be seen. The results are as follows Figure 7B It can be seen that there is no fluorescent signal in the urine of mice, indicating that the metabolism of GPMs-Ⅱ does not pass through the kidneys, while there is a certain fluorescent signal in the feces, indicating that the metabolism of GPMs-Ⅱ passes through the gastrointestinal tract. A mouse was dissected at a certain time, and the fluorescent signals of its heart, liver, spleen, lung, kidney, stomach, and intestine were observed. The results are as follows Figure 7C and Fig.7D It can be seen that on the 5th day, the liver and kidney of the mouse had some fluorescence, and the gastrointestinal tract had certain fluorescence signals from 3 to 15 days, and as the number of days increased, the fluorescence signal weakened. Therefore, it can be seen that the metabolism of GPMs-Ⅱ in mice is mainly through the gastrointestinal tract.
[0210] (3) Blood compatibility test
[0211] The microspheres GPMs-Ⅰ, GPMs-Ⅱ, and GPMs-Ⅲ obtained in Examples 1, 2, and 3 were soaked in a suspension prepared with PBS at a concentration of 10 g / mL for 24 hours. Fresh anticoagulated rat whole blood was centrifuged at 3000 rpm for 10 minutes to obtain red blood cells, which were then washed with PBS and centrifuged again, repeated 3 times, and the red blood cells were diluted with PBS to a 4 vol.% suspension. PBS and the extract were diluted into a mixture of (1:1 v / v) and incubated at 37°C for 3 hours. Next, the mixture was centrifuged at 3000 rpm for 10 minutes, and the absorbance of the supernatant at 540 nm was tested with an enzyme marker. 0.1% Triton solution was used as the positive control, and PBS was used as the negative control. The data obtained are as follows Figure 8 As shown, the hemolysis rate of the sample is less than 5%, indicating that the material is safe.
[0212] (IV) Porous microsphere hemostatic performance test
[0213] (1) Hemostasis experiment in rat tail amputation model
[0214] SD rat tail amputation hemostasis experiment: SD rats (male, 300-350g). Rats were anesthetized with isoflurane gas. After anesthesia, the rats were placed on the operating table, the tails were disinfected, and filter paper was placed under the tails. The picture of 0s was recorded, and the tails were cut off at 1 / 2, and the time was recorded at the same time. The tails were allowed to bleed freely for 5s. After 5s, the blood at the tail was quickly wiped off, and 160mg of hemostatic powder (GPMs-Ⅱ) was sprinkled on the tails. The bleeding was observed every 10s to see if it stopped, and pictures were taken at different times (30s, 1min, 3min). Fig. 9 The hemostatic effect of the tail amputation model of SD rats was significant, among which GPMs-Ⅱ completely stopped the bleeding of tail amputation within 60 seconds, and there was no obvious change after 3 minutes.
[0215] (2) Hemostasis experiment in rat liver lobe model
[0216] SD rat liver lobe hemostasis experiment: SD rats (male, 300-350g). The rats were anesthetized with isoflurane gas. After anesthesia, the rats were placed on the operating table, the abdomen of the rats was shaved, the abdominal cavity was cut open, the liver was found, the liver was properly wiped with cotton, and after wiping off excess body fluids, filter paper was placed under the liver, and photos were taken. The state at 0s was recorded, and a liver lobe of approximately 2cm was cut, and the time was recorded at the same time. After 5s of free bleeding, 300mg of hemostatic powder (GPMs-Ⅱ) was sprinkled, and the bleeding was observed every 10s. Photos were taken at 10s, 30s, 1min, and 2min until the bleeding stopped. The blank group was subjected to the experiment in a free bleeding manner. The results are as follows Fig.10 As shown. It can be seen that in the hemostatic effect of the SD rat liver lobe model, GPMs-Ⅱ successfully stopped bleeding in the rat liver at 1 minute, and there was no obvious change at 2 minutes, while the blank group did not receive any treatment and still failed to stop bleeding significantly at 2 minutes.
[0217] In one embodiment, the microspheres prepared by the present invention have high porosity. The porosity thereof is tested by a solution replacement method and can be as high as more than 90%.
[0218] In one embodiment, the present invention relates to a method for preparing microspheres using macromolecules as crosslinking agents, which can be used to prepare porous microspheres for rapid and large-scale hemostasis. First, a macromolecular crosslinking agent is prepared. The natural compound can be selected from natural polysaccharides, and the natural polysaccharides are oxidized to obtain polysaccharides with multiple aldehyde groups on the molecular chain; or a high molecular compound with two or more aldehyde groups on the molecular chain is synthesized. Then the compound with aldehyde groups is dissolved in a solvent, and the compound with amino groups is also dissolved in the same solvent, and then quickly and fully mixed, and then the mixed liquid is added dropwise to the oil phase containing an emulsifier, and small droplets are formed by an oil-in-water method. The compound with amino groups and the compound with aldehyde groups are crosslinked and cured, because the dispersion time is much shorter than the crosslinking and curing time, therefore, the purpose of completing crosslinking and curing can be achieved after the droplets are fully dispersed in the oil phase; after a period of curing is completed, the oil and emulsifier are washed off with an organic solvent, and then the microspheres are fully soaked with deionized water, and after being fully soaked, they are placed in a refrigerator or liquid nitrogen to form ice crystals of different sizes; finally, freeze-dried to obtain microspheres with a porous structure. The reaction process of the present invention is mild, the cross-linking agent has low toxicity, and the cross-linking density can be adjusted by adjusting the content of the compound with aldehyde group or the degree of oxidation and other aspects. The cross-linking agent can not only play the role of cross-linking, but also provide some properties of the cross-linking agent itself to the microspheres; ice crystals of different sizes can be obtained by adjusting the temperature of ice crystal formation, and then porous microspheres of different pore sizes can be obtained after freeze-drying. When the porous microspheres are used for hemostasis, they can quickly absorb blood through capillary action, and because of their high porosity, they have a high blood absorption capacity. The present invention is suitable for preparing microspheres in multiple fields such as embolism, drug loading (especially controlled release drug loading), porogens, cell scaffolds, etc.
[0219] The above specific examples are used to illustrate the present invention, which is only used to help understand the present invention and is not intended to limit the present invention. For those skilled in the art, according to the concept of the present invention, some simple deductions, modifications or substitutions can be made.
Claims
1. A method for preparing porous microspheres, characterized in that: The porous microspheres are obtained by reacting a polymer containing an amino group with a polymer containing an aldehyde group through a Schiff base reaction; The polymer containing amino group is gelatin; The polymer containing aldehyde groups includes at least one of aldehyde-containing natural polymers and aldehyde-containing synthetic polymers; The natural polymer includes at least one of pullulan, dextran and hyaluronic acid; The aldehyde-modified synthetic polymer comprises at least one of aldehyde-modified linear polyethylene glycol, four-arm polyethylene glycol, and eight-arm polyethylene glycol; The preparation method of the porous microspheres comprises: dripping a solution obtained by mixing a polymer solution containing amino groups and a polymer solution containing aldehyde groups into an oil phase, continuing to stir so that the components continue to react, and after the reaction is completed, sequentially cooling, dehydrating, washing, and centrifuging the product, soaking the washed and centrifuged microspheres, then freezing to grow ice crystals, and finally freeze-drying to obtain the porous microspheres; After adding the solution obtained by mixing the polymer solution containing amino groups and the polymer solution containing aldehyde groups into the oil phase, heating to 37-65°C and continuing stirring; Before adding the solution obtained by mixing the polymer solution containing amino groups with the polymer solution containing aldehyde groups into the oil phase, the two solutions and the oil phase are preheated to 37-65°C respectively; The oil phase also contains an emulsifier.
2. The preparation method according to claim 1, characterized in that After adding the solution obtained by mixing the polymer solution containing amino groups and the polymer solution containing aldehyde groups into the oil phase, the stirring time is continued for 1 to 12 hours; Alternatively, the washed microspheres are soaked in water.
3. The preparation method according to claim 1 or 2, characterized in that: The oil phase comprises at least one of paraffin oil, peanut oil, corn oil and olive oil; Or, the emulsifier includes at least one of Span 80, Span 60, Tween 80, sucrose ester, and sodium dodecylbenzene sulfonate; Alternatively, the reaction is carried out at 37-65°C.
4. A porous microsphere prepared by the preparation method according to any one of claims 1 to 3.
5. A hemostatic material, characterized in that: The porous microspheres according to claim 4 are included.
6. A material for promoting wound healing, characterized in that: The porous microspheres according to claim 4 are included.
7. A drug carrier, characterized in that The porous microspheres according to claim 4 are included.
8. A cell scaffold, characterized in that: The porous microspheres according to claim 4 are included.