A kind of PET copper foil and preparation method thereof
By performing PVD sputtering or evaporating metal layer on the PET film, combined with acid leach activation and chemical copper deposition technology, passivation treatment was performed using 1-propyltrimethoxysilyl-3-methyl acrylate urea. The problem of uneven corrosion and conductive layer thickness of copper foil in lithium-ion batteries is solved, and efficient preparation of PET copper foil and corrosion resistance is achieved.
Patent Information
- Application Number
- CN202310860484.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-07-13
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-07-13
AI Technical Summary
Existing copper foils are prone to corrosion in lithium-ion batteries, resulting in uneven thickness of the conductive layer and insufficient corrosion resistance, making it difficult to achieve continuous production of more than 10,000 meters. In addition, PVD electroplating technology has problems with leakage plating and electric breakdown when preparing thin layers.
Using PET film to sputter or evaporate metal layer, combined with acid leach activation, electroplating of copper and chemical copper deposition technology, 1-propyltrimethoxysilyl-3-methylacrylate urea as silanization reagent Passivation treatment forms a stable covered silane film, optimizing the surface structure and corrosion resistance of the copper foil.
It significantly improves the corrosion resistance and conductivity of copper foil, solves the problems of uneven thickness of the conductive layer and insufficient corrosion resistance, and realizes efficient preparation of PET copper foil, avoids sputtering breakdown and electroplating defects, and supports more than 10,000 meters. continuous production.
Smart Images

Figure SMS_2 
Figure SMS_6
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of copper foil preparation, and in particular to a PET copper foil and a preparation method thereof. Background Art
[0002] Copper foil is divided into two categories according to the production method: one is electrolytic copper foil and the other is rolled copper foil. Electrolytic copper foil uses electrodeposition to make Cu 2+ Under the action of the electric field force, it migrates and deposits on the cathode to form a thin film. The thickness of the copper foil can be controlled by controlling the deposition time.
[0003] Rolled copper foil is formed by repeatedly rolling copper strips through a forging method. Its bending resistance and mechanical strength are much higher than those of electrolytic copper foil. However, its production process is complicated, and the rolled copper foil is easily affected by work hardening and fatigue strength, which cannot meet market demand and is gradually being replaced by electrolytic copper foil.
[0004] Taking PET composite copper foil as an example, if the traditional 6μm electrolytic copper foil is replaced by 1μm copper foil + 4.5μm PET substrate + 1μm copper foil composite current collector, while ensuring the conductive performance and current collection performance of the conductive layer, the weight of the current collector can be significantly reduced, thereby reducing the overall weight of the battery and improving the battery energy density.
[0005] Whether it is rolled copper foil, electrolytic copper foil, or plastic composite copper foil, as an important component of the current collector of lithium-ion batteries, it is easily corroded by the electrolyte when exposed to the electrolyte for a long time, thereby contaminating the electrolyte and even destroying the anode structure. Therefore, it is necessary to passivate the surface of the copper foil to ensure higher oxidation resistance, heat resistance and corrosion resistance. Silanization treatment technology self-assembles to form a monolayer organic film, which not only has the ability to isolate oxidation, but also enhances the corrosion resistance of the outer surface of the copper foil, which can effectively solve the long-term stability of the outer surface of the copper foil.
[0006] In the existing technology, there are problems with copper plating uniformity, and there is an accumulation of uneven thickness during the winding process (the difference between thick or thin areas relative to the fixed winding is getting bigger and bigger), which leads to wrinkles, and thus it is impossible to achieve continuous production of more than 10,000 meters (a length of more than 10,000 meters is required for later support use). The PVD electroplating method makes it difficult for the equipment to conduct electricity, and is prone to problems such as plating leakage and electrical breakdown. The PVD electroplating method has strict requirements on the previous process PVD when producing thicknesses of 3 microns and below, and it is difficult to achieve mass production.
[0007] CN116230949A discloses a composite copper foil film and a preparation method thereof, wherein the composite copper foil film is composed of a substrate layer and a conductive layer attached to both sides of the substrate layer, wherein the conductive layer includes a metal copper sputtering layer, a metal copper electroplating layer and a protective layer in order from the inside to the outside. The preparation method is: the substrate layer is made of a polyester film with a polyester functional masterbatch added; the surfaces of both sides of the substrate layer are subjected to corona treatment to form a corona layer; a barrier layer is formed on the outside of the corona layer; and the conductive layer is formed on the outside of the barrier layer. The technical solution prepares the composite copper foil film by combining the vacuum sputtering process and the water electroplating process, and can obtain excellent electrical properties and adhesion without destroying the surface structure of the substrate layer.
[0008] There are studies in the prior art that use electrolytic copper foil as a matrix, add CeO2 nanoparticles and Ce(NO3)3 as inhibitors to γ-aminopropyltriethoxysilane (APTES), and perform surface passivation treatment on the electrolytic copper foil, which can effectively improve the oxidation resistance, heat resistance and corrosion resistance of the copper foil. However, this system still has certain problems, such as uneven dispersion of nanoparticles, which affects the corrosion resistance of the film layer; and uneven coverage of the silanized film layer on the surface of the copper foil. Summary of the invention
[0009] In view of the above-mentioned defects of the prior art, the present invention provides a method for preparing PET copper foil, comprising the following steps: PET film→PVD sputtering or evaporation of metal layer→acid immersion activation→copper electroplating→water washing→passivation→water washing→drying;
[0010] The metals of the PVD vacuum sputtering or evaporation metal layer are mainly copper and nickel metals, including: copper, nickel, tin, copper / nickel, nickel / chromium, copper / tin, tin / nickel; the thickness of the PVD vacuum sputtering or evaporation metal layer is 20-70nm, and the square resistance is controlled below 1Ω;
[0011] Acid immersion activation is a process using an acid immersion tank. The acid solution is an aqueous solution with sulfuric acid as the main component, and its main functions are to remove oxidation, wet the metal surface, and protect the electroplating copper tank.
[0012] The electroplating copper is a plating solution of a copper sulfate system (containing 10-20wt% sulfuric acid, 5-20wt% copper sulfate, 30-80ppm chloride ion, and copper plating additives), a copper pyrophosphate system, or an alkaline copper plating system.
[0013] The second object of the present invention is to provide a method for preparing PET copper foil, comprising the following steps: PET film → gluing → drying → catalytic coating → drying → curing → chemical copper deposition → water washing → passivation → water washing → drying;
[0014] Glue lamination: The purpose of surface glue lamination is to increase the roughness of the ET film surface to facilitate the subsequent attachment of the catalyst. The glue composition can be photoresist or nitrile glue.
[0015] Coating catalysis refers to coating catalysts to prepare for the subsequent chemical copper so that copper ions can be replaced. The ingredients are glue, palladium powder or palladium salt (palladium chloride, palladium sulfate, palladium acetate), silver or silver salt;
[0016] Chemical copper is a chemical copper deposition solution based on sodium tartrate system or EDTA system (main components are copper ions, formaldehyde, sodium hydroxide, chelating agent and stabilizer) to quickly deposit a chemical copper layer with a target thickness of about 1μm.
[0017] The third object of the present invention is to provide a method for preparing PET copper foil, comprising the following steps: PET film → PVD sputtering or evaporation of metal layer → cleaning and adjustment → water washing → catalysis → water washing → reduction acceleration → water washing → chemical copper deposition → water washing → passivation → water washing → drying;
[0018] The metals of the PVD vacuum sputtering or evaporation metal layer are mainly copper and nickel metals, including: copper, nickel, tin, copper / nickel, nickel / chromium, copper / tin, tin / nickel and other metals or alloys, and the corresponding metal layer thickness can be 10-30nm, which serves as the basic seed metal; since the traditional method is followed by electroplating, the thickness of the metal layer obtained after PVD is required to be above 30nm; this solution is followed by chemical copper deposition, so the metal layer thickness only needs to be above 10nm, which effectively improves the PVD speed while avoiding the problem of sputtering penetrating the film material;
[0019] Cleaning and adjustment: remove slight oxides and slight stains (such as fingerprints, etc.) on the surface, and adjust the charge of the surface to facilitate the attachment of subsequent catalysts;
[0020] Catalysis is to prepare for the subsequent chemical copper so that copper ions can be replaced. It is a reagent with palladium salts (palladium chloride, palladium sulfate, palladium acetate), silver or silver salts (silver nitrate) as main ingredients; chemical copper is a chemical copper precipitation solution with a sodium tartrate system or an EDTA system (main ingredients are copper ions, formaldehyde, sodium hydroxide, chelating agents and stabilizers) to quickly deposit a chemical copper layer with a target thickness of about 1μm.
[0021] The fourth object of the present invention is to provide a method for preparing PET copper foil, comprising the following steps: PET film → PVD sputtering or evaporation of metal layer → cleaning and adjustment → water washing → catalysis → water washing → reduction acceleration → water washing → chemical copper deposition → water washing → acid immersion activation → electroplating copper → water washing → passivation → water washing → drying;
[0022] The metals of the PVD vacuum sputtering or evaporation metal layer are mainly copper and nickel metals, including: copper, nickel, tin, copper / nickel, nickel / chromium, copper / tin, tin / nickel and other metals or alloys, and the corresponding metal layer thickness can be 10-30nm, which serves as the basic seed metal; since the traditional method is followed by electroplating, the thickness of the metal layer obtained after PVD is required to be above 30nm; this solution is followed by chemical copper deposition, so the metal layer thickness only needs to be above 10nm, which effectively improves the PVD speed while avoiding the problem of sputtering penetrating the film material;
[0023] Cleaning and adjustment: remove slight oxides and slight stains (such as fingerprints, etc.) on the surface, and adjust the charge of the surface to facilitate the attachment of subsequent catalysts;
[0024] Catalysis is to prepare for the subsequent chemical copper so that copper ions can be replaced. It is a reagent with palladium salt (palladium chloride, palladium sulfate, palladium acetate), silver or silver salt (silver nitrate) as the main ingredients;
[0025] Chemical copper is a chemical copper solution based on sodium tartrate system or EDTA system (main components are copper ions, formaldehyde, sodium hydroxide, chelating agent and stabilizer) to quickly deposit a chemical copper layer with a target thickness of about 1μm;
[0026] Acid immersion activation is a process using an acid immersion tank. The acid solution is an aqueous solution with sulfuric acid as the main component, and its main functions are to remove oxidation, wet the metal surface, and protect the electroplating copper tank.
[0027] Electroplating copper is a plating solution of a copper sulfate system (containing 10-20% sulfuric acid, 5-20% copper sulfate, 30-80ppm chloride ion, and some copper plating additives), a copper pyrophosphate system or an alkaline copper plating system.
[0028] Preferably, the passivation comprises stirring and mixing the corrosion inhibitor, surfactant, 1-propyltrimethoxysilyl-3-ethyl methacrylate urea, water and ethanol at room temperature; adjusting the pH to 3-6; sealing and standing for 12-36 hours and then ultrasonicating for 30-90 minutes; obtaining a passivation solution; placing the copper foil in the passivation solution for 10-60 seconds, taking out the copper foil, and dehydrating and curing at 100-110° C. for 30-90 minutes to complete the passivation.
[0029] Preferably, the usage ratio of the corrosion inhibitor, surfactant, 1-propyltrimethoxysilyl-3-ethyl methacrylate urea, water and ethanol is 2-6g:2-6Kg:3-8L:3-8L:84-94L.
[0030] Preferably, the corrosion inhibitor is at least one of cerium nitrate and CeO2 nanoparticles.
[0031] Preferably, the surfactant is coconut oil monoethanolamide. Coconut oil monoethanolamide can effectively disperse CeO2 nanoparticles and reduce the agglomeration of CeO2 nanoparticles; at the same time, coconut oil monoethanolamide contains -NH-, C=O, -OH, which can effectively form hydrogen bonds with 1-propyltrimethoxysilyl-3-ethyl methacrylate urea, thereby effectively fixing it on the surface of copper foil. Furthermore, coconut oil monoethanolamide is not only a surfactant, but also can play a good corrosion inhibition effect when it is fixed on the surface of copper foil.
[0032] The invention also discloses a PET copper foil, which is prepared by the preparation method.
[0033] Beneficial effects of the present invention:
[0034] Compared with the prior art, -NH- and C=O between 1-propyltrimethoxysilyl-3-ethyl methacrylate urea molecules can form stable hydrogen bonds, so that a stable and well-covered silanized film can be formed on the surface of the copper foil. The present invention uses 1-propyltrimethoxysilyl-3-ethyl methacrylate urea to replace 3-aminopropyltriethoxysilane (APTES) as a silanization agent to perform surface passivation treatment on the copper foil, which can effectively improve the corrosion resistance of the copper foil. DETAILED DESCRIPTION
[0035] The parameters of some chemical substances in the examples are as follows:
[0036] 1-propyltrimethoxysilyl-3-methylacrylate ethyl urea, .
[0037] CeO2 nanoparticles, 20nm. Example 1
[0038] A preparation method of PET copper foil: PET film→PVD sputtering or evaporation metal layer→acid immersion activation→copper electroplating→water washing→passivation→water washing→drying;
[0039] PVD sputtering: A PET film with a width of 1000mm and a thickness of 4.5μm is fed into the PVD coating chamber for vacuum sputtering coating. Ar is introduced to adjust the vacuum degree to 0.5Pa, and a Cu target is sputtered. The thickness of both sides is controlled to be 50nm, and the square resistance is controlled to be below 1Ω;
[0040] Acid leaching activation: sent to the acid leaching tank, the acid leaching time is 10s; the acid solution is 50g / L sulfuric acid aqueous solution;
[0041] Electroplating copper: sent into the electroplating tank, electroplating parameters: temperature 25℃, current density 0.6A / dm 2The electroplating time is about 10 minutes, and the thickness of both sides is controlled to be 1.5 μm; the electroplating solution is 15wt% sulfuric acid, 10wt% copper sulfate, 0.1wt% sodium 3-mercapto-1-propanesulfonate, 0.008wt% sodium chloride, and the balance is water;
[0042] Water washing: send to the water washing tank and wash for 10s;
[0043] Passivation: Add 1.0g Ce(NO3)3 and 2.36kg coconut oil monoethanolamide to 5L water and stir to mix evenly; then add 1.5g CeO2 nanoparticles and disperse evenly by ultrasonic; then add 5L 1-propyltrimethoxysilyl-3-ethyl methacrylate urea and 90L ethanol and stir to mix evenly at room temperature for 10min; adjust the pH to 5 with 30wt% glacial acetic acid aqueous solution; seal and let stand for 24h, then ultrasonic for 60min to obtain passivation solution; roll the copper foil into the passivation solution to ensure that the copper foil is in contact with the passivation solution for 30s, and then move it into the drying oven for dehydration and curing at 105℃ for 60min, and the passivation is completed;
[0044] Water washing: send to the water washing tank and wash for 10s;
[0045] Drying: Send to drying oven, drying temperature 105℃. Example 2
[0046] A method for preparing PET copper foil: PET film→gluing→drying→catalytic coating→drying→curing→chemical copper deposition→washing→passivation→washing→drying;
[0047] Laminating: Feed the PET film with a width of 1000mm and a thickness of 4.5μm into the laminating machine and coat 0.05μm nitrile glue on both sides of the PET;
[0048] Drying: sent to the drying oven, drying temperature 105℃;
[0049] Catalytic coating: put into the catalytic pool, temperature 55℃, catalytic time 2min; the catalytic pool is a palladium chloride aqueous solution;
[0050] Drying: sent to the drying oven, drying temperature 105℃;
[0051] Curing: put into drying oven, curing temperature 150℃, curing time 30s;
[0052] Chemical copper deposition: sent into the copper deposition tank, the temperature is 55℃, the copper deposition time is about 28min, and the thickness is controlled to be 1.5μm; the copper plating solution is 7.49g / L copper sulfate, 3mL / L formaldehyde, 6g / L sodium hydroxide, 31.6g / L disodium ethylenediaminetetraacetic acid, 30g / L 2,2'-bipyridine, and the balance is water;
[0053] Water washing: send to the water washing tank and wash for 10s;
[0054] Passivation treatment: add 1.0g Ce(NO3)3 and 2.36kg coconut oil monoethanolamide into 5L water and stir to mix evenly; then add 1.5g CeO2 nanoparticles and disperse evenly by ultrasonic; then add 5L 1-propyltrimethoxysilyl-3-ethyl methacrylate urea and 90L ethanol and stir for 10min at room temperature to mix evenly; adjust the pH to 5 with 30wt% glacial acetic acid aqueous solution; seal and let stand for 24h, then ultrasonic for 60min to obtain passivation solution; send copper foil into the passivation solution, ensure that the copper foil is in contact with the passivation solution for 30s, and then move it into a drying oven for dehydration and curing at 105℃ for 60min, and the passivation is completed;
[0055] Water washing: send to the water washing tank and wash for 10s;
[0056] Drying: Send to drying oven, drying temperature 105℃. Example 3
[0057] A preparation method of PET copper foil: PET film→PVD sputtering→cleaning and adjustment→water washing→catalysis→water washing→reduction acceleration→water washing→chemical copper deposition→water washing→passivation→water washing→drying;
[0058] PVD sputtering: A PET film with a width of 1000mm and a thickness of 4.5μm is fed into the PVD coating chamber for vacuum sputtering coating. Ar is introduced to adjust the vacuum degree to 0.5Pa, and a Cu target is sputtered. The thickness of both sides is controlled to be 20nm, and the square resistance is controlled to be below 1Ω;
[0059] Cleaning adjustment: send to the cleaning pool, temperature 25℃, immersion time 30s; cleaning solution is NaOH 10g / L, sodium dodecyl sulfate 0.1g / L, the balance is water;
[0060] Water washing: send to the water washing tank and wash for 10s;
[0061] Catalysis: sent into the catalytic tank, temperature 35℃, immersion time 5 min; catalytic liquid is 17.7g / L PdCl2 aqueous solution;
[0062] Water washing: send to the water washing tank and wash for 10s;
[0063] Reduction acceleration: put into the reduction tank, temperature 35℃, immersion time 5 min; the reducing agent is 12g / L dimethylamine borane aqueous solution;
[0064] Water washing: send to the water washing tank and wash for 10s;
[0065] Chemical copper deposition: sent into the copper deposition tank, the temperature is 55℃, the copper deposition time is about 28min, and the thickness of both sides is controlled to be 1.5μm; the copper plating solution is 7.49g / L copper sulfate, 3mL / L formaldehyde, 6g / L sodium hydroxide, 31.6g / L disodium ethylenediaminetetraacetic acid, 30g / L 2,2'-bipyridine, and the balance is water;
[0066] Water washing: send to the water washing tank and wash for 10s;
[0067] Passivation treatment: add 1.5g Ce(NO3)3 and 2.36kg coconut oil monoethanolamide into 5L water and stir to mix evenly; then add 1.5g CeO2 nanoparticles and disperse evenly by ultrasonic; then add 5L 1-propyltrimethoxysilyl-3-ethyl methacrylate urea and 90L ethanol and stir for 10min at room temperature to mix evenly; adjust the pH to 5 with 30wt% glacial acetic acid aqueous solution; seal and let stand for 24h, then ultrasonic for 60min to obtain passivation solution; send copper foil into the passivation solution, ensure that the copper foil is in contact with the passivation solution for 30s, and move it into a drying oven for dehydration and curing at 105℃ for 60min, and the passivation is completed;
[0068] Water washing: send to the water washing tank and wash for 10s;
[0069] Drying: Send to drying oven, drying temperature 105℃. Example 4
[0070] A preparation method of PET copper foil: PET film → PVD sputtering or evaporation metal layer → cleaning and adjustment → water washing → catalysis → water washing → reduction acceleration → water washing → chemical copper deposition → water washing → acid immersion activation → electroplating copper → water washing → passivation → water washing → drying;
[0071] PVD sputtering: A PET film with a width of 1000mm and a thickness of 4.5μm is fed into the PVD coating chamber for vacuum sputtering coating. Ar is introduced to adjust the vacuum degree to 0.5Pa, and a Cu target is sputtered. The thickness is controlled to be 20nm, and the square resistance is controlled to be below 1Ω;
[0072] Cleaning adjustment: put into the cleaning pool, temperature 25℃, immersion time 30 s; cleaning solution is NaOH 10g / L, sodium dodecyl sulfate 0.1 g / L, the balance is water;
[0073] Water washing: send to the water washing tank and wash for 10s;
[0074] Catalysis: sent into the catalytic tank, temperature 35℃, immersion time 5 min; catalytic liquid is 17.7g / L PdCl2 aqueous solution;
[0075] Water washing: send to the water washing tank and wash for 10s;
[0076] Reduction acceleration: put into the reduction tank, temperature 35℃, immersion time 5 min; the reducing agent is 12g / L dimethylamine borane aqueous solution;
[0077] Water washing: send to the water washing tank and wash for 10s;
[0078] Chemical copper deposition: sent into the copper deposition tank, the temperature is 55℃, the copper deposition time is about 20min, and the thickness is controlled to be 1μm; the copper plating solution is 7.49g / L copper sulfate, 3mL / L formaldehyde, 6g / L sodium hydroxide, 31.6 g / L disodium ethylenediaminetetraacetic acid, 30g / L 2,2'-bipyridine, and the balance is water;
[0079] Water washing: send to the water washing tank and wash for 10s;
[0080] Acid leaching activation: sent to the acid leaching tank, the acid leaching time is 10s; the acid solution is 50g / L sulfuric acid aqueous solution;
[0081] Electroplating copper: sent into the electroplating tank, electroplating parameters: temperature 25℃, current density 0.6A / dm 2 The electroplating time is about 3 minutes, and the thickness is controlled to be 0.5 μm; the electroplating solution is 15wt% sulfuric acid, 10wt% copper sulfate, 0.1wt% sodium 3-mercapto-1-propanesulfonate, 0.008wt% sodium chloride, and the balance is water;
[0082] Water washing: send to the water washing tank and wash for 10s;
[0083] Passivation treatment: add 1.0gCe(NO3)3 and 2.36kg coconut oil monoethanolamide into 5L water and stir to mix evenly; then add 1.5gCeO2 nanoparticles and disperse evenly by ultrasonic; then add 5L1-propyltrimethoxysilyl-3-ethyl methacrylate urea and 90L ethanol and stir for 10min at room temperature to mix evenly; adjust the pH to 5 with 30wt% glacial acetic acid aqueous solution; seal and let stand for 24h, then ultrasonic for 60min to obtain passivation solution; roll the copper foil into the passivation solution to ensure that the copper foil is in contact with the passivation solution for 30s, and then move it into the drying oven for dehydration and curing at 105℃ for 60min, and the passivation is completed;
[0084] Water washing: send to the water washing tank and wash for 10s;
[0085] Drying: Send to drying oven, drying temperature 105℃.
[0086] Example 5
[0087] A method for preparing a PET copper foil is basically the same as that of Example 4, except that the passivation treatment process is different, as follows:
[0088] Passivation treatment: Add 1.0g Ce(NO3)3 into 5L water and stir to mix evenly; then add 1.5g CeO2 nanoparticles and disperse evenly by ultrasonic; then add 5L 1-propyltrimethoxysilyl-3-ethyl methacrylate urea and 90L ethanol and stir for 10min at room temperature to mix evenly; adjust the pH to 5 with 30wt% glacial acetic acid aqueous solution; seal and let stand for 24h, then ultrasonic for 60min to obtain passivation solution; send copper foil into the passivation solution, ensure that the copper foil is in contact with the passivation solution for 30s, and move it into a drying oven for dehydration and curing at 105℃ for 60min, and the passivation is completed.
[0089] Comparative Example 1
[0090] A method for preparing a PET copper foil is basically the same as that of Example 4, except that the passivation treatment process is different, as follows:
[0091] Passivation treatment: Add 1.0g Ce(NO3)3 into 5mL water and stir to mix evenly; then add 1.5g CeO2 nanoparticles and disperse evenly by ultrasonication; then add 5L 3-aminopropyltriethoxysilane and 90L ethanol and stir to mix evenly at room temperature for 10min; adjust the pH to 5 with 30wt% glacial acetic acid aqueous solution; seal and let stand for 24h, then ultrasonicate for 60min to obtain passivation solution; roll the copper foil into the passivation solution, ensure that the copper foil is in contact with the passivation solution for 30s, and move it into the drying oven for dehydration and curing at 105℃ for 60min, and the passivation is completed. Example 6
[0092] A method for preparing a PET copper foil is basically the same as that of Example 4, except that the passivation treatment process is different, as follows:
[0093] Passivation treatment: Add 1g Ce(NO3)3 and 2kg coconut oil monoethanolamide into 3L water and stir to mix evenly; then add 1g CeO2 nanoparticles and disperse evenly by ultrasonic; then add 3L 1-propyltrimethoxysilyl-3-ethyl methacrylate urea and 94L ethanol and stir for 10min at room temperature to mix evenly; adjust the pH to 5 with 30wt% glacial acetic acid aqueous solution; seal and let stand for 24h, then ultrasonic for 60min to obtain the passivation solution; roll the copper foil into the passivation solution to ensure that the copper foil is in contact with the passivation solution for 20s, and move it into the drying oven for dehydration and curing at 105℃ for 60min, and the passivation is completed. Example 7
[0094] A method for preparing a PET copper foil is basically the same as that of Example 4, except that the passivation treatment process is different, as follows:
[0095] Passivation treatment: Add 3g Ce(NO3)3 and 6kg coconut oil monoethanolamide into 8L water and stir to mix evenly; then add 3g CeO2 nanoparticles and disperse evenly by ultrasonic; then add 8L 1-propyltrimethoxysilyl-3-ethyl methacrylate urea and 84L ethanol and stir for 10min at room temperature to mix evenly; adjust the pH to 5 with 30wt% glacial acetic acid aqueous solution; seal and let stand for 24h, then ultrasonic for 60min to obtain the passivation solution; roll the copper foil into the passivation solution to ensure that the copper foil is in contact with the passivation solution for 60s, and move it into the drying oven for dehydration and curing at 105℃ for 60min, and the passivation is completed.
[0096] Test Example 1
[0097] The copper foils obtained in Examples 4 and 5 and Control Example 1 were subjected to potentiodynamic polarization tests using an electrochemical workstation (CHI660E). The potentiodynamic polarization test is also called the Tafel test. The quantitative relationship between potential and current density can be expressed by the Tafel formula I to reflect the electrode surface reaction kinetics.
[0098] Formula I
[0099] In the formula is the overpotential is the current density A·cm -2 , a and b are constants. Corrosion current (i corr ) and corrosion potential (E corr ) is obtained from the potentiodynamic polarization curve by Tafel extrapolation method. The corrosion potential reflects the difficulty of self-corrosion in the corrosive solution, and the corrosion current reflects the speed of self-corrosion of the copper foil.
[0100] The test parameters set in the experiment were as follows: a three-electrode system was used, the working electrode was a copper foil (1 cm × 1 cm), the counter electrode was a platinum sheet electrode (1.5 cm × 1.5 cm), the reference electrode was a saturated calomel electrode, the test solution was a 3.5 wt% NaCl neutral aqueous solution, the open circuit potential was -0.4 V ~ 0.4 V, and the scan rate was 5 mV·s -1 , the test temperature is 25℃.
[0101] Table 1 Corrosion potential
[0102]
[0103] Note: It is generally believed that the lower the corrosion potential (absolute value), the more likely it is that corrosion will occur; and the corrosion current density is a kinetic parameter. The smaller the corrosion current density, the lower the corrosion rate.
[0104] As can be seen from Table 1, in the preparation method of the PET copper foil of the present invention, the corrosion resistance of the copper foil after the surface passivation treatment of the copper foil using 1-propyltrimethoxysilyl-3-ethyl methacrylate urea as a silanization agent is significantly better than that of the prior art (Comparative Example 1) using 3-aminopropyltriethoxysilane (APTES) as a silanization agent. The reason is that -NH- and C=O between the molecules of 1-propyltrimethoxysilyl-3-ethyl methacrylate urea can form a stable hydrogen bond, so that a stable and well-covered silane film can be formed on the surface of the copper foil. Moreover, in Example 4 of the present invention, a surfactant, coconut oil monoethanolamide, which has corrosion inhibition properties, is added to address the problem of easy agglomeration of CeO2 nanoparticles, which can effectively improve the problems of agglomeration and uneven dispersion of CeO2 nanoparticles; and coconut oil monoethanolamide contains -NH-, C=O, and -OH, which can effectively form hydrogen bonds with 1-propyltrimethoxysilyl-3-ethyl methacrylate urea, thereby effectively fixing it on the surface of copper foil; thereby further improving the corrosion resistance of the copper foil after passivation.
Claims
1. A method for preparing PET copper foil, characterized in that: The process is: PET film → PVD sputtering or evaporation metal layer → acid immersion activation → copper electroplating → water washing → passivation → water washing → drying; The passivation comprises the following steps: uniformly mixing the corrosion inhibitor, the surfactant, 1-propyltrimethoxysilyl-3-ethyl methacrylate urea, water and ethanol at room temperature; adjusting the pH to 3-6; sealing and standing for 12-36 hours and then ultrasonicating for 30-90 minutes; obtaining the passivation solution; placing the copper foil in the passivation solution for 10-60 seconds, taking out the copper foil, and dehydrating and curing at 100-110° C. for 30-90 minutes, and then completing the passivation. The usage ratio of the corrosion inhibitor, surfactant, 1-propyltrimethoxysilyl-3-ethyl methacrylate urea, water, and ethanol is 2-6g: 2-6Kg: 3-8L: 3-8L: 84-94L; The corrosion inhibitor is at least one of cerium nitrate and CeO2 nanoparticles; The surfactant is coconut oil monoethanolamide.
2. A method for preparing PET copper foil, characterized in that: The process is: PET film → lamination → drying → catalytic coating → drying → curing → chemical copper deposition → water washing → passivation → water washing → drying; The passivation comprises the following steps: uniformly mixing the corrosion inhibitor, the surfactant, 1-propyltrimethoxysilyl-3-ethyl methacrylate urea, water and ethanol at room temperature; adjusting the pH to 3-6; sealing and standing for 12-36 hours and then ultrasonicating for 30-90 minutes; obtaining the passivation solution; placing the copper foil in the passivation solution for 10-60 seconds, taking out the copper foil, and dehydrating and curing at 100-110° C. for 30-90 minutes, and then completing the passivation. The usage ratio of the corrosion inhibitor, surfactant, 1-propyltrimethoxysilyl-3-ethyl methacrylate urea, water, and ethanol is 2-6g: 2-6Kg: 3-8L: 3-8L: 84-94L; The corrosion inhibitor is at least one of cerium nitrate and CeO2 nanoparticles; The surfactant is coconut oil monoethanolamide.
3. A method for preparing PET copper foil, characterized in that: The process is: PET film → PVD sputtering or evaporation metal layer → cleaning and adjustment → water washing → catalysis → water washing → reduction acceleration → water washing → chemical copper deposition → water washing → passivation → water washing → drying; The passivation comprises the following steps: uniformly mixing the corrosion inhibitor, the surfactant, 1-propyltrimethoxysilyl-3-ethyl methacrylate urea, water and ethanol at room temperature; adjusting the pH to 3-6; sealing and standing for 12-36 hours and then ultrasonicating for 30-90 minutes; obtaining the passivation solution; placing the copper foil in the passivation solution for 10-60 seconds, taking out the copper foil, and dehydrating and curing at 100-110° C. for 30-90 minutes, and then completing the passivation. The usage ratio of the corrosion inhibitor, surfactant, 1-propyltrimethoxysilyl-3-ethyl methacrylate urea, water, and ethanol is 2-6g: 2-6Kg: 3-8L: 3-8L: 84-94L; The corrosion inhibitor is at least one of cerium nitrate and CeO2 nanoparticles; The surfactant is coconut oil monoethanolamide.
4. A method for preparing PET copper foil, characterized in that: The process is: PET film → PVD sputtering or evaporation metal layer → cleaning and adjustment → water washing → catalysis → water washing → reduction acceleration → water washing → chemical copper deposition → water washing → acid immersion activation → electroplating copper → water washing → passivation → water washing → drying; The passivation comprises the following steps: uniformly mixing the corrosion inhibitor, the surfactant, 1-propyltrimethoxysilyl-3-ethyl methacrylate urea, water and ethanol at room temperature; adjusting the pH to 3-6; sealing and standing for 12-36 hours and then ultrasonicating for 30-90 minutes; obtaining the passivation solution; placing the copper foil in the passivation solution for 10-60 seconds, taking out the copper foil, and dehydrating and curing at 100-110° C. for 30-90 minutes, and then completing the passivation. The usage ratio of the corrosion inhibitor, surfactant, 1-propyltrimethoxysilyl-3-ethyl methacrylate urea, water, and ethanol is 2-6g: 2-6Kg: 3-8L: 3-8L: 84-94L; The corrosion inhibitor is at least one of cerium nitrate and CeO2 nanoparticles; The surfactant is coconut oil monoethanolamide.
5. A PET copper foil, characterized in that: Prepared by the method described in any one of claims 1 to 4.
6. A passivation solution for copper foil surface treatment, characterized in that: The method is prepared by the following method: a corrosion inhibitor, a surfactant, 1-propyltrimethoxysilyl-3-ethyl methacrylate urea, water and ethanol are stirred and mixed uniformly at room temperature; the pH is adjusted to 3-6; a passivation solution is obtained after being sealed and allowed to stand for 12-36 hours and then ultrasonicated for 30-90 minutes; a copper foil is placed in the passivation solution for 10-60 seconds, the copper foil is taken out, and dehydrated and cured at 100-110° C. for 30-90 minutes to complete the passivation; The usage ratio of the corrosion inhibitor, surfactant, 1-propyltrimethoxysilyl-3-ethyl methacrylate urea, water, and ethanol is 2-6g: 2-6Kg: 3-8L: 3-8L: 84-94L; The corrosion inhibitor is at least one of cerium nitrate and CeO2 nanoparticles; The surfactant is coconut oil monoethanolamide.