Silver paste for medium-temperature sintering ceramic filter and preparation method thereof
By using a combination of 72-80% conductive silver powder, 3-11% glass powder and 12-19% organic carrier in a ceramic filter, combining a mixing technique of spherical and sheet silver powder, high adhesion and conductivity are formed at medium temperatures. The silver film solves the problem of high sintering temperature of existing ceramic filters, and realizes the high-efficiency medium-temperature sintering and improved conductivity of ceramic filters.
Patent Information
- Application Number
- CN202311058610.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-22
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2043-08-22
AI Technical Summary
The high sintering temperature of the existing ceramic filters leads to an increase in industrial costs and adversely affecting the ceramic materials, and it is difficult to achieve silver film formation with high adhesion and electrical conductivity at medium temperatures.
Using a combination of 72-80% conductive silver powder, 3-11% glass powder and 12-19% organic carrier, the wetting properties of the glass powder and the high sintering activity of the conductive silver powder are used to mix spherical silver powder and sheet silver powder. Sintered at 600-700°C to form a dense silver film.
It effectively reduces the sintering temperature of the silver paste, improves the adhesion and conductivity of the silver film, reduces the silver powder content, and enhances the density and brightness of the silver film on the surface of the ceramic matrix.
Smart Images

Figure CN116994795B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electronic pastes, and in particular relates to a silver paste for medium-temperature sintering ceramic filters and a preparation method thereof. Background Art
[0002] Since ceramics are not conductive, metallization is a key technology for the proper functioning of ceramic filters. Silver is used as an electrode material for ceramic filters due to its high conductivity, thermal stability, and weldability. Many metallization techniques can be used to coat ceramics, including screen printing, low-temperature co-fired ceramics, ball milling, magnetron sputtering, and chemical plating. Screen printing is the most commonly used method for metallization of ceramic surfaces. In this method, silver paste is applied to the ceramic surface and sintered to form a silver coating.
[0003] However, the current sintering temperature of silver paste is above 850°C or even higher. Higher sintering temperature not only increases industrial costs, but also affects the properties of the ceramic itself. High temperature tends to promote grain growth and increase the porosity of the ceramic material itself. Larger grains and more porosity have an impact on the thermal shock resistance, dielectric properties, and mechanical properties of ceramics. In order to reduce industrial costs and reduce the impact of the sintering temperature of silver paste on the ceramic itself. It is very necessary to develop a slurry that is sintered at medium temperature (600-700°C) and has good matching with the substrate, good conductivity, high adhesion, and high sintering densification. It is a special silver paste for 5G ceramic filter surface metallization. Summary of the invention
[0004] In view of the above-mentioned shortcomings of the prior art, the present invention provides a silver paste for medium-temperature sintering ceramic filters and a preparation method thereof.
[0005] To achieve the above object, the technical solution adopted by the present invention is: a silver paste for medium temperature sintering ceramic filter, comprising the following components in percentage by weight: 72-80% conductive silver powder, 3-11% glass powder and 12-19% organic carrier; the glass powder comprises the following components in percentage by weight: 40-52% Bi 2 O 3 20-30% B 2 O 3 10-15% SiO 2 , 7-9% ZnO, 1-3% Al 2 O 3 , 2-3% CaO, 3%-5% BaO; the conductive silver powder includes spherical silver powder and flaky silver powder, and the weight percentage of the flaky silver powder in the conductive silver powder is 3-10%.
[0006] As a preferred embodiment of the present invention, the silver paste for medium-temperature sintering ceramic filter includes the following components in percentage by weight: 75% conductive silver powder, 8% glass powder and 17% organic vehicle.
[0007] As a preferred embodiment of the present invention, the glass powder comprises the following components in percentage by weight: 49% Bi 2 O 3 24% B 2 O 3 、12%SiO 2 、7% ZnO、2% Al 2 O 3 , 2%CaO, 4%BaO.
[0008] As a preferred embodiment of the present invention, the weight percentage of the flaky silver powder in the conductive silver powder is 5%.
[0009] As a preferred embodiment of the present invention, the particle size of the flaky silver powder is 5-9 μm, and the specific surface area is 0.5-0.8 m 2 / g; the surface of the spherical silver powder is formed by nano-scale silver powder clusters, has high sintering activity, the particle size of the spherical silver powder is 1-1.5μm, and the specific surface area is 1.7-2.9m 2 / g.
[0010] The present invention mixes spherical silver powder with a large specific surface area and a high surface activity formed by nano-scale silver particle clusters on the surface with flaky silver powder with a small bulk density, so that the silver powder with a high energy state and high sintering activity can be sintered into a film at a lower temperature, effectively reducing the silver powder content and greatly reducing the sintering temperature. In addition, the present invention utilizes the wettability of glass powder to promote the sintering of the silver film layer, and the two silver films fully fill the gaps in the sintering process, which is more conducive to obtaining a dense conductive network. The addition of flaky silver powder can improve the anti-sedimentation performance of the silver paste, and after sintering, the brightness of the silver film layer on the surface of the ceramic substrate can be improved.
[0011] As a preferred embodiment of the present invention, the glass powder has a softening temperature of 500-520°C.
[0012] As a preferred embodiment of the present invention, the average particle size of the glass powder is ≤3 μm.
[0013] As a preferred embodiment of the present invention, the organic carrier is composed of the following components in percentage by mass: 79% to 89% organic solvent, 9% to 19% thickener, and 2% surfactant.
[0014] More preferably, the organic carrier is composed of the following components in percentage by weight: 86% organic solvent, 12% thickener, and 2% surfactant.
[0015] As a preferred embodiment of the present invention, the organic solvent is one or two of dibutyl phthalate, terpineol, isopropyl alcohol, petroleum ether, and epoxy resin.
[0016] As a preferred embodiment of the present invention, the thickener is ethyl cellulose and / or polyisobutylene.
[0017] As a preferred embodiment of the present invention, the surfactant is toluene and / or ethanol.
[0018] As a preferred embodiment of the present invention, the method for preparing the organic carrier comprises: placing an organic solvent and a surfactant in a water bath to completely dissolve them to obtain an organic carrier.
[0019] As a preferred embodiment of the present invention, the temperature of the water bath is 60°C-80°C.
[0020] As a preferred embodiment of the present invention, the sintering temperature of the silver paste for medium-temperature sintering ceramic filter is 600-670°C.
[0021] The present invention also claims a method for preparing the silver paste for the medium-temperature sintered ceramic filter, comprising the following steps:
[0022] (1) preparing raw materials according to the composition of glass powder, mixing them uniformly, drying them, and then melting them to obtain glass liquid, quenching the glass liquid with water to obtain glass slag, and then successively ball milling, drying, and sieving to obtain glass powder;
[0023] (2) The organic carrier, the conductive silver powder and the glass powder are uniformly mixed and then ground to obtain a silver paste for medium-temperature sintering ceramic filter with a fineness of ≤5 μm.
[0024] Compared with the prior art, the beneficial effects of the present invention are as follows: on the one hand, the present invention adds CaO to the glass powder, and reacts with other glass powder components to obtain glass powder with perfect comprehensive performance, uniform particle size distribution and expansion coefficient matching the ceramic dielectric filter substrate, so that the prepared silver paste has a lower sintering temperature and high adhesion to the substrate. On the other hand, spherical silver powder and flaky silver powder are mixed so that the silver powder is sintered into a film at a lower temperature, which effectively reduces the silver powder content and greatly reduces the sintering temperature of the silver paste to 600-670°C, while improving the adhesion of the silver paste to the substrate and enhancing the conductivity. In addition, the present invention compounds conductive silver powder, glass powder and organic carrier to jointly achieve the purpose of reducing the sintering temperature of the silver paste, while making the silver paste have high adhesion and conductivity on the ceramic substrate. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is the surface morphology of spherical silver powder.
[0026] Figure 2 Schematic diagram of the wetting angle of the glass powder prepared in Example 2 after sintering.
[0027] Figure 3This is a scanning electron microscope image of the medium-temperature sintered ceramic filter prepared in Example 1 after sintering with silver paste.
[0028] Figure 4 This is a scanning electron microscope image of the medium-temperature sintered ceramic filter prepared in Example 2 after sintering with silver paste.
[0029] Figure 5 This is a scanning electron microscope image of the medium-temperature sintered ceramic filter prepared in Example 3 after sintering with silver paste. DETAILED DESCRIPTION
[0030] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments.
[0031] Example 1
[0032] A silver paste for medium-temperature sintering ceramic filter comprises the following components in percentage by weight: 80% conductive silver powder, 3% glass powder and 17% organic carrier.
[0033] The glass powder includes the following components in percentage by weight: 40% Bi 2 O 3 30% B 2 O 3 、10%SiO 2 , 9% ZnO, 3% Al 2 O 3 , 3%CaO, 5%BaO.
[0034] The conductive silver powder is composed of 97% by weight of spherical silver powder and 3% by weight of flaky silver powder; the particle size of the flaky silver powder is 9 μm and the specific surface area is 0.5 m 2 / g; the surface of the spherical silver powder is formed by nano-scale silver powder clusters, the spherical silver powder particle size is 1.5μm, and the specific surface area is 1.7m 2 / g.
[0035] The organic carrier is composed of the following components in percentage by mass: 79% terpineol, 19% ethyl cellulose and 2% toluene.
[0036] The method for preparing the silver paste for the medium-temperature sintered ceramic filter comprises the following steps:
[0037] (1) preparing raw materials according to the composition of glass powder, using ultrasonic oscillation for 0.5 h to fully disperse and mix the raw material powder particles, then using a magnetic stirrer at a speed of 300 r / min to mix for 1 h, drying at 80° C. for 5 h, and then melting in a box-type resistance furnace to obtain glass liquid, quenching the glass liquid with water, drying for 8 h to obtain glass slag, and then putting it into a planetary ball mill for 12 h, the ball mill speed is 300 r / min, and after ball milling, putting it into a constant temperature drying oven at 80° C. for 10 h, and sieving to obtain glass powder with an average particle size of ≤3 μm;
[0038] (2) The organic solvent and the surfactant are completely dissolved in a 60° C. water bath, then cooled to room temperature, and sealed for storage to obtain an organic carrier.
[0039] (3) The organic carrier, the conductive silver powder and the glass powder are placed in a mortar, and after being fully wetted, they are fully mixed and ground by a three-roll mill to obtain a silver paste for medium-temperature sintered ceramic filters with a fineness of ≤5 μm.
[0040] The scanning electron microscope image of the silver paste for the medium-temperature sintered ceramic filter prepared in this embodiment sintered at 670°C on the ceramic sheet is as follows: Figure 3 As shown, it can be seen from the figure that the sintering of the silver layer is not completely uniform and dense.
[0041] Example 2
[0042] A silver paste for medium-temperature sintering ceramic filter comprises the following components in percentage by weight: 75% conductive silver powder, 8% glass powder and 17% organic carrier.
[0043] The glass powder includes the following components in percentage by weight: 49% Bi 2 O 3 24% B 2 O 3 、12%SiO 2 、7% ZnO、2% Al 2 O 3 , 2%CaO, 4%BaO.
[0044] The conductive silver powder is composed of 95% by weight of spherical silver powder and 5% by weight of flaky silver powder; the particle size of the flaky silver powder is 5 μm and the specific surface area is 0.8 m 2 / g; the surface of the spherical silver powder is formed by nano-scale silver powder clusters, the particle size of the spherical silver powder is 1 μm, and the specific surface area is 2.9m 2 / g.
[0045] The organic carrier is composed of the following components in percentage by mass: 86% of dibutyl phthalate, 12% of ethyl cellulose and polyisobutylene, and 2% of ethanol.
[0046] The method for preparing the silver paste for the medium-temperature sintered ceramic filter comprises the following steps:
[0047] (1) preparing raw materials according to the composition of glass powder, using ultrasonic oscillation for 0.5 h to fully disperse and mix the raw material powder particles, then using a magnetic stirrer at a speed of 300 r / min to mix for 1 h, drying at 80° C. for 5 h, and then melting in a box-type resistance furnace to obtain glass liquid, quenching the glass liquid with water, drying for 8 h to obtain glass slag, and then putting it into a planetary ball mill for 12 h, the ball mill speed is 300 r / min, and after ball milling, putting it into a constant temperature drying oven at 80° C. for 10 h, and sieving to obtain glass powder with an average particle size of ≤3 μm;
[0048] (2) The organic solvent and the surfactant are completely dissolved in a 60° C. water bath, then cooled to room temperature, and sealed for storage to obtain an organic carrier.
[0049] (3) The organic carrier, the conductive silver powder and the glass powder are placed in a mortar, and after being fully wetted, they are fully mixed and ground by a three-roll mill to obtain a silver paste for medium-temperature sintered ceramic filters with a fineness of ≤5 μm.
[0050] The scanning electron microscope image of the silver paste for the medium-temperature sintered ceramic filter prepared in this embodiment sintered at 670°C on the ceramic sheet is as follows: Figure 4 As shown in the figure, it can be seen that the silver layer after sintering is completely densified, the silver particles melt and grow, and are completely connected together. And the silver paste does not show any warping or cracking after sintering.
[0051] Example 3
[0052] A silver paste for medium-temperature sintering ceramic filter comprises the following components in percentage by weight: 72% conductive silver powder, 11% glass powder and 17% organic carrier.
[0053] The glass powder includes the following components in percentage by weight: 52% Bi 2 O 3 , 20% B 2 O 3 、15%SiO 2 、7% ZnO、1% Al 2 O 3 , 2%CaO, 3%BaO.
[0054] The conductive silver powder is composed of 90% by weight of spherical silver powder and 10% by weight of flaky silver powder; the particle size of the flaky silver powder is 5 μm and the specific surface area is 0.8 m 2 / g; the surface of the spherical silver powder is formed by nano-scale silver powder clusters, the particle size of the spherical silver powder is 1 μm, and the specific surface area is 2.9m 2 / g.
[0055] The organic carrier is composed of the following components in percentage by mass: 89% isopropyl alcohol and epoxy resin, 9% polyisobutylene, and 2% ethanol and toluene.
[0056] The method for preparing the silver paste for the medium-temperature sintered ceramic filter comprises the following steps:
[0057] (1) preparing raw materials according to the composition of glass powder, using ultrasonic oscillation for 0.5 h to fully disperse and mix the raw material powder particles, then using a magnetic stirrer at a speed of 300 r / min to mix for 1 h, drying at 80° C. for 5 h, and then melting in a box-type resistance furnace to obtain glass liquid, quenching the glass liquid with water, drying for 8 h to obtain glass slag, and then putting it into a planetary ball mill for 12 h, the ball mill speed is 300 r / min, and after ball milling, putting it into a constant temperature drying oven at 80° C. for 10 h, and sieving to obtain glass powder with an average particle size of ≤3 μm;
[0058] (2) The organic solvent and the surfactant are completely dissolved in a 60° C. water bath, then cooled to room temperature, and sealed for storage to obtain an organic carrier.
[0059] (3) The organic carrier, the conductive silver powder and the glass powder are placed in a mortar, and after being fully wetted, they are fully mixed and ground by a three-roll mill to obtain a silver paste for medium-temperature sintered ceramic filters with a fineness of ≤5 μm.
[0060] The scanning electron microscope image of the silver paste for the medium-temperature sintered ceramic filter prepared in this embodiment sintered at 670°C on the ceramic sheet is as follows: Figure 5 As shown in the figure, it can be seen that the silver layer is completely densified after sintering, but there are still holes and a few defects.
[0061] Comparative Example 1
[0062] A silver paste for medium-temperature sintering ceramic filter comprises the following components in percentage by weight: 72% conductive silver powder, 11% glass powder and 17% organic carrier.
[0063] The glass powder includes the following components in percentage by weight: 52% Bi 2 O 3 23% B 2 O 3 、15%SiO 2 、7% ZnO、1% Al 2 O 3 、3%BaO.
[0064] The conductive silver powder and organic carrier are the same as those in Example 3.
[0065] The preparation method of the silver paste for medium-temperature sintering ceramic filter is the same as that in Example 3.
[0066] The silver paste prepared in this comparative example cannot fully wet the silver powder and promote sintering when sintered at 670°C, which leads to a sharp decline in the comprehensive properties of the silver paste, such as resistivity and adhesion. Therefore, it is necessary to sinter on a ceramic sheet at 840°C, but the surface roughness of the silver film after sintering is relatively high, and the formed silver film is not dense enough, which affects the conductive properties of the silver paste.
[0067] Comparative Example 2
[0068] A silver paste for medium-temperature sintering ceramic filter comprises the following components in percentage by weight: 72% conductive silver powder, 11% glass powder and 17% organic carrier.
[0069] The glass powder includes the following components in percentage by weight: 47% Bi 2 O 3 , 20% B 2 O 3 、15%SiO 2 、7% ZnO、1% Al 2 O 3 , 2%CaO, 3%BaO, 5%K 2 O.
[0070] The conductive silver powder and organic carrier are the same as those in Example 3.
[0071] The preparation method of the silver paste for medium-temperature sintering ceramic filter is the same as that in Example 3.
[0072] The silver paste prepared in this comparative example cannot fully wet the silver powder and promote sintering when sintered at 670°C, which leads to a sharp decline in the comprehensive properties of the silver paste, such as resistivity and adhesion. Therefore, the silver paste prepared in this comparative example needs to be sintered at 920°C, but the surface flatness of the sintered silver film on the ceramic sheet is not enough. Under 3000 times SEM, it is observed that there are many glass particles floating on the surface of the silver film, which affects the conductivity of the silver film.
[0073] Comparative Example 3
[0074] A silver paste for medium-temperature sintering ceramic filter comprises the following components in percentage by weight: 72% conductive silver powder, 11% glass powder and 17% organic carrier.
[0075] The glass powder and conductive silver powder are the same as those in Example 3.
[0076] The organic carrier is composed of the following components in percentage by mass: 89% isopropyl alcohol and epoxy resin, 9% polyisobutylene, and 2% xylene.
[0077] The preparation method of the silver paste for medium-temperature sintering ceramic filter is the same as that in Example 3.
[0078] The silver paste prepared in this comparative example cannot fully wet the silver powder and cannot promote sintering when sintered at 670°C, which leads to a sharp decline in the comprehensive properties of the silver paste, such as resistivity and adhesion. Therefore, the silver paste prepared in this comparative example needs to be sintered on ceramics at 880°C, but because the organic carrier used in this comparative example is not wettable enough, the components cannot be fully wetted and dispersed during the preparation of the silver paste, and the comprehensiveness of the obtained silver paste is poor. When screen printing is performed, the printability of the silver paste and the leveling performance of the silver paste on ceramics are poor.
[0079] Comparative Example 4
[0080] A silver paste for medium-temperature sintering ceramic filter comprises the following components in percentage by weight: 72% conductive silver powder, 11% glass powder and 17% organic carrier.
[0081] The glass powder and conductive silver powder are the same as those in Example 3.
[0082] The organic carrier is composed of the following components in percentage by mass: 89% isopropanol and epoxy resin, 9% polyisobutylene, and 2% triethanolamine.
[0083] The preparation method of the silver paste for medium-temperature sintering ceramic filter is the same as that in Example 3.
[0084] The silver paste prepared in this comparative example cannot fully wet the silver powder and cannot promote sintering when sintered at 670°C, which leads to a sharp decline in the comprehensive properties of the silver paste, such as resistivity and adhesion. Therefore, the silver paste prepared in this comparative example needs to be sintered on ceramics at 820°C, but due to the high viscosity of the organic carrier used in this comparative example, it is difficult to wet and disperse the silver powder, resulting in excessive viscosity of the prepared silver paste. When screen printing, the silver paste is difficult to pass through the screen, and the printed silver film has obvious screen printing, and the comprehensive performance of the silver film after sintering is poor.
[0085] Comparative Example 5
[0086] A silver paste for medium-temperature sintering ceramic filter comprises the following components in percentage by weight: 72% conductive silver powder, 11% glass powder and 17% organic carrier.
[0087] The glass powder and conductive silver powder are the same as those in Example 3.
[0088] The organic carrier is composed of the following components in percentage by mass: 86% isopropyl alcohol and epoxy resin, 9% polyisobutylene, 2% ethanol and toluene, and 3% hydrogenated castor oil.
[0089] The preparation method of the silver paste for medium-temperature sintering ceramic filter is the same as that in Example 3.
[0090] The silver paste prepared in this comparative example cannot fully wet the silver powder and promote sintering when sintered at 670°C, which leads to a sharp decline in the comprehensive properties of the silver paste, such as resistivity and adhesion. Therefore, the silver paste prepared in this comparative example needs to be sintered on ceramics at 850°C, but since the viscosity of the organic carrier in this comparative example is too low, the fluidity of the silver paste is relatively strong, and the silver film after screen printing has serious edge expansion behavior, which affects the comprehensive performance of the product.
[0091] Comparative Example 6
[0092] A silver paste for medium-temperature sintering ceramic filter comprises the following components in percentage by weight: 72% conductive silver powder, 11% glass powder and 17% organic carrier.
[0093] The glass powder and organic carrier are the same as those in Example 3.
[0094] The conductive silver powder is spherical silver powder, the surface of which is formed by nano-scale silver powder clusters, the particle size of the spherical silver powder is 1 μm, and the specific surface area is 2.9 m 2 / g.
[0095] The preparation method of the silver paste for medium-temperature sintering ceramic filter is the same as that in Example 3.
[0096] The silver paste prepared in this comparative example cannot fully wet the silver powder and promote sintering when sintered at 670°C, which leads to a sharp decline in the comprehensive properties of the silver paste, such as resistivity and adhesion. Therefore, the silver paste prepared in this comparative example needs to be sintered on ceramics at 850°C, but a large number of unevenly dispersed holes are observed in the sintered silver film under 3000 times SEM. The holes are uneven in size and dispersed throughout the silver film, and a large amount of glass floats to the surface. Under excessive glass, the silver film does not form an effective connection, and there are defects such as holes, pores, and glass on the surface.
[0097] Comparative Example 7
[0098] A silver paste for medium-temperature sintering ceramic filter comprises the following components in percentage by weight: 72% conductive silver powder, 11% glass powder and 17% organic carrier.
[0099] The glass powder and organic carrier are the same as those in Example 3.
[0100] The conductive silver powder is flaky silver powder, the particle size of the flaky silver powder is 5 μm, and the specific surface area is 0.8 m 2 / g.
[0101] The preparation method of the silver paste for medium-temperature sintering ceramic filter is the same as that in Example 3.
[0102] The silver paste prepared in this comparative example cannot fully wet the silver powder and promote sintering when sintered at 670°C, which leads to a sharp decline in the comprehensive properties of the silver paste, such as resistivity and adhesion. Therefore, the sintering temperature of the silver paste prepared in this comparative example is 870°C, but a large number of holes and laminated structures are observed in the sintered silver film under 3000 times SEM, which affects the conductivity of the silver film. When the cross section of the silver film is observed at 8000-12000 times, the silver film and the substrate are not completely bonded, there are a large number of pores and gaps, and there are a large number of holes in the silver film layer, and the sintering is not dense.
[0103] Comparative Example 8
[0104] A silver paste for medium-temperature sintering ceramic filter comprises the following components in percentage by weight: 72% conductive silver powder, 11% glass powder and 17% organic carrier.
[0105] The glass powder and organic carrier are the same as those in Example 3.
[0106] The conductive silver powder is composed of 10% by weight of spherical silver powder and 90% by weight of flaky silver powder; the particle size of the flaky silver powder is 5 μm, and the specific surface area is 0.8 m 2 / g; the surface of the spherical silver powder is formed by nano-scale silver powder clusters, the particle size of the spherical silver powder is 1 μm, and the specific surface area is 2.9m 2 / g.
[0107] The preparation method of the silver paste for medium-temperature sintering ceramic filter is the same as that in Example 3.
[0108] The silver paste prepared in this comparative example cannot fully wet the silver powder and cannot promote sintering when sintered at 670°C, which leads to a sharp drop in the comprehensive properties of the silver paste, such as resistivity and adhesion. Therefore, the silver paste prepared in this comparative example needs to be sintered on ceramics at 900°C, but the sintered silver film is observed to have pores and laminations at 3000-6000 times SEM, and some nanosilver grains exist on the surface and in the gaps, and dense sintering is not achieved. And at 8000-14000 times SEM, it was observed that there was an obvious gap between the cross section of the silver film and the substrate, and the sintering of the silver layer had defects such as holes, resulting in poor comprehensive performance of the silver film.
[0109] The results of the conductivity, adhesion, density, sintering temperature and wetting angle of the silver paste for medium-temperature sintered ceramic filters obtained in Examples 1-3 and Comparative Examples 1-8 are shown in Table 1.
[0110] Table 1
[0111]
[0112]
[0113] According to Comparative Examples 1, 2 and Example 3, the lack of CaO in Comparative Example 1 leads to poor wetting effect of glass powder and unstable glass structure, and the glass transition temperature is too high, thus causing the silver paste to be 3 The ceramic substrate cannot be well connected, and the silver paste is sintered on the MgTiO 3 The temperature on the ceramic filter is too high at 840°C. The present invention adds CaO to the glass to increase the density of the glass and effectively reduce the viscosity of the glass, which is beneficial to the MgTiO 3 Application of medium temperature sintering on ceramic filters. However, adding K 2 O and other first group oxides will cause the transition temperature of the glass to become higher, the thermal properties of the glass to be poor, the glass cannot fully wet the silver powder at medium temperature, and cannot play a good connecting role, resulting in poor performance.
[0114] According to the comparison between Comparative Examples 3 and 4 and Example 3, toluene and / or ethanol surfactants can reduce the interaction force between particles, make the fluidity of silver powder stronger, reduce viscosity, reduce sintering temperature, and enhance the bonding between silver paste and MgTiO 3 The adhesion and conductivity of the ceramic substrate, as well as the density and wettability, are greatly improved. However, the surfactants xylene or triethanolamine will affect the viscosity and rheology of the silver paste, reducing the overall performance of the silver paste.
[0115] According to Example 3 and Comparative Example 5, adding a thixotropic agent to the silver paste system of the present invention will cause the prepared silver paste to be 3 The sintering temperature on the ceramic substrate is significantly increased, and the adhesion, conductivity, density and wettability on the substrate are significantly reduced. This is mainly because the addition of the thixotropic agent causes the silver paste system to lose fluidity, increasing the viscosity of the paste, deteriorating the dispersion of the silver particles, failing to form an effective connection, and deteriorating the sintering performance.
[0116] According to the comparison between Comparative Examples 6-8 and Example 3, it can be seen that using only spherical silver powder or flake silver powder will cause the thermal expansion coefficient of the glass powder to be similar to that of MgTiO 3 The ceramic substrate does not match, resulting in many defects in the sintered silver film. In addition, the glass softening temperature is too high, and the glass powder and MgTiO 3 The wettability of the ceramic substrate is poor, which in turn affects the medium-temperature sintering performance of the material. However, the present invention compounds spherical silver powder and flaky silver powder. Since the nanoparticles promote the refinement of microcracks and subgrain boundaries in the micron particles, the degree of sintering densification is significantly improved, the uniformity of the structure is improved, and the mechanical properties of the silver film are increased. The present invention utilizes the high sintering activity of the mixed silver powder and cooperates with glass powder to achieve medium-temperature sintering of the silver film. After medium-temperature sintering, the silver film is densified and has good bonding with the MgTiO3 ceramic substrate.
[0117] However, according to the comparison between Comparative Example 8 and Example 3, the ratio of spherical silver powder to flake silver powder is crucial. Since the flake silver powder plays a supporting role in the silver network, the spherical silver powder plays a connecting role in the flake silver powder, and the free nano silver particles act as a connecting bridge, compounding the spherical silver powder and the flake silver powder can reduce the sintering temperature and promote the interconnection of the silver powder. When the weight percentage of the flake silver powder in the conductive silver powder is not within the range of 3-10%, the silver paste cannot achieve medium-temperature sintering.
[0118] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A silver paste for medium temperature sintering ceramic filter, characterized in that: The invention comprises the following components in percentage by weight: 72-80% conductive silver powder, 3-11% glass powder and 12-19% organic carrier; the glass powder is composed of the following components in percentage by weight: 40-52% Bi2O3, 20-30% B2O3, 10-15% SiO2, 7-9% ZnO, 1-3% Al2O3, 2-3% CaO and 3%-5% BaO; the conductive silver powder is composed of spherical silver powder and flaky silver powder; the weight percentage of flaky silver powder in the conductive silver powder is 3-10%; the sintering temperature of the silver paste is 600-670°C.
2. The silver paste for medium temperature sintering ceramic filter according to claim 1, characterized in that: The particle size of the flaky silver powder is 5-9 μm, and the specific surface area is 0.5-0.8 m 2 / g; the surface of the spherical silver powder is formed by nano-scale silver powder clusters, has high sintering activity, the particle size of the spherical silver powder is 1-1.5 μm, and the specific surface area is 1.7-2.9 m 2 / g.
3. The silver paste for medium temperature sintering ceramic filter according to claim 1, characterized in that: The softening temperature of the glass powder is 500-520°C.
4. The silver paste for medium temperature sintering ceramic filter according to claim 1, characterized in that: The average particle size of the glass powder is ≤3 μm.
5. The silver paste for medium temperature sintering ceramic filter according to claim 1, characterized in that: The organic carrier is composed of the following components in percentage by mass: 79% to 89% of an organic solvent, 9% to 19% of a thickener and 2% of a surfactant.
6. The silver paste for medium temperature sintering ceramic filter according to claim 5, characterized in that: The organic solvent is one or two of dibutyl phthalate, terpineol, isopropyl alcohol, petroleum ether and epoxy resin.
7. The silver paste for medium temperature sintering ceramic filter according to claim 5, characterized in that: The thickener is ethyl cellulose and / or polyisobutylene.
8. The silver paste for medium temperature sintering ceramic filter according to claim 5, characterized in that: The surfactant is toluene and / or ethanol.
9. The method for preparing the silver paste for medium temperature sintering ceramic filter according to any one of claims 1 to 8, characterized in that: The steps include: (1) preparing raw materials according to the composition of glass powder, mixing them uniformly, drying them, and then melting them to obtain glass liquid, quenching the glass liquid with water to obtain glass slag, and then successively ball milling, drying, and sieving to obtain glass powder; (2) The organic carrier, the conductive silver powder and the glass powder are mixed evenly, and then ground to obtain a silver paste for medium-temperature sintering ceramic filters with a fineness of ≤5 μm.