A method for preparing modified light calcium carbonate from phosphogypsum

Through the dissolution of phosphogypsum and ammonium lactate and the separation of nanofiltration membranes combined with the surface treatment of polyvinyl carboxylate and carbon nitride modifiers, the impurity problems and high energy consumption in the preparation of modified calcium carbonate from phosphogypsum are solved, forming a high Purity modified light calcium carbonate, improving its dispersion and plastic properties.

CN117004249BActive Publication Date: 2024-10-15YIDU XINGFA CHEMICAL CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310743057.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-21
Publication Date
2024-10-15
Estimated Expiration
2043-06-21

AI Technical Summary

Technical Problem

In the existing technology, when preparing modified calcium carbonate from phosphogypsum, there are problems such as high impurity content, high energy consumption for phase transfer agent recovery, and low product purity. Moreover, the surface of light calcium carbonate is highly hydrophilic, which affects its interaction with organic polymers. affinity and dispersion.

Method used

Dissolve phosphogypsum and ammonium lactate solution, add dispersant and ammonium carbonate for phase transfer method to prepare light calcium carbonate, and separate and recover the phase transfer agent through nanofiltration membrane, and then use polyvinyl carboxylate, carbon nitride and vitamin E Polyethylene glycol succinate compound modifier is used for surface modification to form a stable hydrophobic coating layer.

Benefits of technology

The preparation of high-purity modified light calcium carbonate is achieved, which improves its dispersion and compatibility in polymers, reduces production costs, and enhances the heat resistance, strength and stiffness of plastic products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117004249B_ABST
    Figure CN117004249B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing modified light calcium carbonate from phosphogypsum. The method comprises dissolving phosphogypsum in an ammonium lactate solution, filtering to obtain a calcium-rich solution, carbonizing with ammonium carbonate to obtain light calcium carbonate, and wet-surface-modifying the light calcium carbonate with a composite modifier of polyvinyl carboxylate, carbon nitride and vitamin E polyethylene glycol succinate, so that a stable macromolecular organic hydrophobic coating layer is formed on the surface of the light calcium carbonate, the lipophilicity of the surface of the light calcium carbonate is increased, and the compatibility with the resin is better. The prepared modified light calcium carbonate is filled in a PP material, so that the heat resistance, impact resistance and bending resistance of the PP material can be significantly enhanced. The invention has a simple process and low production cost, and can realize high-value utilization of phosphogypsum.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of chemical industry, and in particular to a method for preparing modified light calcium carbonate from phosphogypsum. Background Art

[0002] Phosphogypsum is an industrial solid waste residue produced during the preparation of phosphoric acid by the sulfuric acid method. Every ton of phosphoric acid produced produces 4 to 5 tons of phosphogypsum. The main components of phosphogypsum are calcium sulfate dihydrate, followed by silicon dioxide, and a small amount of phosphorus and fluorine. The output of phosphogypsum is large, and stockpiling is the main disposal method. The stockpiling of phosphogypsum occupies a large amount of land resources and is prone to water pollution. Phosphogypsum is a misplaced resource, so processing and recycling phosphogypsum to produce high-value products can not only bring environmental benefits, but also create economic benefits.

[0003] At present, there is a process for preparing calcium carbonate using phosphogypsum. In the method of using phosphogypsum to co-produce ammonium sulfate and calcium carbonate in patent CN101492178A, phosphogypsum and ammonium carbonate are directly mixed and reacted to prepare modified calcium carbonate and ammonium sulfate. Although this method realizes the high-value utilization of phosphogypsum, the prepared modified calcium carbonate contains impurities and the purity is only 93.13%. The purity of calcium carbonate can be improved by dissolving phosphogypsum with a phase transfer agent, removing impurities and then carbonizing. In patent CN114368771A, ammonium chloride is used to dissolve phosphogypsum, remove impurities and then carbonize to prepare spherical calcium carbonate. In patent CN113321232A, an ammonia-containing phase transfer agent is used to dissolve and remove impurities and then carbonize to prepare light calcium carbonate. The ammonium sulfate in the phase transfer agent is recovered by evaporation and crystallization. Although this method can obtain relatively pure calcium carbonate, the energy consumption of evaporation and crystallization to recover ammonium sulfate is high, and when the cation of the phase transfer agent and the cation of the carbonizing agent are different, the purity of the product obtained by evaporation and crystallization is low.

[0004] Light calcium carbonate has highly hydrophilic hydroxyl groups on its surface, which shows strong alkalinity. This hydrophilic and oleophobic property makes light calcium carbonate have poor affinity with organic polymers, and it is easy to form aggregates and unevenly dispersed inside the polymer, which affects the use effect. In order to improve the reinforcing effect of light calcium carbonate and its dispersion effect in plastics, it is necessary to modify its surface. Commonly used surface modifiers include long-chain fatty acid salts such as stearate and oleate. These long-chain fatty acid salts form precipitation with calcium and wrap on the surface of calcium carbonate, but the wrapping layer is unstable and easily eluted during the washing process, which affects its role in plastic filling. Therefore, it is very necessary to design a surface wrapping layer of light calcium carbonate with a stable structure.

[0005] Based on this, it is necessary to develop a method for preparing modified light calcium carbonate using phosphogypsum, using phosphogypsum as raw material, adopting the phase transfer method to prepare light calcium carbonate, selecting appropriate separation technology to recover the phase transfer agent and ammonium sulfate, and surface modifying the light calcium carbonate to form a stable hydrophobic coating layer on its surface, thereby improving the surface stability of light calcium carbonate, enhancing its affinity with organic polymers and its dispersibility inside the polymers. Summary of the invention

[0006] The present invention aims to overcome the deficiencies in the prior art and aims to provide a method for preparing modified light calcium carbonate using phosphogypsum, which can prepare phosphogypsum into high-purity modified light calcium carbonate and effectively separate and recover phase transfer agent and ammonium sulfate. The prepared modified light calcium carbonate has a uniform and stable surface coating layer, strong hydrophobicity, is evenly dispersed in polymers and has good compatibility. The preparation process is simple, the cost is low, the conversion product has good performance, and meets the requirements of the target market.

[0007] In order to achieve the above object, the present invention is implemented through the following technical solutions:

[0008] (1) adding phosphogypsum to an ammonium lactate solution, heating and stirring to dissolve, and filtering after complete dissolution to obtain a calcium-rich solution and high-silicon slag;

[0009] (2) adding a dispersant to the calcium-rich solution obtained in step (1), slowly dripping the ammonium carbonate solution into the calcium-rich solution under heating conditions, and continuously stirring, filtering to obtain light calcium carbonate after the dripping is completed, separating ammonium lactate and ammonium sulfate from the filtrate using a nanofiltration membrane, and recycling the ammonium lactate to step (1);

[0010] (3) slurrying the light calcium carbonate obtained in step (2), adding a surface modifier to the slurry, heating and fully stirring the slurry for a period of time, filtering, washing, and drying to obtain modified light calcium carbonate.

[0011] Preferably, in step (1), the mass ratio of phosphogypsum to ammonium lactate is 1:2-4, the concentration of ammonium lactate is 15wt%-25wt%, the dissolution temperature is 40-60°C, the stirring speed is 200-400r / min, and the dissolution time is 0.5-2h.

[0012] Preferably, in step (2), the dispersant is sodium laurate, the dosage is 0.1wt% to 0.5wt%, the concentration of the ammonium carbonate solution is 2-5wt%, the carbonization reaction temperature is 75 to 95°C, the stirring speed is 200 to 400 r / min, and the dropping time is 10 to 30 min.

[0013] Preferably, in step (2), the nanofiltration membrane has a molecular weight cutoff of 300D and two-stage nanofiltration is used.

[0014] Preferably, the slurry concentration in step (3) is 40wt% to 60wt%, the surface modifier is a composite modifier prepared by polyvinyl carboxylate, carbon nitride and vitamin E polyethylene glycol succinate in a ratio of 2:0.1-1.5:1-5, the dosage is 3wt% to 5wt%, the heating temperature is 75 to 95°C, and the stirring time is 0.5 to 1h.

[0015] Beneficial effects of the present invention:

[0016] 1. The process flow of the present invention is simple, the energy consumption is low, the entire reaction system forms a closed loop, the ammonium lactate solution is recycled, and no waste is generated;

[0017] 2. The present invention adopts a composite modifier of polyvinyl carboxylate, carbon nitride and vitamin E polyethylene glycol succinate to wet-modify the surface of light calcium carbonate to form a uniform and stable lipophilic and hydrophobic coating layer, which significantly improves the hydrophobicity and dispersibility of light calcium carbonate. When used as a filler for plastic products, it can enhance the heat resistance, strength and rigidity of plastic products and reduce production costs; 3. The present invention prepares phosphogypsum into a high-value modified light calcium carbonate product, realizes the resource recycling of phosphogypsum, can effectively alleviate the environmental problems caused by phosphogypsum, and create economic value. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 It is a process flow chart of the present invention. Specific implementation plan

[0019] In order to better explain the present invention, the following examples are listed. The following examples are only some implementation plans of the present invention. The phosphogypsum used in the examples is taken from a phosphorus chemical enterprise, and its composition table is as follows:

[0020] Table 1: Main components of phosphogypsum:

[0021]

[0022] Example 1

[0023] (1) adding phosphogypsum to a 15 wt % ammonium lactate solution, with the mass ratio of phosphogypsum to ammonium lactate being 1:2, heating to 40° C., maintaining the temperature, stirring and dissolving for 2 h at a stirring speed of 300 r / min, and filtering to obtain a calcium-rich solution;

[0024] (2) adding 0.2 wt % sodium lauryl sulfate to the calcium-rich solution obtained in step (1), heating the calcium-rich solution to 80° C., maintaining the temperature, dripping a 2 wt % ammonium carbonate solution into the calcium-rich solution for 10 min, and stirring continuously at a stirring speed of 300 r / min. After the dripping is completed, filtering to obtain light calcium carbonate, and performing two-stage nanofiltration of the filtrate using a nanofiltration membrane with a molecular weight cutoff of 300D. The ammonium lactate is reused in step (1), and the recovery rate of ammonium lactate is 91.5%;

[0025] (3) The light calcium carbonate obtained in step (2) is slurried to a concentration of 40 wt %. 3 wt % of a surface modifier is added to the slurry. The surface modifier is a composite modifier prepared by mixing polyvinyl carboxylate, carbon nitride and vitamin E polyethylene glycol succinate in a ratio of 2:1.5:2. The slurry is heated to 80° C. and stirred for 0.5 h. The modified light calcium carbonate is obtained after filtering, washing and drying.

[0026] Example 2

[0027] The method and steps are the same as those in Example 1, except that the concentration of ammonium lactate is 20wt%, the mass ratio of phosphogypsum to ammonium lactate is 1:3, the dissolution temperature is 45°C, the dissolution time is 1h, the dissolution stirring speed is 200r / min, the amount of dispersant is 0.3wt%, the carbonization reaction temperature is 85°C, the ammonium carbonate concentration is 3wt%, the dropping time is 15min, the carbonization stirring speed is 400r / min, the slurry adjustment concentration is 50wt%, the amount of surface modifier is 4wt%, the surface modifier is a composite modifier prepared by polyvinyl carboxylate, carbon nitride and vitamin E polyethylene glycol succinate at a ratio of 2:0.5:3, the modification reaction temperature is 85°C, the modification stirring time is 1h, and the recovery rate of ammonium lactate is 91.1%;

[0028] Example 3

[0029] The method and steps are the same as those in Example 1, except that the concentration of ammonium lactate is 25wt%, the mass ratio of phosphogypsum to ammonium lactate is 1:4, the dissolution temperature is 50°C, the dissolution time is 1h, the amount of dispersant is 0.4wt%, the carbonization reaction temperature is 90°C, the ammonium carbonate concentration is 4wt%, the dropping time is 20min, the carbonization stirring speed is 400r / min, the slurry adjustment concentration is 60wt%, the amount of surface modifier is 4wt%, the surface modifier is a composite modifier prepared by polyvinyl carboxylate, carbon nitride and vitamin E polyethylene glycol succinate at a ratio of 2:0.3:3, the modification reaction temperature is 90°C, and the recovery rate of ammonium lactate is 91.1%.

[0030] Example 4

[0031] The method and steps are the same as those in Example 1, except that the ammonium lactate concentration is 20wt%, the mass ratio of phosphogypsum to ammonium lactate is 1:4, the dissolution temperature is 50°C, the dissolution time is 0.5h, the dissolution stirring speed is 400r / min, the dispersant dosage is 0.5wt%, the carbonization reaction temperature is 75°C, the ammonium carbonate concentration is 4wt%, the dropping time is 20min, the carbonization stirring speed is 400r / min, the slurry adjustment concentration is 55wt%, the surface modifier dosage is 5wt%, the surface modifier is a composite modifier prepared by polyvinyl carboxylate, carbon nitride and vitamin E polyethylene glycol succinate in a ratio of 2:1:3, the modification reaction temperature is 95°C, the modification stirring time is 1h, and the recovery rate of ammonium lactate is 90.4%.

[0032] Comparative Example 1

[0033] The method and steps are the same as those in Example 1, except that the surface modifier is a mixture of polyvinyl carboxylate and vitamin E polyethylene glycol succinate in a ratio of 1:1, with an amount of 3 wt %, and a recovery rate of ammonium lactate of 90.7%.

[0034] Comparative Example 2

[0035] The method steps are the same as those in Example 1, except that no dispersant is added during the carbonization process. The recovery rate of ammonium lactate is 91.2%.

[0036] Comparative Example 3

[0037] The method steps are the same as those in Example 1, except that ammonium chloride is used to dissolve phosphogypsum, and the recovery rate of ammonium chloride is 92.5%.

[0038] The modified calcium carbonate obtained in Examples 1-4 and Comparative Example 1 was washed with water 6 times, and the elution rate of the hydrophobic coating layer was measured. The results are shown in Table 2:

[0039] Table 2: Elution rate experimental data of Examples 1-4

[0040] sample 1 time 2 times 3 times 4 times 5 times 6 times Example 1 0.10% 0.17% 0.17% 0.19% 0.19% 0.19% Example 2 0.09% 0.11% 0.11% 0.11% 0.11% 0.11% Example 3 0.12% 0.15% 0.15% 0.16% 0.16% 0.16% Example 4 0.15% 0.15% 0.16% 0.17% 0.17% 0.17% Comparative Example 1 0.95% 1.32% 1.77% 2.52% 2.98% 3.57%

[0041] As can be seen from Table 2, after each washing, the elution rates of Examples 1-4 are lower than those of Comparative Example 1. After two washings, the elution rates of each sample of Examples 1-4 no longer change, indicating that after two washings, the coating layer on the surface of calcium carbonate will not be reduced by washing again, indicating that the coating layer can remain stable in the liquid phase dispersion system, while the elution rate of Comparative Example 1 increases after each washing, indicating that the coating layer will be reduced each time it is washed, and the coating layer is unstable. It can be seen that the addition of carbon nitride can effectively improve the stability of the coating layer, which is due to the high stability and hardness of the unit cell structure of carbon nitride. When used in combination with polyvinyl carboxylate and vitamin E polyethylene glycol succinate, a stable organic coating layer can be formed on the surface of calcium carbonate.

[0042] The light calcium carbonate prepared in Example 1 was used as Comparative Example 4, and the modified light calcium carbonates of Examples 1-4 and Comparative Examples 1-3 and the light calcium carbonate of Comparative Example 4 were analyzed and tested to determine the purity, sedimentation volume, and oil absorption value. The test results are shown in Table 3:

[0043] Table 3: Test data of examples and comparative examples

[0044] sample purity Sedimentation volume mL / g Oil absorption value Example 1 98.2% 4.5 34.4 Example 2 97.9% 4.8 37.5 Example 3 97.5% 4.4 32.8 Example 4 97.1% 4.9 37.9 Comparative Example 1 98.5% 3.9 41.2 Comparative Example 2 98.7% 2.5 48.1 Comparative Example 3 97.1% 2.2 35.4 Comparative Example 4 99.8% 2.8 58.9

[0045] It can be seen from Table 3 that the purities of Examples 1-4 and Comparative Examples 1-2 are all above 97%, indicating that high-purity modified light calcium carbonate can be prepared by this method; the sedimentation volume of Example 1 is higher than that of Comparative Example 4, and the oil absorption value is lower than that of Comparative Example 4, indicating that the surface coating modification of light calcium carbonate makes the surface of light calcium carbonate more oleophilic and hydrophobic, and has better dispersibility in water, so the sedimentation volume is larger, and the organic hydrophobic coating layer on the surface of light calcium carbonate reduces its oil absorption value; the sedimentation volume of Example 1 is higher than that of Comparative Example 2, indicating that the addition of dispersant during carbonization can increase the sedimentation volume of modified calcium carbonate, which is mainly because the dispersant can be adsorbed on the surface of calcium carbonate particles, inhibiting the growth and agglomeration of particles, so that the prepared modified light calcium carbonate particles are smaller and have better dispersibility. The sedimentation volume of Example 1 is greater than that of Comparative Example 1, and the oil absorption value is lower than that of Comparative Example 1, indicating that the addition of carbon nitride can increase the sedimentation volume of modified light calcium carbonate and reduce the oil absorption value, which is due to the addition of carbon nitride, which makes the encapsulation layer more hydrophobic, more stable in structure, and reduces the surface voids of calcium carbonate particles. All indicators of Example 1 are better than those of Comparative Example 3, because ammonium lactate is combined with calcium ions in a complex form. During the carbonization process, the calcium of calcium lactate is slowly released into the solution and combined with ammonium carbonate to form calcium carbonate. The formed calcium carbonate has a small particle size and a uniform shape, and light calcium carbonate can be obtained. Ammonium chloride promotes the dissolution of calcium sulfate through the salt effect, and calcium exists in the form of ions. During the carbonization process, a large amount of calcium ions and ammonium carbonate are combined to easily form particles with large particle size, and heavy calcium carbonate is obtained.

[0046] The modified light calcium carbonate in Examples 1-4 was added to the polypropylene material at an addition rate of 20%, and the same amount of light calcium carbonate prepared in Examples 1-4 was added to the polypropylene material at an addition rate of 20% as Comparative Examples 4-7, and the pure polypropylene material was used as Comparative Example 8. Performance tests were performed on Examples 1-4 and Comparative Examples 1-7. The performance test results are shown in Table 4:

[0047] Table 4: Comparative Examples and Examples Performance Test Experimental Data

[0048]

[0049]

[0050] It can be seen from Table 4 that various performance indicators of Comparative Examples 4-7 are higher than those of Comparative Example 8, indicating that the addition of light calcium carbonate can simultaneously improve the tensile strength, flexural strength, impact strength and heat resistance of PP materials. The heat resistance, flexural strength and impact strength of Comparative Example 3 are better than those of Comparative Example 8, but the tensile strength is lower than that of Comparative Example 8, indicating that the addition of heavy calcium carbonate can also improve the heat resistance and some mechanical properties of plastics, but cannot simultaneously improve the tensile strength, flexural strength, impact strength and heat resistance. All performance indicators of Examples 1-4 are higher than those of Comparative Examples 4-7, indicating that after the light calcium carbonate is modified, it has better compatibility with the PP material, and the mechanical properties and heat resistance of the PP material are greatly improved. All performances of Example 1 are better than those of Comparative Example 2, indicating that the addition of dispersant can improve the filling effect of calcium carbonate in plastic fillers. All performances of Example 1 are better than those of Comparative Example 1, and the heat resistance and impact resistance of the plastic are significantly improved. This is due to the high hardness and high temperature resistance of carbon nitride, which makes the wrapping layer more stable. Adding modified light calcium carbonate to the plastic enhances the impact strength, tensile strength, bending strength and heat resistance of the plastic.

[0051] The above description is only a preferred embodiment of the present invention and is not intended to be a limitation of the present invention. Any improvements and modifications made on the basis of the creative concept of the present invention are within the protection scope of the present invention.

Claims

1. A method for preparing modified light calcium carbonate from phosphogypsum, The following steps are involved: (1) adding phosphogypsum to ammonium lactate solution, heating and stirring to dissolve, and filtering to obtain calcium-rich liquid and high-silicon slag after complete dissolution; (2) adding a dispersant to the calcium-rich solution obtained in step (1), wherein the dispersant is sodium laurate, and slowly dropping an ammonium carbonate solution into the calcium-rich solution under heating conditions, while continuously stirring. After the dropwise addition is completed, filtering is performed to obtain light calcium carbonate, and the filtrate is separated into ammonium lactate and ammonium sulfate using a nanofiltration membrane, and the ammonium lactate is recycled to step (1); (3) The light calcium carbonate obtained in step (2) is slurried, and a surface modifier is added to the slurry, wherein the surface modifier is a composite modifier obtained by mixing polyvinyl carboxylate, carbon nitride and vitamin E polyethylene glycol succinate in a ratio of 2:0.1-1.5:1-5, the slurry is heated and fully stirred for a period of time, and then filtered, washed, and dried to obtain modified light calcium carbonate.

2. The method according to claim 1, It is characterized in that In step (1), the mass ratio of phosphogypsum to ammonium lactate is 1:2-4, and the concentration of ammonium lactate is 15wt%-25wt%.

3. The method according to claim 1, It is characterized in that In step (1), the dissolution temperature is 40-60° C., the stirring speed is 200-400 r / min, and the dissolution time is 0.5-2 h.

4. The method according to claim 1, It is characterized in that In step (2), the amount of dispersant used is 0.1 wt % to 0.5 wt %, and the concentration of ammonium carbonate solution is 2 wt % to 5 wt %.

5. The method according to claim 1, It is characterized in that In step (2), the carbonization reaction temperature is 75-95°C, the stirring speed is 200-400 r / min, and the dropping time is 10-30 min.

6. The method according to claim 1, It is characterized in that In the step (2), the nanofiltration membrane uses a nanofiltration membrane with a molecular weight cutoff of 300D, and two-stage nanofiltration is used.

7. The method according to claim 1, It is characterized in that In step (3), the concentration of light calcium carbonate slurry is 40wt%~60wt%, and the dosage is 3wt%~5wt%.

8. The method according to claim 1, It is characterized in that In step (3), the heating temperature is 75-95° C. and the stirring time is 0.5-1 h.