Preparation method of temporary coating material and its application on zirconium alloy cladding surface
Through a temporary coating coating preparation method, the problem of the existing water-soluble coating being difficult to dissolve in low-temperature water is solved, and a coating with hardness and scratch resistance is prepared to ensure that the zirconium alloy nuclear fuel cladding is capable of being installed after installation Completely clean up to reduce the risk of rupture.
Patent Information
- Application Number
- CN202310977043.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-04
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-08-04
AI Technical Summary
The existing water-soluble coating is difficult to completely dissolve in low-temperature water, resulting in residual surface of the zirconium alloy nuclear fuel cladding, continuous erosion, causing secondary scratches, and increasing the risk of rupture.
By adopting a temporary coating coating preparation method, a seed emulsion with a buffer is formed by stirring the mixture liquids A and B and dropping the initiator, and a neutralizing agent and an inorganic filler are added after pH adjustment to prepare the A coating with good hardness and scratch resistance, the coating can be completely dissolved in low temperature water.
The formed coating has good hardness and scratch resistance on the surface of the zirconium alloy shell. It can be completely cleaned in low-temperature water after the installation of the zirconium alloy nuclear fuel, without affecting subsequent work, and reducing the risk of rupture of the zirconium alloy shell.
Smart Images

Figure CN117004281B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of protective coatings, and in particular to a method for preparing a temporary coating material and application thereof on the surface of a zirconium alloy cladding. Background Art
[0002] The working environment of the fuel rod is very extreme. It has to withstand high pressure, high temperature, high radiation and high vibration in the reactor. In this case, it is expected that the fuel rod will be damaged. Therefore, the damage of zirconium alloy nuclear fuel cladding is the main reason for small nuclear leaks in recent years. One of the reasons for the damage of zirconium alloy nuclear fuel cladding is that it is very easy to scratch with the spring sheet and guide wing of the fixed skeleton during the installation of the zirconium alloy nuclear fuel cladding, resulting in deep scratches on the surface of the zirconium alloy nuclear fuel cladding. A large amount of debris is generated during the scratching process, which will wash the surface of the zirconium alloy nuclear fuel cladding when the nuclear fuel assembly is working, causing secondary scratches and increasing the probability of rupture of the zirconium alloy nuclear fuel cladding.
[0003] Based on the above problems, the prior art also provides a temporary protective coating for the surface of nuclear fuel rods. By forming a layer of water-soluble coating on the surface of the nuclear fuel cladding, it is applied to the surface of the cladding before the zirconium alloy nuclear fuel cladding is installed. The coating is formed after curing, which can prevent the zirconium alloy nuclear fuel cladding from being damaged during the assembly process. After the assembly is completed, the coating can be completely dissolved by water without affecting the subsequent normal operation of the zirconium alloy nuclear fuel cladding.
[0004] However, the water-soluble coating provided in the prior art has poor water solubility in cold water and is difficult to be completely washed off in low-temperature water. The coating will still remain on the surface of the zirconium alloy fuel cladding. During the subsequent operation of the nuclear fuel rod, the surface of the zirconium alloy nuclear fuel cladding is impacted by a large amount of water vapor, and the residual coating flocs continue to wash the surface of the cladding, which is easy to cause secondary scratches. Therefore, it is urgent to provide a solution to improve this problem. Summary of the invention
[0005] The purpose of the present invention is to provide a method for preparing a temporary coating material and its application on the surface of a zirconium alloy cladding, which can form a coating with good hardness and scratch resistance on the surface of the zirconium alloy cladding, improve the scratching of the guided wing and the spring sheet, and after the zirconium alloy nuclear fuel is installed, the coating can be dissolved in low-temperature water and completely cleaned without affecting the subsequent normal operation of the zirconium alloy cladding.
[0006] In a first aspect, the present invention provides a method for preparing a temporary protective coating, comprising the following steps:
[0007] Adding mixed liquid B dropwise to mixed liquid A in a stirring state to obtain a pre-emulsion; wherein the mixed liquid B contains isooctyl acrylate, methyl methacrylate and styrene, and the mixed liquid A contains emulsifier A and acrylic acid;
[0008] The mixed solution D and the initiator A are simultaneously added dropwise to the mixed solution C in a stirring state to obtain a seed emulsion; wherein the mixed solution D contains isooctyl acrylate, methyl methacrylate and styrene, and the mixed solution C contains an emulsifier B dissolved therein;
[0009] The seed emulsion and initiator B are stirred and mixed to obtain a mixed system, and the pre-emulsified liquid is then added dropwise into the mixed system and stirred and dispersed, and the pH is adjusted to 6.8-7.2 and filtered, and a neutralizer and an inorganic filler are added and uniformly dispersed to obtain a temporary coating paint; wherein a buffer is pre-mixed in the seed emulsion.
[0010] Optionally, the mass mixing ratio of isooctyl acrylate, methyl methacrylate, styrene, emulsifier A and acrylic acid in the pre-emulsion is (100-120):(70-90):(80-100):(7.8-9.8):(3-4); and the seed emulsion includes the product of the reaction polymerization of isooctyl acrylate, methyl methacrylate, styrene and emulsifier B in a mass ratio of (10-14):(8-10):(10-12):(0.7-1.6).
[0011] Optionally, the step of adding the mixed solution B dropwise to the mixed solution A in a stirring state to obtain the pre-emulsion includes the following steps: adding the mixed solution B dropwise to the mixed solution A in a stirring state and heated to 35-45° C. in a water bath, and controlling the dropping rate to 4-5 mL / min; after the dropping is completed, maintaining the stirring state and stirring for 5-10 minutes to obtain the pre-emulsion.
[0012] Optionally, during the step of simultaneously dropping the mixed solution D and the initiator A into the mixed solution C in a stirring state to prepare the seed emulsion, the initiator C is pre-dissolved in the mixed solution C.
[0013] Optionally, before executing the step of synchronously dropping the mixed solution D and the initiator A into the mixed solution C in a stirring state to obtain the seed emulsion, the following steps are executed: dissolving the emulsifier B in water to prepare an aqueous solution, and then uniformly mixing it with the initiator C to obtain the mixed solution C.
[0014] Optionally, during the step of synchronously adding the mixed liquid D and the initiator A to the mixed liquid C in a stirring state to prepare the seed emulsion, the dropping rate of the mixed liquid D is controlled to be 0.40-0.80 mL / min, the dropping rate of the initiator A is controlled to be 0.05-0.30 mL / min, and the dropping time is controlled to be 60-90 min.
[0015] Optionally, before performing the step of stirring and mixing the seed emulsion and the initiator B to prepare a mixed system, the following step is performed: pre-dissolving a buffer in the seed emulsion.
[0016] Optionally, the emulsifier A and the emulsifier B independently include an anionic emulsifier and a nonionic emulsifier.
[0017] In a second aspect, the present invention provides a temporary coating material prepared by any of the above optional preparation methods.
[0018] In a third aspect, the present invention provides the use of a temporary coating prepared by any of the above optional preparation methods on the surface of a nuclear fuel zirconium alloy cladding. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 It is a flowchart of a method for preparing a temporary coating material in an embodiment of the present invention;
[0020] Figure 2 The particle size distribution diagram of the temporary coating material provided in Example 1(a), Example 2(b) and Example 3(c) of the present invention;
[0021] Figure 3 This is a Fourier infrared spectrum of the temporary coating material provided in Example 1 of the present invention. DETAILED DESCRIPTION
[0022] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Unless otherwise defined, the technical terms or scientific terms used herein should be understood by people with general skills in the field to which the present invention belongs. "Including" and similar words used in this article mean that the elements or objects appearing before the word include the elements or objects listed after the word and their equivalents, without excluding other elements or objects.
[0023] See also Figure 1In an embodiment of the present invention, a method for preparing a temporary coating material is provided, comprising the following steps:
[0024] S1. Preparation of pre-emulsion: adding mixed solution B dropwise to mixed solution A in a stirring state to obtain a pre-emulsion;
[0025] S2, seed emulsion preparation: the mixed solution D and the initiator A are simultaneously added dropwise to the mixed solution C in a stirring state to obtain a seed emulsion;
[0026] S3. Coating preparation: The seed emulsion premixed with a buffer is stirred and mixed with initiator B to obtain a mixed system, and the pre-emulsified liquid is added dropwise to the mixed system and stirred and dispersed, and the pH is adjusted to 6.8-7.2 and filtered, and a neutralizer and an inorganic filler are added and uniformly dispersed to obtain a temporary coating.
[0027] Among them, emulsifier A and acrylic acid are dissolved in mixed liquid A; isooctyl acrylate, methyl methacrylate and styrene are mixed in mixed liquid B; emulsifier B is dissolved in mixed liquid C; and isooctyl acrylate, methyl methacrylate and styrene are mixed in mixed liquid D.
[0028] In some embodiments, the order of performing step S1 and step S2 can be interchanged or performed simultaneously, that is, step S2 can be performed first and then step S1, or step S1 and step S2 can be performed simultaneously.
[0029] In some embodiments, emulsifier A and emulsifier B independently include anionic emulsifiers and nonionic emulsifiers. Specifically, the anionic emulsifier can be sodium dodecylbenzene sulfonate, sodium dodecyl sulfate, sodium salt of dibutyl sulfosuccinate, and the nonionic emulsifier can be alkylphenol polyoxyethylene ether and nonylphenol polyethylene oxide ether.
[0030] In some embodiments, in the pre-emulsion, the mass mixing ratio of isooctyl acrylate, methyl methacrylate, styrene, emulsifier A and acrylic acid is (100-120):(70-90):(80-100):(7.8-9.8):(3-4).
[0031] In some embodiments, the seed emulsion includes a product of polymerization of isooctyl acrylate, methyl methacrylate, styrene and emulsifier B in a mass ratio of (10-14):(8-10):(10-12):(0.7-1.6).
[0032] In some embodiments, see Figure 1 , before executing step S1, perform the following steps:
[0033] S0. Preparation of mixed solution: dissolving emulsifier A and acrylic acid to prepare mixed solution A; mixing isooctyl acrylate, methyl methacrylate and styrene to prepare mixed solution B; dissolving emulsifier B to prepare mixed solution C; mixing isooctyl acrylate, methyl methacrylate and styrene to prepare mixed solution D.
[0034] In some embodiments, when emulsifier A and emulsifier B are both compositions of alkylphenol polyoxyethylene ether and sodium dodecylbenzene sulfonate, the mixed solution in step S0 is prepared as follows: dissolving alkylphenol polyoxyethylene ether, sodium dodecylbenzene sulfonate and acrylic acid in deionized water to obtain mixed solution A; dissolving alkylphenol polyoxyethylene ether and sodium dodecylbenzene sulfonate in deionized water to obtain mixed solution C.
[0035] Furthermore, when preparing the mixed solution A in step S0, the alkylphenol polyoxyethylene ether, sodium dodecylbenzene sulfonate and acrylic acid are mixed with deionized water in advance, heated to 35-45° C. in a water bath, and stirred at a speed of 150-400 rpm to completely dissolve the alkylphenol polyoxyethylene ether, sodium dodecylbenzene sulfonate and acrylic acid in the deionized water, thereby obtaining the mixed solution A.
[0036] In some embodiments, during the execution of step S2, an initiator C is pre-dissolved in the mixed solution C. Specifically, the initiator C may be ammonium persulfate, potassium persulfate, or sodium persulfate.
[0037] Furthermore, when preparing the mixed solution C in step S0, the emulsifier B is dissolved in deionized water to prepare an aqueous solution, and then uniformly mixed with the initiator C to obtain the mixed solution C.
[0038] Furthermore, when the emulsifier B is alkylphenol polyoxyethylene ether and sodium dodecylbenzene sulfonate, and the initiator C is ammonium persulfate, preparing the mixed solution C in step S0 includes: dissolving ammonium persulfate in deionized water in advance to prepare an ammonium persulfate solution, and then adding the alkylphenol polyoxyethylene ether, sodium dodecylbenzene sulfonate and ammonium persulfate solution into the deionized water and mixing them evenly, and preparing the mixed solution C after complete dissolution.
[0039] Furthermore, when preparing the mixed solution C in step S0, the mixed solution may be stirred at a speed of 250-400 rpm in a water bath heating environment at 80-90°C to accelerate the dissolution of the emulsifier B.
[0040] In some embodiments, the process of executing step S1 includes the following steps:
[0041] Add mixed solution B dropwise into mixed solution A which is stirred and heated to 35-45°C in a water bath, and control the drop rate to 4-5 mL / min;
[0042] After the dropwise addition is completed, the stirring state is maintained for 5-10 minutes to obtain a pre-emulsion.
[0043] Furthermore, when preparing the mixed solution A in step S0, the emulsifier A and acrylic acid are mixed with ionized water, heated in a water bath to 35-45° C., stirred at 150 rpm to dissolve and disperse the emulsifier A and acrylic acid, and then the stirring speed is gradually increased to 400 rpm to connect to step S1.
[0044] In some embodiments, during step S2, the dripping rate of the mixed solution D to the mixed solution C is controlled to be 0.40-0.80 mL / min, the dripping rate of the initiator A to the mixed solution C is controlled to be 0.05-0.30 mL / min, and the dripping time is controlled to be 60-90 min.
[0045] In some embodiments, after the mixed solution C is prepared in step S0, the mixed solution C is kept in a stirring state at a rotation speed of 300-400 rpm to proceed to step S2.
[0046] In some embodiments, before performing the process of stirring and mixing the seed emulsion and the initiator B to prepare the mixed system in step S3, the buffer is pre-dissolved in the seed emulsion. Specifically, the buffer can be sodium bicarbonate, sodium carbonate, or ammonium bicarbonate.
[0047] In some embodiments, the initiator B can be ammonium persulfate, potassium persulfate, or sodium persulfate.
[0048] In some embodiments, the neutralizing agent can be ethanolamine, dimethylethanolamine, ammonia water, or diethanolamine.
[0049] In some embodiments, the inorganic filler may be nano-silicon dioxide, nano-titanium dioxide, or quartz sand in the form of silica sol.
[0050] The embodiments of the present invention also provide a temporary coating material prepared by the preparation method in any of the above embodiments.
[0051] The embodiments of the present invention also provide the use of a temporary coating prepared by the preparation method in any of the above embodiments on the surface of a nuclear fuel zirconium alloy cladding.
[0052] Example 1
[0053] The present embodiment 1 provides a method for preparing a temporary coating applied to the surface of a zirconium alloy nuclear fuel, which comprises the following steps:
[0054] S0, mixed solution preparation: 2.8g alkylphenol polyoxyethylene ether, 5.2g sodium dodecylbenzene sulfonate and 3g acrylic acid were put into a three-necked flask, and after adding 200g deionized water, the three-necked flask was stirred at 40°C and 400rpm, and stirred until completely dissolved to obtain a mixed solution A; 110g isooctyl acrylate, 75g methyl methacrylate and 80g styrene were mixed to obtain a mixed solution B; 0.3g ammonium persulfate was dissolved in 8g deionized water to obtain an ammonium persulfate solution, and 0.35g alkylphenol polyoxyethylene ether, 0.5g sodium dodecylbenzene sulfonate, 25g deionized water and ammonium persulfate solution were added to a four-necked flask, and stirred at 85°C and 300rpm in the four-necked flask. After stirring until completely dissolved, a mixed solution C was obtained; 12g isooctyl acrylate, 10g methyl methacrylate and 10g styrene were mixed to obtain a mixed solution D;
[0055] S1. Preparation of pre-emulsion: pre-adding mixed solution A into a continuously stirred pre-emulsification kettle for continuous stirring, then adding mixed solution B into a constant pressure dropping funnel, connecting the dropping funnel to the pre-emulsification kettle, and then dropping mixed solution B into the pre-emulsification kettle, controlling the dropping time to be 45 min ± 1 min, and after the dropping is completed, continuing to stir for 5 min to obtain a pre-emulsion;
[0056] S2, seed emulsion preparation: pre-dissolve 0.2g ammonium persulfate in 6g deionized water to prepare initiator A, and add initiator A to a constant pressure dropping funnel, add mixed solution D to another constant pressure dropping funnel, and then put mixed solution C into a continuously stirred emulsifying kettle for continuous stirring, and simultaneously add mixed solution D and initiator A to the emulsifying kettle at 82°C, control the dropping time to 80min±1min, and after the dropping is completed, heat to 88°C and keep warm for 2.5h to obtain seed emulsion;
[0057] S3, coating preparation: pre-dissolve 2.8g ammonium persulfate in 40g deionized water to prepare initiator B; mix the seed emulsion with 1.4g sodium bicarbonate and 80g deionized water and put into a four-necked flask, and place the four-necked flask in a 60°C water bath and stir until the sodium bicarbonate is completely dissolved, then slowly add initiator B into the four-necked flask and mix evenly, and adjust the water bath temperature to slowly heat up to 88°C, and use a constant pressure dropping funnel to drop the pre-emulsified liquid into the four-necked flask, and add The mixture was stirred continuously during the process and the dropping time was controlled to be 150 min ± 1 min. After the dropping was completed, the mixture was kept warm for 120 min to obtain a mixed emulsion. The mixed emulsion in the four-necked flask was cooled to room temperature, the pH value of the mixed emulsion was adjusted to 7 with ammonia water, the mixed emulsion was filtered with a 300-mesh filter cloth, and the filtered mixed emulsion was transferred to a water bath at 60°C. 100 g of ethanolamine and 6 g of nano-silicon dioxide in the form of silica sol were added and uniformly dispersed to obtain a temporary coating.
[0058] Example 2
[0059] The preparation method of a temporary coating applied to the surface of zirconium alloy nuclear fuel provided in this embodiment 2 is different from that in embodiment 1 in that, in the preparation of the mixed solution in step S0, 3.4 g of alkylphenol polyoxyethylene ether, 6.2 g of sodium dodecylbenzene sulfonate and 4 g of acrylic acid are dissolved in 280 g of deionized water to prepare a mixed solution A; 120 g of isooctyl acrylate, 80 g of methyl methacrylate and 100 g of styrene are mixed to prepare a mixed solution B; 0.3 g of ammonium persulfate is dissolved in 8 g of deionized water to prepare an ammonium persulfate solution, and 0.5 g of alkylphenol polyoxyethylene ether, 1.0 g of sodium dodecylbenzene sulfonate, 35 g of deionized water and the ammonium persulfate solution are added to a four-necked flask, dissolved fully and mixed evenly to prepare a mixed solution C; 14 g of isooctyl acrylate, 10 g of methyl methacrylate and 12 g of styrene are evenly mixed to prepare a mixed solution D.
[0060] Also, in the preparation of the seed emulsion in step S2, the dripping time of the mixed solution D and the initiator A is controlled to be 90 min±1 min.
[0061] Also, in step S3, in the coating preparation, 3.2 g of ammonium persulfate is dissolved in 60 g of deionized water to prepare initiator B; the water bath temperature of the seed emulsion, sodium bicarbonate and deionized water is 70° C.; the added amount of ethanolamine is 110 g, and the added amount of nano-silica is 8 g.
[0062] Example 3
[0063] The preparation method of a temporary coating applied to the surface of zirconium alloy nuclear fuel provided in this embodiment 3 is different from that in embodiment 1 in that, in the preparation of the mixed solution in step S0, 3.4 g of alkylphenol polyoxyethylene ether, 6.2 g of sodium dodecylbenzene sulfonate and 4 g of acrylic acid are dissolved in 280 g of deionized water to prepare a mixed solution A; 140 g of isooctyl acrylate, 80 g of methyl methacrylate and 80 g of styrene are mixed to prepare a mixed solution B; 0.3 g of ammonium persulfate is dissolved in 8 g of deionized water to prepare an ammonium persulfate solution, and 1.0 g of alkylphenol polyoxyethylene ether, 1.0 g of sodium dodecylbenzene sulfonate, 35 g of deionized water and the ammonium persulfate solution are added to a four-necked flask, dissolved fully and mixed evenly to prepare a mixed solution C; 14 g of isooctyl acrylate, 10 g of methyl methacrylate and 12 g of styrene are evenly mixed to prepare a mixed solution D.
[0064] Also, in the preparation of the seed emulsion in step S2, the dripping time of the mixed solution D and the initiator A is controlled to be 90 min±1 min.
[0065] Also, in step S3, in the coating preparation, 3.2 g of ammonium persulfate is dissolved in 60 g of deionized water to prepare initiator B; the water bath temperature of the seed emulsion, sodium bicarbonate and deionized water is 70° C.; the added amount of ethanolamine is 100 g, and the added amount of nano-silica is 10 g.
[0066] Comparative Example
[0067] Comparative Example 1
[0068] S0, mixed solution preparation: 2.8g alkylphenol polyoxyethylene ether, 5.2g sodium dodecylbenzene sulfonate and 3g acrylic acid were put into a three-necked flask, and 200g deionized water was added, and the three-necked flask was stirred at 40°C and 400rpm until completely dissolved to obtain a mixed solution A; 110g butyl acrylate, 75g methyl methacrylate and 80g styrene were mixed to obtain a mixed solution B;
[0069] S1. Coating preparation: 3.0 g of ammonium persulfate was dissolved in 46 g of deionized water to prepare initiator A; mixed solution A was mixed with 1.4 g of sodium bicarbonate and 80 g of deionized water and then put into a four-necked flask, and the four-necked flask was placed in a 60°C water bath and stirred until the sodium bicarbonate was completely dissolved, initiator A was slowly added to the four-necked flask and mixed evenly, and the water bath temperature was adjusted to slowly increase the temperature to 88°C, mixed solution B was dripped into the four-necked flask using a constant pressure dropping funnel, and The mixture was stirred continuously during the process and the dropping time was controlled to be 150 min ± 1 min. After the dropping was completed, the mixture was kept warm for 120 min to obtain a mixed emulsion. The mixed emulsion in the four-necked flask was cooled to room temperature, the pH value of the mixed emulsion was adjusted to 7 with ammonia water, the mixed emulsion was filtered with a 300-mesh filter cloth, and the filtered mixed emulsion was transferred to a water bath at 60°C. 100 g of ethanolamine and 6 g of nano-silicon dioxide in the form of silica sol were added and uniformly dispersed to obtain a temporary coating.
[0070] Performance Testing
[0071] The coatings prepared in Examples 1-3 and Comparative Example 1 were pre-evenly coated on the surface of zirconium alloy nuclear fuel rods with a diameter of 10 mm, a wall thickness of 0.5 mm, and a length of 20 cm, and then cured at 90° C. for 30 minutes, and then the following tests were performed.
[0072] Hardness: The hardness of the coating was measured according to the national standard GB T 6739-1996 "Coating Hardness Pencil Test Method", and the results are shown in Table 1;
[0073] Scratch resistance: The coated nuclear fuel cladding is loaded on a spacer grid. The spacer grid scratches the coating and leaves scratches. The scratches are observed with a metallographic microscope and their widths are measured. The test is repeated three times to obtain the average value.
[0074] The results are shown in Table 2;
[0075] Water solubility: The coating was rinsed at a fixed volume of 200 ml and the temperature was increased by 5°C from 20°C to test the temperature at which the coating could be completely rinsed away and there was no flocculent in the rinsed aqueous solution. The results are shown in Table 3.
[0076] Table 1 Hardness test data of the coating in Examples 1-3 and Comparative Example 1
[0077] Example 1 Example 2 Example 3 Comparative Example 1 hardness H H H HB
[0078] Table 2 Scratch resistance test data of the coatings in Examples 1-3 and Comparative Example 1
[0079] Example 1 Example 2 Example 3 Comparative Example 1 Scratch resistant 346.7μm 320.9μm 454.8μm 561.2μm
[0080] Table 3 Water solubility test data of the coatings in Examples 1-3 and Comparative Example 1
[0081] Example 1 Example 2 Example 3 Comparative Example 1 Water Solubility 60℃ 45℃ 45℃ 90℃
[0082] Compared with the emulsion prepared in the comparative example, the comparative example directly adds the monomer mixture into the four-necked flask without treatment for polymerization, and the emulsion stability is poor. In contrast, in the examples 1-3, the monomer mixture is pre-emulsified to make the monomer and the emulsifier mix very evenly, which increases the stability of the emulsion polymerization, can effectively control the particle size and viscosity of the emulsion, and can avoid the phenomenon of micelles forming gels due to excessive local concentration of the emulsifier in the four-necked flask. It can be seen from Table 1 that after the coating prepared by the preparation method provided in the embodiment of the present invention forms a coating, it has better hardness than that of the comparative example 1, and it can be seen from Table 2 that after the coating in the embodiment of the present invention is scratched, the scratches formed are smaller than those in the comparative example 1, so the scratch resistance is also more prominent. At the same time, it can be seen from Table 3 that when the water solubility test is carried out, the coating in the present invention can be completely dissolved in low-temperature water of 45-60°C, achieving a good removal effect, while the coating in the comparative example 1 needs to be completely dissolved in high-temperature water of 90°C.
[0083] Although the embodiments of the present invention are described in detail above, it is obvious to those skilled in the art that various modifications and variations can be made to these embodiments. However, it should be understood that such modifications and variations are within the scope and spirit of the present invention as described in the claims. Moreover, the present invention described herein may have other embodiments and may be implemented or realized in a variety of ways.
Claims
1. A method for preparing a temporary coating material, It is characterized in that The following steps are involved: Add the mixed solution B dropwise into the mixed solution A which is in a stirring state and heated to 35-45° C. in a water bath, and control the dropping rate to 4-5 mL / min; after the dropping is completed, keep stirring for 5-10 minutes to obtain a pre-emulsion; wherein the mixed solution B contains isooctyl acrylate, methyl methacrylate and styrene, and the mixed solution A contains emulsifier A and acrylic acid; the mass mixing ratio of isooctyl acrylate, methyl methacrylate, styrene, emulsifier A and acrylic acid in the pre-emulsion is (100-120): (70-90): (80-100): (7.8-9.8): (3-4); The mixed liquid D and the initiator A are synchronously added dropwise to the mixed liquid C in a stirring state to obtain a seed emulsion, the dropping rate of the mixed liquid D is controlled to be 0.40-0.80 mL / min, the dropping rate of the initiator A is controlled to be 0.05-0.30 mL / min, and the dropping time is controlled to be 60-90 min; wherein the mixed liquid D is mixed with isooctyl acrylate, methyl methacrylate and styrene, and the mixed liquid C is dissolved with an emulsifier B; the seed emulsion includes a product of the reaction polymerization of isooctyl acrylate, methyl methacrylate, styrene and emulsifier B in a mass ratio of (10-14): (8-10): (10-12): (0.7-1.6); the initiator C is pre-dissolved in the mixed liquid C; after the emulsifier B is dissolved in water to prepare an aqueous solution, it is evenly mixed with the initiator C to obtain the mixed liquid C; The buffer is pre-dissolved in the seed emulsion and then stirred and mixed with the initiator B to obtain a mixed system. The pre-emulsified liquid is then added dropwise to the mixed system and stirred and dispersed. The pH is adjusted to 6.8-7.2 and filtered. Ethanolamine and inorganic fillers are then added and uniformly dispersed to obtain a temporary coating.
2. The method for preparing a temporary coating material according to claim 1, It is characterized in that The emulsifier A and the emulsifier B independently include an anionic emulsifier and a nonionic emulsifier.
3. A temporary coating material prepared by the method for preparing a temporary coating material according to any one of claims 1 to 2.
4. An application of a temporary coating prepared by the method for preparing a temporary coating as described in any one of claims 1 to 2 on the surface of a nuclear fuel zirconium alloy cladding.