A method for preparing iron phosphate and co-producing silicon-aluminum composite filler using Bayer red mud

By mixing red mud with alkali, calcining, water quenching and acid leaching reaction, efficient separation and recovery of iron and aluminum in Bayer red mud was achieved, and low acid consumption and low silicon-aluminum composite fillers were prepared for iron phosphate and silicon-aluminum composite fillers. The alkali consumption process solves the problems of high energy consumption and low resource utilization in the prior art.

CN117049490BActive Publication Date: 2024-12-06ALUMINUM CORP OF CHINA LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311023403.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-08-15
Publication Date
2024-12-06
Estimated Expiration
2043-08-15

AI Technical Summary

Technical Problem

The prior art has problems such as high energy consumption, complex acid leachate composition, difficult separation of iron and aluminum, and large alkali consumption when recycling iron and aluminum by Bayer method red mud. The existence of iron and aluminum in red mud affects the leaching of iron phosphate. and extraction, it is difficult to achieve efficient resource utilization.

Method used

The red mud is dried, crushed and mixed with alkali and roasted, and quenched in water to separate solid-liquid. Then the acid leach reaction and alkali liquid are adjusted to adjust the pH to separate iron and aluminum. The impurities are removed by sodium fluoride, and finally the phosphorus source is added and the pH is adjusted. Prepare iron phosphate dihydrate and silicon-aluminum composite filler to achieve a process flow with low acid and low alkali consumption.

Benefits of technology

The efficient separation and recycling of iron and aluminum in red mud is achieved. The prepared iron phosphate can be used in lithium iron phosphate batteries and other fields. Silicon-aluminum composite filler can be used in papermaking and other fields. The process is simple, the operability is strong, and the product added value is high, which reduces the acid and alkali consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
Patent Text Reader

Abstract

The invention discloses a method for preparing iron phosphate co-production silicon-aluminum composite filler from red mud of Bayer process, comprising the following steps: (1) drying and crushing red mud into fine powder, mixing alkali and red mud fine powder to obtain a first mixed material; (2) roasting the first mixed material at 500-1100°C to obtain a second material; (3) quenching the second material, and separating the solid and liquid to obtain a third material and a first leachate; (4) adding an acid solution to the third material, performing an acid leaching reaction under heating, and filtering to obtain an iron-containing acid leaching solution; (5) adding sodium fluoride to the acid leaching solution for dealuminization and impurity removal, supplementing a phosphorus source, adding an alkaline solution to adjust pH, standing, filtering, washing and drying a precipitate to obtain a dihydrated iron phosphate; (6) introducing carbon dioxide into the first leachate for carbon fractionation reaction, and filtering to obtain a second leachate and a silicon-aluminum composite filler. The method of the present invention can simultaneously realize the separation and recycling of iron and aluminum, and has the effects of low acid consumption and low alkali consumption.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of resource utilization of solid waste from alumina production, and specifically relates to a method for preparing iron phosphate and co-producing silicon-aluminum composite filler from Bayer process red mud. Background Art

[0002] Bayer red mud is a highly alkaline waste residue obtained after bauxite is refined into alumina by the Bayer process. It is similar in appearance to red soil and is rich in iron oxide, so it is called red mud. According to the characteristics of bauxite and process conditions, about 1.0 to 2.5 tons of red mud are produced for every ton of alumina produced. Due to its high alkalinity content, complex composition and difficulty in direct utilization, red mud is a large solid waste with low comprehensive utilization rate. Most of the red mud is disposed of in the form of stockpiling, which is easy to cause pollution to the surrounding environment of the stockpile and has gradually become a bottleneck restricting the sustainable development of the alumina industry.

[0003] The main components of Bayer red mud are Fe2O3, Al2O3, SiO2, CaO, Na2O, TiO2, etc., among which the iron content is very high, and it is a solid waste with great development potential. At present, the main methods for recovering iron in red mud are magnetic separation after reduction roasting and wet concentrated acid leaching. For example, CN112609074A proposes "A method for recovering iron, aluminum and sodium from Bayer red mud", which is to mix red mud with mineralizer magnesium oxide, dolomite and reducing agent in proportion and press them into blocks, and then subject them to high-temperature reduction magnetization-salination roasting. The roasting product is first magnetically separated and then leached with a dilute alkaline solution to obtain medium-grade iron concentrate and sodium aluminate solution, but the recovery rate after magnetic separation is not high and the energy consumption is large; CN112795784A discloses "A method for comprehensive recovery of valuable components in red mud", which is to mix red mud with ammonium sulfate and sulfuric acid and roast it to convert the valuable metals in the red mud into soluble sulfates, and then sequentially undergo reduction hydrolysis, extraction stripping, precipitation Operations such as precipitation and re-dissolution can achieve the separation of valuable components, but the steps are cumbersome and not conducive to industrialization; CN113860278A discloses "A method for preparing battery-grade iron phosphate using high-iron Bayer red mud as an iron source", which uses sulfuric acid leaching to leach iron and aluminum, and adjusts the pH in two stages. The first stage of the acid leaching liquid adjusts the pH to 3.5-5.5 to form an iron and aluminum co-precipitate, and the second stage adjusts the pH of the filter residue (iron and aluminum co-precipitate) to 12±0.5 to separate iron and aluminum, obtain an iron hydroxide filter cake, and add phosphoric acid to prepare iron phosphate, which achieves high-price recovery of iron, but the sulfuric acid concentration used for acid leaching in this method is high, and the amount of alkali required for the two-step pH adjustment is large. The presence of iron and aluminum in red mud affects the leaching and extraction of scandium and rare earths. He Ruiming et al. designed a technical solution for the coordinated recovery of aluminum and iron by reduction sintering. Under optimal conditions, aluminosilicate minerals are converted into sodium aluminate, and sodium aluminate solution is obtained by alkali leaching, which can be used to prepare polyaluminum chloride products later. The iron-containing complex minerals in the red mud are converted into magnetic magnetite and elemental iron, and the iron-containing minerals are recovered by magnetic separation, achieving an iron recovery rate of 90.27%, an iron concentrate grade of 73.97%, and an aluminum dissolution rate of 96.28%. This method achieves the coordinated recovery of iron and aluminum, but has the disadvantages of high energy consumption and low product added value.

[0004] With the large-scale application of lithium iron phosphate batteries, the demand for iron phosphate is also increasing. Using Bayer red mud to provide iron sources to prepare iron phosphate broadens the resource utilization of red mud and has good application prospects. The main pain points of the current method of recovering iron from red mud and preparing iron phosphate are: direct concentrated acid leaching, which consumes a large amount of acid; the acid leaching solution has complex components and is difficult to separate iron and aluminum. If the iron-aluminum co-precipitation method is used for precipitation, the alkali consumption is large. Summary of the invention

[0005] The purpose of the present invention is to provide a method for preparing iron phosphate and co-producing silicon-aluminum composite filler from Bayer process red mud. The method of the present invention can simultaneously realize the separation and recycling of iron and aluminum. The prepared iron phosphate can be used in the fields of raw materials, catalysts, ceramics, etc. for lithium iron phosphate batteries, and the silicon-aluminum composite filler can be used in the fields of papermaking, etc. It has the effects of low acid consumption and low alkali consumption, and opens up a new way for preparing iron phosphate using red mud as an iron source.

[0006] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0007] The method for preparing iron phosphate and co-producing silicon-aluminum composite filler from Bayer red mud comprises the following steps:

[0008] ⑴, drying and crushing the red mud into fine powder, and mixing the alkali and the red mud fine powder in a mass ratio of 0.1-2:1 to obtain a first mixed material;

[0009] (2) calcining the first mixed material at 500-1100° C. to obtain a second material;

[0010] (3) quenching the second material with water, and performing solid-liquid separation to obtain the third material and the first leachate;

[0011] (4) adding an acid solution to the third material, performing an acid leaching reaction under heating, and filtering to obtain an iron-containing acid leaching solution after the reaction is completed;

[0012] ⑸. Add alkali solution to the acid leaching solution to adjust the pH to 0.2-3, add sodium fluoride to dealuminate and remove impurities, separate the solid and liquid, and obtain a dealuminized acid leaching solution;

[0013] (6) Add a phosphorus source to the dealuminization acid leaching solution, add an acid solution to adjust the pH to 1-2.5, let stand, filter, take the precipitate, wash, and dry to obtain ferric phosphate dihydrate; add acid to the filtered liquid to adjust the pH, and then return it to step (4) for recycling;

[0014] (7) introducing carbon dioxide into the first leaching solution to carry out a carbonization reaction, and filtering to obtain a second leaching solution and a silicon-aluminum composite filler.

[0015] In the step (1), the base used is one or a mixture of more than one of Na2CO3, NaOH, NaHCO3, KOH, Mg(OH)2, and NH3·H2O.

[0016] In the step (2), the roasting time is 30-180 min.

[0017] The conditions of water quenching in step (3) are: temperature of 30-90° C., time of 5-30 min, and solid-liquid ratio of 1:3-10.

[0018] In the step (4), the acid solution added is a mixed acid solution of one or more of hydrochloric acid, nitric acid, sulfuric acid and phosphoric acid, and the concentration of the acid solution is 2-10 mol / L.

[0019] In the step (4), the conditions for the acid leaching reaction are: temperature of 60-120° C., time of 1-8 h, and a solid-liquid ratio of the third material to the acid of 1:5-14.

[0020] In the step (5), the alkali solution is sodium hydroxide with a concentration of 0.5-17 mol / L, and the conditions for adding sodium fluoride for dealumination and impurity removal are: temperature of 10-70°C, time of 1-90 min, and the molar ratio of fluoride ions to aluminum elements in the acid leaching solution is 3-18:1.

[0021] In step (6), the supplemented phosphorus source is phosphoric acid or sodium dihydrogen phosphate, and the process of adding acid-base solution to adjust pH is: standing at a temperature of 50-90° C. for 2-6 hours. The acid solution is any one of sulfuric acid, hydrochloric acid, and nitric acid. The alkaline solution is any one of sodium hydroxide and ammonia water.

[0022] In the step (7), the reaction conditions of the carbonization reaction are: a carbon dioxide ventilation rate of 0.1-0.6 L / min and a temperature of 30-70°C.

[0023] In the step (7), the second leachate is concentrated, crystallized and dried, and the obtained alkali is recycled and used in steps (1) and (5).

[0024] The present invention has the following advantages:

[0025] (1) The present invention uses Bayer red mud as raw material, adds alkali for high-temperature roasting, and water quenching to achieve the first separation of iron and aluminum, while improving the leaching rate of iron in acid leaching. In addition, the consumption of acid and alkali can be greatly reduced by recycling the alkali and acid solution.

[0026] (2) The present invention utilizes Bayer red mud to produce iron phosphate and co-produce silicon-aluminum composite fillers. Among them, iron phosphate can be used in the fields of raw materials, catalysts, ceramics, etc. of lithium iron phosphate batteries; the main component of the silicon-aluminum composite filler is a mixture of aluminum hydroxide and white carbon black, which can be used in the fields of papermaking, etc., realizing the efficient resource recycling of iron and aluminum in red mud, and having the characteristics of simple process flow, strong operability and high product added value. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is the XRD spectrum of the iron phosphate dihydrate prepared in Example 4 after calcination and dehydration at 650°C; DETAILED DESCRIPTION

[0028] In order to facilitate a better understanding of the present invention, the following examples are used to illustrate the present invention. These examples belong to the protection scope of the present invention, but do not limit the protection scope of the present invention.

[0029] The red mud components used in the following examples are shown in Table 1.

[0030] Table 1 Chemical composition of red mud (wt.%)

[0031] Fe Ca Al Na Si Ti 19.75 9.843 6.69 4.418 4.313 2.879

[0032] Example 1

[0033] The method for preparing iron phosphate and co-producing silicon-aluminum composite filler from Bayer red mud comprises the following steps:

[0034] (1) Drying and crushing the red mud into fine powder, and mixing the alkali and the red mud fine powder in a mass ratio of 0.1:1 to obtain a first mixed material;

[0035] The base used is a mixture of Na2CO3, NaOH, and NaHCO3.

[0036] (2) calcining the first mixed material at 500° C. for 30 min to obtain a second material;

[0037] (3) quenching the second material with water, and performing solid-liquid separation to obtain the third material and the first leachate;

[0038] The conditions for water quenching are: temperature 30°C, time 5 min, and solid-liquid ratio 1:3.

[0039] (4) adding an acid solution to the third material, performing an acid leaching reaction under heating, and filtering to obtain an iron-containing acid leaching solution after the reaction is completed; the added acid solution is a mixed acid solution of hydrochloric acid and nitric acid, and the concentration of the acid solution is 2 mol / L.

[0040] The conditions of the acid leaching reaction are: temperature of 60° C., time of 1 h, and a solid-liquid ratio of the third material to the acid of 1:5.

[0041] (5) Add alkali solution to the acid leaching solution to adjust the pH to 0.2, add sodium fluoride to dealuminate and remove impurities, separate the solid and liquid, and obtain a dealuminized acid leaching solution;

[0042] The alkali solution is sodium hydroxide with a concentration of 0.5 mol / L. The conditions for adding sodium fluoride for dealumination and impurity removal are: temperature of 10° C., time of 1 min, and a molar ratio of fluoride ions to aluminum elements in the acid leaching solution of 3:1.

[0043] (6) Add a phosphorus source to the dealuminization acid leaching solution, add an acid solution to adjust the pH to 1, let it stand, filter, take the precipitate, wash, and dry to obtain ferric phosphate dihydrate; add acid to the filtered liquid to adjust the pH, and then return it to step (4) for recycling;

[0044] The supplemented phosphorus source is phosphoric acid, and the process of adding acid-base solution to adjust pH is: standing for 2 hours at a temperature of 50°C. The acid solution is nitric acid. The base solution is sodium hydroxide.

[0045] (7) introducing carbon dioxide into the first leaching solution to carry out a carbonization reaction, and filtering to obtain a second leaching solution and a silicon-aluminum composite filler.

[0046] The reaction conditions of the carbonization reaction were: a carbon dioxide ventilation rate of 0.1 L / min and a temperature of 30°C.

[0047] The second leachate is concentrated, crystallized and dried, and the obtained alkali is recycled and used in steps (1) and (5).

[0048] Example 2

[0049] The method for preparing iron phosphate and co-producing silicon-aluminum composite filler from Bayer red mud comprises the following steps:

[0050] (1) Drying and crushing the red mud into fine powder, and mixing the alkali and the red mud fine powder in a mass ratio of 2:1 to obtain a first mixed material;

[0051] The base used was a mixture of KOH, Mg(OH)2, and NH3·H2O.

[0052] (2) calcining the first mixed material at 1100° C. for 180 min to obtain a second material;

[0053] (3) quenching the second material with water, and performing solid-liquid separation to obtain the third material and the first leachate;

[0054] The conditions for water quenching are: temperature 90°C, time 30 min, and solid-liquid ratio 1:10.

[0055] (4) adding an acid solution to the third material, performing an acid leaching reaction under heating, and filtering to obtain an iron-containing acid leaching solution after the reaction is completed; the added acid solution is a phosphoric acid solution, and the concentration of the acid solution is 10 mol / L.

[0056] The conditions of the acid leaching reaction are: temperature of 120° C., time of 8 h, and a solid-liquid ratio of the third material to the acid of 1:14.

[0057] (5) Add alkali solution to the acid leaching solution to adjust the pH to 3, add sodium fluoride to dealuminate and remove impurities, separate the solid and liquid, and obtain a dealuminized acid leaching solution;

[0058] The alkali solution is sodium hydroxide with a concentration of 17 mol / L. The conditions for adding sodium fluoride for dealumination and impurity removal are: temperature of 70° C., time of 90 min, and a molar ratio of fluoride ions to aluminum elements in the acid leaching solution of 18:1.

[0059] (6) Add a phosphorus source to the dealuminization acid leaching solution, add an acid solution to adjust the pH to 2.5, let it stand, filter, take the precipitate, wash, and dry to obtain ferric phosphate dihydrate; add acid to the filtered liquid to adjust the pH, and then return it to step (4) for recycling;

[0060] The supplemented phosphorus source is sodium dihydrogen phosphate, and the process of adding acid-base solution to adjust pH is: standing for 6 hours at a temperature of 90°C. The acid solution is sulfuric acid. The base solution is ammonia water.

[0061] (7) introducing carbon dioxide into the first leaching solution to carry out a carbonization reaction, and filtering to obtain a second leaching solution and a silicon-aluminum composite filler.

[0062] The reaction conditions of the carbonization reaction are: carbon dioxide ventilation rate of 0.6L / min, temperature of 70°C.

[0063] The second leachate is concentrated, crystallized and dried, and the obtained alkali is recycled and used in steps (1) and (5).

[0064] Example 3

[0065] The method for preparing iron phosphate and co-producing silicon-aluminum composite filler from Bayer red mud comprises the following steps:

[0066] (1) Drying and crushing the red mud into fine powder, and mixing the alkali and the red mud fine powder in a mass ratio of 1:1 to obtain a first mixed material;

[0067] The base used was a mixture of Na2CO3 and Mg(OH)2.

[0068] (2) calcining the first mixed material at 800° C. for 100 min to obtain a second material;

[0069] (3) quenching the second material with water, and performing solid-liquid separation to obtain the third material and the first leachate;

[0070] The conditions of water quenching are: temperature 60°C, time 20 min, and solid-liquid ratio 1:6.

[0071] (4) adding an acid solution to the third material, performing an acid leaching reaction under heating, and filtering to obtain an iron-containing acid leaching solution after the reaction is completed; the added acid solution is a nitric acid solution, and the concentration of the acid solution is 7 mol / L.

[0072] The conditions of the acid leaching reaction are: temperature of 90° C., time of 5 h, and a solid-liquid ratio of the third material to the acid of 1:9.

[0073] (5) Add alkali solution to the acid leaching solution to adjust the pH to 2, add sodium fluoride to dealuminate and remove impurities, separate the solid and liquid, and obtain a dealuminized acid leaching solution;

[0074] The alkali solution is sodium hydroxide with a concentration of 10 mol / L. The conditions for adding sodium fluoride for dealumination and impurity removal are: temperature of 40° C., time of 60 min, and a molar ratio of fluoride ions to aluminum elements in the acid leaching solution of 11:1.

[0075] (6) Add a phosphorus source to the dealuminization acid leaching solution, add an acid solution to adjust the pH to 1.5, let it stand, filter, take the precipitate, wash, and dry to obtain ferric phosphate dihydrate; add acid to the filtered liquid to adjust the pH, and then return it to step (4) for recycling;

[0076] The supplemented phosphorus source is phosphoric acid, and the process of adding acid-base solution to adjust pH is: standing for 4 hours at a temperature of 70°C. The acid solution is hydrochloric acid. The base solution is sodium hydroxide.

[0077] (7) introducing carbon dioxide into the first leaching solution to carry out a carbonization reaction, and filtering to obtain a second leaching solution and a silicon-aluminum composite filler.

[0078] The reaction conditions of the carbonization reaction were: a carbon dioxide ventilation rate of 0.3 L / min and a temperature of 50°C.

[0079] The second leachate is concentrated, crystallized and dried, and the obtained alkali is recycled and used in steps (1) and (5).

[0080] Example 4

[0081] The method for preparing iron phosphate co-production silicon-aluminum composite filler by using Bayer red mud comprises the following steps:

[0082] (1) Drying and crushing the red mud into fine powder below 100 mesh, and mixing the alkali and the red mud fine powder at a mass ratio of 0.2:1 to obtain a first mixed material;

[0083] The base used was NaOH.

[0084] (2) calcining the first mixed material at 700° C. for 80 min to obtain a second material;

[0085] (3) quenching the second material with water, and performing solid-liquid separation to obtain the third material and the first leachate;

[0086] The conditions of water quenching are: temperature 30°C, time 15 min, and solid-liquid ratio 1:4.

[0087] (4) adding an acid solution to the third material, performing an acid leaching reaction under heating, and filtering to obtain an iron-containing acid leaching solution after the reaction is completed; the added acid solution is a sulfuric acid solution, and the concentration of the acid solution is 6 mol / L.

[0088] The conditions of the acid leaching reaction are: temperature of 120° C., time of 2 h, and a solid-liquid ratio of the third material to the acid of 1:5.

[0089] (5) Add alkali solution to the acid leaching solution to adjust the pH to 2, add sodium fluoride to dealuminate and remove impurities, separate the solid and liquid, and obtain a dealuminized acid leaching solution;

[0090] The alkali solution is sodium hydroxide with a concentration of 6 mol / L. The conditions for adding sodium fluoride for dealumination and impurity removal are: temperature of 60° C., time of 70 min, and a molar ratio of fluoride ions to aluminum elements in the acid leaching solution of 7:1.

[0091] (6) Add a phosphorus source to the dealuminization acid leaching solution, add an acid solution to adjust the pH to 1.5, let it stand, filter, take the precipitate, wash, and dry to obtain ferric phosphate dihydrate; add acid to the filtered liquid to adjust the pH, and then return it to step (4) for recycling;

[0092] The supplemented phosphorus source is sodium dihydrogen phosphate, and the process of adding acid-base solution to adjust pH is: standing for 4 hours at a temperature of 70°C. The acid solution is sulfuric acid. The base solution is ammonia water.

[0093] (7) introducing carbon dioxide into the first leaching solution to carry out a carbonization reaction, and filtering to obtain a second leaching solution and a silicon-aluminum composite filler.

[0094] The reaction conditions of the carbonization reaction were: a carbon dioxide ventilation rate of 0.2 L / min and a temperature of 30°C.

[0095] The second leachate is concentrated, crystallized and dried, and the obtained alkali is recycled and used in steps (1) and (5).

[0096] According to the test, the iron leaching rate of this embodiment reaches 85%, and the recovery rate of water-quenched aluminum is 10%.

[0097] Example 5

[0098] The method for preparing iron phosphate and co-producing silicon-aluminum composite filler from Bayer red mud comprises the following steps:

[0099] (1) Drying, crushing and grinding the red mud into fine powder with a particle size of less than 100 mesh, and mixing the alkali and the red mud fine powder in a mass ratio of 0.4:1 to obtain a first mixed material;

[0100] The base used was a mixture of Na2CO3, NaOH, and KOH.

[0101] (2) calcining the first mixed material at 850° C. for 130 min to obtain a second material;

[0102] (3) quenching the second material with water, and performing solid-liquid separation to obtain the third material and the first leachate;

[0103] The conditions of water quenching are: temperature of 50°C, time of 10 min, and solid-liquid ratio of 1:8.

[0104] (4) adding an acid solution to the third material, performing an acid leaching reaction under heating, and filtering to obtain an iron-containing acid leaching solution after the reaction is completed; the added acid solution is a sulfuric acid solution, and the concentration of the acid solution is 6 mol / L.

[0105] The conditions of the acid leaching reaction are: temperature of 100° C., time of 2 h, and a solid-liquid ratio of the third material to the acid of 1:5.

[0106] (5) Add alkali solution to the acid leaching solution to adjust the pH to 2, add sodium fluoride to dealuminate and remove impurities, separate the solid and liquid, and obtain a dealuminized acid leaching solution;

[0107] The alkali solution is sodium hydroxide with a concentration of 3 mol / L. The conditions for adding sodium fluoride for dealumination and impurity removal are: temperature of 60° C., time of 40 min, and a molar ratio of fluoride ions to aluminum elements in the acid leaching solution of 15:1.

[0108] (6) Add a phosphorus source to the dealuminization acid leaching solution, add an acid solution to adjust the pH to 2, let it stand, filter, take the precipitate, wash, and dry to obtain ferric phosphate dihydrate; add acid to the filtered liquid to adjust the pH, and then return it to step (4) for recycling;

[0109] The supplemented phosphorus source is phosphoric acid, and the process of adding acid-base solution to adjust pH is: standing for 5 hours at a temperature of 55°C. The acid solution is nitric acid. The base solution is ammonia water.

[0110] (7) introducing carbon dioxide into the first leaching solution to carry out a carbonization reaction, and filtering to obtain a second leaching solution and a silicon-aluminum composite filler.

[0111] The reaction conditions of the carbonization reaction were: a carbon dioxide ventilation rate of 0.2 L / min and a temperature of 30°C.

[0112] The second leachate is concentrated, crystallized and dried, and the obtained alkali is recycled and used in steps (1) and (5).

[0113] According to the test, the iron leaching recovery rate of this embodiment reaches 80%, and the recovery rate of water-quenched aluminum is 40%.

[0114] Example 6

[0115] The method for preparing iron phosphate co-production silicon-aluminum composite filler by using Bayer red mud comprises the following steps:

[0116] (1) Drying, crushing and grinding the red mud into fine powder with a particle size of less than 100 mesh, and mixing the alkali and the red mud fine powder in a mass ratio of 0.6:1 to obtain a first mixed material;

[0117] The base used is a mixture of Na2CO3 and NH3·H2O.

[0118] (2) calcining the first mixed material at 1000° C. for 160 min to obtain a second material;

[0119] (3) quenching the second material with water, and performing solid-liquid separation to obtain the third material and the first leachate;

[0120] The conditions of water quenching are: temperature 60°C, time 25 min, and solid-liquid ratio 1:6.

[0121] (4) adding an acid solution to the third material, performing an acid leaching reaction under heating, and filtering to obtain an iron-containing acid leaching solution after the reaction is completed; the added acid solution is sulfuric acid, and the concentration of the acid solution is 6 mol / L.

[0122] The conditions of the acid leaching reaction are: temperature of 120° C., time of 2 h, and a solid-liquid ratio of the third material to the acid of 1:5.

[0123] (5) Add alkali solution to the acid leaching solution to adjust the pH to 2, add sodium fluoride to dealuminate and remove impurities, separate the solid and liquid, and obtain a dealuminized acid leaching solution;

[0124] The alkali solution is sodium hydroxide with a concentration of 7 mol / L. The conditions for adding sodium fluoride for dealumination and impurity removal are: temperature of 60° C., time of 35 min, and a molar ratio of fluoride ions to aluminum elements in the acid leaching solution of 8:1.

[0125] (6) Add a phosphorus source to the dealuminization acid leaching solution, add an acid solution to adjust the pH to 1.8, let it stand, filter, take the precipitate, wash, and dry to obtain ferric phosphate dihydrate; add acid to the filtered liquid to adjust the pH, and then return it to step (4) for recycling;

[0126] The supplemented phosphorus source is phosphoric acid or sodium dihydrogen phosphate, and the process of adding acid-base solution to adjust pH is: standing for 4 hours at a temperature of 65°C. The acid solution is sulfuric acid. The base solution is sodium hydroxide.

[0127] (7) introducing carbon dioxide into the first leaching solution to carry out a carbonization reaction, and filtering to obtain a second leaching solution and a silicon-aluminum composite filler.

[0128] The reaction conditions of the carbonization reaction were: a carbon dioxide ventilation rate of 0.2 L / min and a temperature of 30°C.

[0129] The second leachate is concentrated, crystallized and dried, and the obtained alkali is recycled and used in steps (1) and (5).

[0130] According to the test, the iron leaching recovery rate of this embodiment reaches 84%, and the recovery rate of water-quenched aluminum is 68%.

[0131] Comparative Example 1

[0132] The main difference between this comparative example and Example 4 is that no soda ash is added for high temperature roasting. In this comparative example, the red mud is not subjected to high temperature roasting treatment, but directly acid leached.

[0133] This comparative example processing method comprises the following steps:

[0134] (1) Dry, crush and grind the red mud to a particle size of less than 100 mesh.

[0135] (2) mixing the red mud obtained in step (1) with a 6 mol / L sulfuric acid solution at a solid-liquid ratio of 1:12 for leaching reaction, heating and stirring at 120° C. for 4 h, and filtering to obtain an iron-containing acid leaching solution;

[0136] The iron leaching rate of this embodiment is 74%. The results show that at the same acid concentration, the iron leaching rate is far less than that of Example 4 when the solid-liquid ratio is increased (the amount of sulfuric acid is increased) and the reaction time is prolonged.

[0137] Comparative Example 2

[0138] The main difference between this comparative example and Example 4 is that no soda ash is added for high temperature roasting. In this comparative example, the red mud is not subjected to high temperature roasting treatment, but directly acid leached.

[0139] This comparative example processing method comprises the following steps:

[0140] (1) Dry, crush and grind the red mud to a particle size of less than 100 mesh.

[0141] (2) mixing the red mud obtained in step (1) with 8 mol / L sulfuric acid solution at a solid-liquid ratio of 1:5 for leaching reaction, heating and stirring at 120° C. for 2 h, and filtering to obtain an iron-containing acid leaching solution;

[0142] The iron leaching rate of this embodiment is 75%. The results show that under the same solid-liquid ratio and reaction time, the iron leaching rate is far less than that of Example 4 when the sulfuric acid concentration is increased.

[0143] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing iron phosphate and co-producing silicon-aluminum composite filler from Bayer red mud, It is characterized in that The following steps are involved: ⑴, drying and crushing the red mud into fine powder, and mixing the alkali and the red mud fine powder in a mass ratio of 0.1-2:1 to obtain a first mixed material; (2) calcining the first mixed material at 500-1100° C. to obtain a second material; (3) quenching the second material with water, and performing solid-liquid separation to obtain the third material and the first leachate; (4) adding an acid solution to the third material, performing an acid leaching reaction under heating, and filtering to obtain an iron-containing acid leaching solution after the reaction is completed; ⑸. Add alkali solution to the acid leaching solution to adjust the pH to 0.2-3, add sodium fluoride to dealuminate and remove impurities, separate the solid and liquid, and obtain a dealuminized acid leaching solution; (6) Add a phosphorus source to the dealuminization acid leaching solution, add an acid solution to adjust the pH to 1-2.5, let stand, filter, take the precipitate, wash, and dry to obtain ferric phosphate dihydrate; add acid to the filtered liquid to adjust the pH, and then return it to step (4) for recycling; (7) introducing carbon dioxide into the first leaching solution to carry out a carbonization reaction, and filtering to obtain a second leaching solution and a silicon-aluminum composite filler.

2. The method for preparing iron phosphate and co-producing silicon-aluminum composite filler from Bayer red mud according to claim 1, Features: In the step (1), the base used is NaOH, KOH, Mg(OH) 2 NH 3 ·H 2 O or a mixture of more than one.

3. The method for preparing iron phosphate and co-producing silicon-aluminum composite filler from Bayer red mud according to claim 1, Features: In the step (2), the roasting time is 30-180 min.

4. The method for preparing iron phosphate and co-producing silicon-aluminum composite filler from Bayer red mud according to claim 1, Features: The conditions of water quenching in step (3) are: temperature of 30-90° C., time of 5-30 min, and solid-liquid ratio of 1:3-10.

5. The method for preparing iron phosphate and co-producing silicon-aluminum composite filler from Bayer red mud according to claim 1, Features: In the step (4), the acid solution added is a mixed acid solution of one or more of hydrochloric acid, nitric acid, sulfuric acid and phosphoric acid, and the concentration of the acid solution is 2-10 mol / L.

6. The method for preparing iron phosphate and co-producing silicon-aluminum composite filler from Bayer red mud according to claim 5, Features: In the step (4), the conditions for the acid leaching reaction are: temperature of 60-120° C., time of 1-8 h, and a solid-liquid ratio of the third material to the acid of 1:5-14.

7. The method for preparing iron phosphate and co-producing silicon-aluminum composite filler from Bayer red mud according to claim 1, Features: In the step (5), the alkali solution is sodium hydroxide with a concentration of 0.5-17 mol / L, and the conditions for adding sodium fluoride for dealumination and impurity removal are: temperature of 10-70°C, time of 1-90 min, and the molar ratio of fluoride ions to aluminum elements in the acid leaching solution is 3-18:

1.

8. The method for preparing iron phosphate and co-producing silicon-aluminum composite filler from Bayer red mud according to claim 1, Features: In the step (6), the supplemented phosphorus source is phosphoric acid or sodium dihydrogen phosphate, and the process of adding acid-base solution to adjust the pH is: standing at a temperature of 50-90°C for 2-6 hours, the acid solution is any one of sulfuric acid, hydrochloric acid, and nitric acid, and the alkaline solution is any one of sodium hydroxide and ammonia water.

9. The method for preparing iron phosphate and co-producing silicon-aluminum composite filler from Bayer red mud according to claim 1, Features: In the step (7), the reaction conditions of the carbonization reaction are: a carbon dioxide ventilation rate of 0.1-0.6 L / min and a temperature of 30-70°C.

10. The method for preparing iron phosphate and co-producing silicon-aluminum composite filler from Bayer red mud according to claim 1, Features: In the step (7), the second leachate is concentrated, crystallized and dried, and the obtained alkali is recycled and used in steps (1) and (5).