A water-based antistatic epoxy floor paint

By combining bisphenol A type epoxy resin, aqueous epoxy curing agent and modified composite conductive materials, the problems of emulsification and curing unevenness of traditional epoxy floor paint and poor compatibility of conductive fillers are solved, and water-based anti-static electricity is achieved The excellent mechanical properties and anti-static properties of epoxy floor paint.

CN117126584BActive Publication Date: 2024-11-08XINJIANG QINGDA COATINGS CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202211539307.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-07-28
Publication Date
2024-11-08
Estimated Expiration
2041-07-28

AI Technical Summary

Technical Problem

Traditional epoxy floor paint has unevenness during emulsification and curing, resulting in a decrease in mechanical properties and poor compatibility with polymers, which makes it impossible to effectively improve anti-static properties.

Method used

Bisphenol A type epoxy resin is used to combine with aqueous epoxy curing agent and composite conductive material, and improve its compatibility and dispersion through modification treatment to form an optimized component A and component B slurry, and mix evenly to Prepare water-based anti-static epoxy floor paint, and use the modification of graphene oxide aerogel and silica nanoparticles to form a conductive network to increase anti-static and mechanical properties.

Benefits of technology

The uniform curing and full cross-linking of epoxy floor paint is achieved, which improves impact resistance and anti-static properties, while enhancing the mechanical properties, ensuring efficient conductive network formation and electrostatic charge removal.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 407345DEST_PATH_IMAGE002
    Figure 407345DEST_PATH_IMAGE002
Patent Text Reader

Abstract

The present invention discloses a water-based antistatic epoxy floor paint. The epoxy floor paint comprises a component A slurry and a component B slurry; the raw materials of the component A slurry comprise the following components: by weight, 86 parts of bisphenol A epoxy resin and 14 parts of active diluent; the raw materials of the component B slurry comprise the following components: by weight, 55 parts of water-based epoxy curing agent, 11 parts of composite conductive material, 0.8 parts of defoaming agent, and 0.2 parts of leveling agent. Excellent effects: (1) Effectively balance the emulsification and curing rates to obtain a water-based epoxy curing agent with dual functions of emulsification and curing; (2) Utilize the three-dimensional structure of the composite conductive material to increase the flow and penetration of the liquid resin; increase the dispersibility of the composite conductive material; construct an effective conductive network to eliminate electrostatic charges and increase antistatic properties; assist the water-based epoxy curing agent in solving the problem of stress concentration; increase page interaction and improve mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of epoxy flooring, in particular to a water-based antistatic epoxy floor paint. Background Art

[0002] The present invention relates to bisphenol A epoxy resin, which is a thermosetting resin with excellent anticorrosive performance and environmental friendliness. Therefore, it is widely used in epoxy floor paint and has been widely used in organic anticorrosive coatings. Traditional epoxy floor paint consists of two components, A and B, and usually a curing agent is a separate component, which is mixed and cured with bisphenol A epoxy resin before use. The water solubility of the materials in the two components and the compatibility between the two components have always been the focus of research. Especially the water solubility of bisphenol A epoxy resin and the compatibility with the curing agent. Therefore, preparing a curing agent with the emulsification function of bisphenol A epoxy resin is one of the ways to solve the problem. However, there is an emulsification rate that is less than the curing rate, which makes the emulsification uneven, the curing is insufficient, the mechanical properties are reduced, and the service life is reduced.

[0003] In addition, due to the increasing market demand for epoxy floor paint functionalization, anti-static is one of the functions. Generally, the anti-static property of epoxy floor paint is increased by adding conductive fillers, but the poor compatibility of conductive fillers and polymers will reduce the mechanical properties of epoxy floor paint. The poor dispersion of conductive fillers cannot form an effective conductive channel on the surface and inside of epoxy floor paint to increase the anti-static property.

[0004] Therefore, solving the above problems and preparing a water-based antistatic epoxy floor paint with excellent mechanical ability is an urgent problem to be solved. Summary of the invention

[0005] The object of the present invention is to provide a water-based antistatic epoxy floor paint and a preparation method thereof to solve the problems raised in the above-mentioned background technology.

[0006] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0007] A water-based antistatic epoxy floor paint, the epoxy floor paint comprising a component A slurry and a component B slurry; the raw materials of the component A slurry comprise the following components: by weight, 82-90 parts of bisphenol A epoxy resin and 12-20 parts of active diluent; the raw materials of the component B slurry comprise the following components: by weight, 50-62 parts of water-based epoxy curing agent, 8-12 parts of composite conductive material, 0.1-2 parts of defoaming agent, and 0.05-2 parts of leveling agent.

[0008] More optimally, the raw materials of the composite conductive material include the following components: by weight, 8 to 12 parts of graphene oxide aerogel, 16 to 24 parts of 3-aminopropyltriethoxysilane, and 40 to 60 parts of silicon dioxide nanoparticles.

[0009] More optimally, the raw materials of the water-based epoxy curing agent include the following components: by weight, 80-95 parts of bisphenol A epoxy resin, 10-15 parts of triethylenetetramine, and 4-8 parts of glycidyl carboxylate.

[0010] More optimally, the epoxy group equivalent of the glycidyl carboxylate is 240 g / mol.

[0011] More preferably, the bisphenol A epoxy resin is bisphenol A epoxy resin.

[0012] More optimally, the mixing ratio of the A component slurry to the B component slurry is (1:0.8) to (1:1).

[0013] More optimally, a method for preparing a water-based antistatic epoxy floor paint comprises the following steps:

[0014] S1: Preparation of composite conductive materials;

[0015] S2: Preparation of waterborne epoxy curing agent;

[0016] S3: Preparation of epoxy floor paint.

[0017] More optimally, the following steps are included:

[0018] S1: Preparation of composite conductive material: (1) Using 3-aminopropyltriethoxysilane to modify the surface of silica nanoparticles to obtain amino-modified silica, which is set aside; (2) Using amino-modified silica to modify the surface of graphene oxide aerogel to obtain a composite conductive material, which is set aside;

[0019] S2: Preparation of water-based epoxy curing agent; reacting triethylenetetramine with bisphenol A epoxy resin solution in a mixed solvent of 2-butoxyethanol and n-butanol, and neutralizing with acetic acid to obtain a water-based epoxy curing agent for standby use;

[0020] S3: Preparation of epoxy floor paint: (1) Mix and disperse the weighed bisphenol A epoxy resin and active diluent in deionized water, and homogenize to obtain component A slurry; (2) Disperse the weighed water-based epoxy curing agent, composite conductive material, defoaming agent, and leveling agent in deionized water in turn, and homogenize to obtain component B slurry; (3) Evenly mix the component A slurry and the component B slurry to obtain epoxy floor paint.

[0021] More optimally, in step S1, the specific steps are: (1) dispersing the weighed 3-aminopropyltriethoxysilane in anhydrous ethanol by stirring, setting the stirring speed to 300-400 rpm and the stirring time to 40-60 minutes; adding an ammonia solution to adjust the pH to 10; adding silica nanoparticles, reacting for 1-2 hours, centrifugally washing, filtering, and drying at 50-55°C to obtain amino-containing silica for later use; (2) ultrasonically dispersing the graphene oxide aerogel in deionized water, adding amino-containing silica, setting the stirring speed to 500-600 rpm; adding ammonia solution to promote dispersion and avoid partial concentrated gelation, setting the reaction temperature to 90-95°C for reaction for 5-6 hours, filtering and washing, and freeze-drying at -30--50°C to obtain a composite conductive material for later use.

[0022] More optimally, in step S2, the specific steps are: dissolving the weighed triethylenetetramine in a mixed solvent of 2-butoxyethanol and n-butanol; adding dropwise 50wt% bisphenol A epoxy resin solution, setting the reaction temperature to 65-68°C and reacting for 4-4.5 hours; adding glycidyl carboxylate to the reaction solution, setting the reaction temperature to 70-75°C and continuing the reaction for 3 hours, and detecting the epoxy conversion rate every 30 minutes; after the reaction is completed, removing the small molecular amine by vacuum distillation, adding acetic acid to neutralize the reaction, filtering, washing, and drying to obtain a water-based epoxy curing agent for standby use.

[0023] More optimally, in step S3, the solid content of the A component slurry is 60wt%; the solid content of the B component slurry is 55wt%.

[0024] In the technical scheme, bisphenol A epoxy resin is used as the main body and mixed with an active diluent to form component A slurry; a water-based epoxy curing agent is prepared with bisphenol A epoxy resin as the matrix, and a composite conductive material, a defoaming agent, and a leveling agent are mixed as component B slurry.

[0025] Among them, the water-based epoxy curing agent has emulsifying properties for bisphenol A epoxy resin, increasing the dispersion of bisphenol A epoxy resin in water; the composite conductive material can effectively increase the antistatic and mechanical properties of epoxy floor paint, and at the same time, assist the water-based epoxy curing agent to increase the curing rate; and the defoaming agent is to eliminate the formation of bubbles and voids during the drying process, effectively enhance the formation of the conductive network of the composite conductive material in the epoxy floor, and effectively prevent static electricity. The details are as follows:

[0026] (1) Water-based epoxy curing agent: Generally, the curing agent has the dual functions of emulsification and curing. Because the curing rate is faster than the emulsification rate, it will cause the curing stress concentration, resulting in reduced strength and cracks.

[0027] In this scheme, in order to increase the compatibility of the curing agent and the epoxy resin, bisphenol A epoxy resin is used as the main body, triethylenetetramine curing agent is grafted, carboxylic acid glycidyl ester is used to stop the reaction, acetic acid is added for neutralization reaction, and a water-based epoxy curing agent with emulsification properties is prepared. Among them, carboxylic acid glycidyl ester is used as a terminator of the reaction, which determines the content of epoxy groups and amino groups in the curing agent and can adjust the curing speed; when its content decreases, the termination rate is too low, the curing speed is too fast, and gaps will be generated; when its content increases, the average particle size of the emulsified epoxy resin emulsion increases, and the dispersibility and water solubility decrease; therefore, its content needs to be controlled. The acetic acid neutralization reaction is to increase the water solubility of the curing agent.

[0028] Among them, the termination reaction of carboxylic acid glycidyl ester weakens the activity of the primary amine on the prepared curing agent molecular chain, reduces the curing rate, allows the dry moisture to fully volatilize, fully cures, increases the cross-linking density, and solves the stress concentration problem; and the long-chain fatty amine in its molecular structure is flexible and can effectively buffer the impact of external instantaneous force, effectively improving the impact resistance of the epoxy floor.

[0029] (2) Composite conductive materials: Inorganic materials have conductivity and can effectively increase the anti-static properties of epoxy flooring. However, they have the disadvantage of poor compatibility with polymers, which will affect the mechanical properties of epoxy flooring. Therefore, it is necessary to modify the inorganic materials to synergistically increase the mechanical properties and conductivity of epoxy flooring.

[0030] In this scheme, silane coupling agent is used to wrap silica nanoparticles, and amino groups are generated around them, which react with some hydroxyl or carboxyl groups on the surface of graphene oxide aerogel and anchor on its surface to obtain a conductive composite material. Graphene oxide aerogel is a three-dimensional structured material with low density and high structural stability. The existence of the three-dimensional structure: first, it ensures the dispersibility of graphene sheets, which is conducive to the flow and penetration of liquid resin, and can build an effective conductive network. Through the conductive network, electron transfer is implemented, static charge is eliminated, and antistatic properties are increased; second, due to the continuous multi-void structure, stress transfer during epoxy resin curing is promoted, and stress concentration problems are solved synergistically; third, the interface interaction is increased, due to the covalent reaction between the introduced active amino group and the epoxy group, and the hydrogen bonding between the oxygen-containing group in its own structure and the epoxy resin; the interface interaction between the composite conductive material and the epoxy resin is enhanced, and the mechanical properties of the epoxy floor are significantly improved. In addition, due to the increase in the abundance of amino groups in the composite conductive material, the hydrophilicity in the aqueous composition is increased; secondly, the ring-opening reaction of the amino groups on the epoxy groups produces secondary crosslinking, which promotes the sufficiency of the curing reaction.

[0031] At the same time, gas stagnation is likely to occur during the drying and curing process, which affects the formation of a conductive network that affects the performance of the epoxy floor. Therefore, adding a defoaming agent can effectively solve the problem and inhibit the formation of bubbles and the generation of voids.

[0032] Compared with the prior art, the beneficial effects achieved by the present invention are as follows: (1) the present invention uses bisphenol A epoxy resin as the main body, grafts triethylenetetramine curing agent, uses carboxylic acid glycidyl ester to stop the reaction, and adds acetic acid to neutralize the reaction to prepare a water-based epoxy curing agent with emulsification properties. It effectively balances the emulsification and curing rates and improves the impact resistance of epoxy flooring; (2) Silane coupling agent is used to modify silica nanoparticles to form nanoparticles surrounded by surface amino groups, and the formed amino groups are used to modify the surface of graphene oxide aerogel to obtain a composite conductive material; the three-dimensional structure of graphene oxide aerogel is used to increase the flow and penetration of liquid resin; the dispersibility of composite conductive materials is increased; an effective conductive network is constructed to eliminate electrostatic charges and increase antistatic properties; assists water-based epoxy curing agents in solving stress concentration problems; increases page interactions and improves mechanical properties. DETAILED DESCRIPTION

[0033] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0034] Embodiment 1:

[0035] A method for preparing a water-based antistatic epoxy floor paint comprises the following steps:

[0036] S1: Preparation of composite conductive material: (1) Disperse 21 parts of 3-aminopropyltriethoxysilane in anhydrous ethanol with stirring, set the stirring speed to 400 rpm, and the stirring time to 40 minutes; add ammonia solution to adjust the pH to 10; add 46 parts of silica nanoparticles, react for 1 hour, centrifuge, wash, filter, and dry at 55°C to obtain amino silica for use; (2) Ultrasonic disperse 8 parts of graphene oxide aerogel in deionized water, add amino silica, set the stirring speed to 500 rpm; add ammonia water, set the reaction temperature to 90°C, react for 5 hours, filter, wash, and freeze-dry at -50°C to obtain a composite conductive material for use.

[0037] S2: Preparation of water-based epoxy curing agent; 12 parts of triethylenetetramine are dissolved in a mixed solvent of 2-butoxyethanol and n-butanol; 86 parts of bisphenol A epoxy resin are prepared into a 50wt% bisphenol A epoxy resin solution, and added dropwise to the reaction solution, and the reaction temperature is set to 65°C for 4 hours; 6 parts of glycidyl carboxylate are added to the reaction solution, and the reaction temperature is set to 75°C for 3 hours, and the epoxy conversion rate is detected every 30 minutes; after the reaction is completed, the small molecular amine is removed by vacuum distillation, acetic acid is added to neutralize the reaction, filtered, washed, and dried to obtain a water-based epoxy curing agent for use.

[0038] S3: Preparation of epoxy floor paint: (1) 85 parts of bisphenol A epoxy resin and 14 parts of active diluent were mixed and dispersed in deionized water, and homogenized to obtain component A slurry; (2) 55 parts of water-based epoxy curing agent, 11 parts of composite conductive material, 0.8 parts of defoaming agent, and 0.2 parts of leveling agent were dispersed in deionized water in sequence, and homogenized to obtain component B slurry. (3) The mixing ratio of component A slurry and component B slurry was 1:0.8 and mixed evenly to obtain epoxy floor paint.

[0039] Embodiment 2:

[0040] A method for preparing a water-based antistatic epoxy floor paint comprises the following steps:

[0041] S1: Preparation of composite conductive material: (1) Disperse 16 parts of 3-aminopropyltriethoxysilane in anhydrous ethanol with stirring, set the stirring speed to 300 rpm, and the stirring time to 40 minutes; add ammonia solution to adjust the pH to 10; add 40 parts of silica nanoparticles, react for 1 hour, centrifuge and wash, filter, and dry at 50°C to obtain amino silica for use; (2) Ultrasonic disperse 8 parts of graphene oxide aerogel in deionized water, add amino silica, set the stirring speed to 500 rpm; add ammonia water, set the reaction temperature to 90°C, react for 5 hours, filter and wash, and freeze-dry at -30°C to obtain a composite conductive material for use.

[0042] S2: Preparation of water-based epoxy curing agent; 10 parts of triethylenetetramine are dissolved in a mixed solvent of 2-butoxyethanol and n-butanol; 80 parts of bisphenol A epoxy resin are prepared into a 50wt% bisphenol A epoxy resin solution, and the solution is added dropwise to the reaction solution, and the reaction temperature is set to 65°C for 4 to 4.5 hours; 4 parts of glycidyl carboxylate are added to the reaction solution, and the reaction temperature is set to 70°C for 3 hours, and the epoxy conversion rate is detected every 30 minutes; after the reaction is completed, the small molecular amine is removed by vacuum distillation, acetic acid is added to neutralize the reaction, filtered, washed, and dried to obtain a water-based epoxy curing agent for use.

[0043] S3: Preparation of epoxy floor paint: (1) 82 parts of bisphenol A epoxy resin and 12 parts of active diluent were mixed and dispersed in deionized water, and homogenized to obtain component A slurry; (2) 50 parts of water-based epoxy curing agent, 8 parts of composite conductive material, 0.1 parts of defoaming agent, and 0.05 parts of leveling agent were dispersed in deionized water in sequence, and homogenized to obtain component B slurry. (3) The mixing ratio of component A slurry and component B slurry was 1:0.8 and mixed evenly to obtain epoxy floor paint.

[0044] Embodiment 3:

[0045] A method for preparing a water-based antistatic epoxy floor paint comprises the following steps:

[0046] S1: Preparation of composite conductive material: (1) Disperse 24 parts of 3-aminopropyltriethoxysilane in anhydrous ethanol with stirring, set the stirring speed to 400 rpm, and the stirring time to 60 minutes; add ammonia solution to adjust the pH to 10; add 60 parts of silica nanoparticles, react for 2 hours, centrifuge, wash, filter, and dry at 55°C to obtain amino silica for use; (2) Ultrasonic disperse 12 parts of graphene oxide aerogel in deionized water, add amino silica, set the stirring speed to 600 rpm; add ammonia water, set the reaction temperature to 95°C, react for 6 hours, filter, wash, and freeze-dry at -50°C to obtain a composite conductive material for use.

[0047] S2: Preparation of water-based epoxy curing agent; 15 parts of triethylenetetramine are dissolved in a mixed solvent of 2-butoxyethanol and n-butanol; 95 parts of bisphenol A epoxy resin are prepared into a 50wt% bisphenol A epoxy resin solution, and the solution is added dropwise to the reaction solution, and the reaction temperature is set to 68°C for 4 to 4.5 hours; 8 parts of glycidyl carboxylate are added to the reaction solution, and the reaction temperature is set to 75°C for 3 hours, and the epoxy conversion rate is detected every 30 minutes; after the reaction is completed, the small molecular amine is removed by vacuum distillation, acetic acid is added to neutralize the reaction, filtered, washed, and dried to obtain a water-based epoxy curing agent for use.

[0048] S3: Preparation of epoxy floor paint: (1) Mix and disperse 90 parts of bisphenol A epoxy resin and 20 parts of active diluent in deionized water, and homogenize to obtain component A slurry; (2) Disperse 62 parts of water-based epoxy curing agent, 12 parts of composite conductive material, 2 parts of defoaming agent, and 2 parts of leveling agent in deionized water in turn, and homogenize to obtain component B slurry. (3) Mix component A slurry and component B slurry in a ratio of 1:1 and mix them evenly to obtain epoxy floor paint.

[0049] Embodiment 4:

[0050] A method for preparing a water-based antistatic epoxy floor paint comprises the following steps:

[0051] S1: Preparation of composite conductive material: (1) Disperse 20 parts of 3-aminopropyltriethoxysilane in anhydrous ethanol with stirring, set the stirring speed to 350 rpm, and the stirring time to 50 min; add ammonia solution to adjust the pH to 10; add 50 parts of silica nanoparticles, react for 1.5 hours, centrifuge, wash, filter, and dry at 52°C to obtain amino silica for use; (2) Ultrasonic disperse 10 parts of graphene oxide aerogel in deionized water, add amino silica, set the stirring speed to 550 rpm; add ammonia solution, set the reaction temperature to 92°C for reaction for 5-6 hours, filter, wash, and freeze-dry at -40°C to obtain a composite conductive material for use.

[0052] S2: Preparation of water-based epoxy curing agent; 13 parts of triethylenetetramine were dissolved in a mixed solvent of 2-butoxyethanol and n-butanol; 88 parts of bisphenol A epoxy resin were prepared into a 50wt% bisphenol A epoxy resin solution, and added dropwise to the reaction solution, and the reaction temperature was set to 66°C for 4.25 hours; 6 parts of glycidyl carboxylate were added to the reaction solution, and the reaction temperature was set to 73°C for 3 hours, and the epoxy conversion rate was detected every 30 minutes; after the reaction was completed, the small molecular amine was removed by vacuum distillation, acetic acid was added to neutralize the reaction, filtered, washed, and dried to obtain a water-based epoxy curing agent for use.

[0053] S3: Preparation of epoxy floor paint: (1) 86 parts of bisphenol A epoxy resin and 16 parts of active diluent were mixed and dispersed in deionized water, and homogenized to obtain component A slurry; (2) 56 parts of water-based epoxy curing agent, 10 parts of composite conductive material, 1 part of defoamer, and 1 part of leveling agent were dispersed in deionized water in sequence, and homogenized to obtain component B slurry. (3) The mixing ratio of component A slurry and component B slurry was 1:0.9 and mixed evenly to obtain epoxy floor paint.

[0054] Example 5: The amount of glycidyl carboxylate added is reduced to 2 parts; the rest is the same as Example 1;

[0055] Example 6: The amount of glycidyl carboxylate added was increased to 10 parts; the rest was the same as Example 1;

[0056] Example 7: The graphene oxide aerogel is replaced by a graphene oxide monolith; the rest is the same as Example 1;

[0057] Example 8: Graphene aerogel is used directly without surface modification; the rest is the same as Example 1;

[0058] Experiment: A water-based antistatic epoxy floor paint prepared in Examples 1 to 8 was applied to a concrete sample and subjected to a series of characterizations. (1) According to the SJ / T10694-2006 standard method, its surface resistivity and volume resistivity were tested to determine the antistatic performance; (2) According to the GB / T9286 standard method, its adhesion was tested; (3) According to the GB50212 standard method, its compressive strength was tested; the results are shown in the following table:

[0059]

[0060] Conclusion: From the data of Examples 1 to 4, it can be seen that the prepared water-based antistatic epoxy floor paint has lower conductivity, higher compressive strength and adhesion, indicating that it has excellent antistatic and mechanical properties. The more preferred solution is Example 1.

[0061] In Example 5 and Example 6, the water-based epoxy curing agent used is respectively an embodiment of reducing and increasing the amount of terminator carboxylic acid glycidyl ester, and it can be found that both compressive strengths are reduced. The resistivity of Example 5 decreases more significantly than that of Example 6, because carboxylic acid glycidyl ester is used as a terminator for the reaction, which determines the content of epoxy groups and amino groups in the curing agent and can adjust the curing speed; when its content is reduced, the termination rate is too low, the curing speed is too fast, and gaps will be generated, so that the mechanical properties are reduced, the internal conductive network is disconnected, and the resistivity is increased. The reason for the decrease in data in Example 6 is that the average particle size of the emulsified epoxy resin emulsion increases, the dispersibility and water solubility decrease, resulting in a decrease in compressive strength.

[0062] And embodiment 7 is the embodiment of graphene oxide monolithic replacement graphene oxide aerogel. From the data, the resistivity and compressive strength are slightly decreased. The reason is that graphene aerogel has a three-dimensional porous structure, which effectively increases the flow and penetration of liquid resin, increases the dispersibility of composite conductive materials, facilitates the formation of conductive networks, and increases antistatic properties. And graphene oxide monolithic easily causes stacking and is not easy to disperse. And it has no three-dimensional structure, which inhibits stress transfer and effectively reduces mechanical properties. And the data of embodiment 8 are also slightly decreased, and the adhesion ability is decreased. The reason is that, without modification, the water solubility and dispersibility of the composite conductive material are reduced, and the amino abundance in the molecular structure is reduced, so the mechanical strength and adhesion are reduced.

[0063] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A water-based antistatic epoxy floor paint, characterized in that: The epoxy floor paint comprises a component A slurry and a component B slurry; the raw materials of the component A slurry comprise the following components: 85 parts by weight of bisphenol A epoxy resin and 14 parts of active diluent; The raw materials of the B component slurry include the following ingredients: by weight, 55 parts of waterborne epoxy curing agent, 11 parts of composite conductive material, 0.8 parts of defoaming agent, and 0.2 parts of leveling agent; The raw materials of the composite conductive material include the following components: by weight, 8 parts of graphene oxide aerogel, 21 parts of 3-aminopropyltriethoxysilane, and 46 parts of silicon dioxide nanoparticles; The raw materials of the waterborne epoxy curing agent include the following components: by weight, 86 parts of bisphenol A epoxy resin, 12 parts of triethylenetetramine, and 6 parts of glycidyl carboxylate; the epoxy group equivalent of the glycidyl carboxylate is 240 g / mol; The mixing mass ratio of the A component slurry to the B component slurry is 1:0.8; The preparation method of the floor paint comprises the following steps: S1: Preparation of composite conductive material: (1) Disperse 21 parts of 3-aminopropyltriethoxysilane in anhydrous ethanol with stirring, set the stirring speed to 400 rpm, and the stirring time to 40 minutes; add ammonia solution to adjust the pH to 10; add 46 parts of silica nanoparticles, react for 1 hour, centrifuge, wash, filter, and dry at 55°C to obtain amino silica for use; (2) Ultrasonic disperse 8 parts of graphene oxide aerogel in deionized water, add amino silica, set the stirring speed to 500 rpm; add ammonia solution, set the reaction temperature to 90°C, react for 5 hours, filter, wash, and freeze-dry at -50°C to obtain a composite conductive material for use; S2: Preparation of water-based epoxy curing agent; 12 parts of triethylenetetramine were weighed and dissolved in a mixed solvent of 2-butoxyethanol and n-butanol; 86 parts of bisphenol A epoxy resin were weighed to prepare a 50wt% bisphenol A epoxy resin solution, which was added dropwise to the reaction solution, and the reaction temperature was set to 65°C for 4 hours; 6 parts of glycidyl carboxylate were added to the reaction solution, and the reaction temperature was set to 75°C for 3 hours, and the epoxy conversion rate was detected every 30 minutes; after the reaction was completed, the small molecular amine was removed by vacuum distillation, acetic acid was added for neutralization, filtered, washed, and dried to obtain a water-based epoxy curing agent for standby use; S3: Preparation of epoxy floor paint: (1) 85 parts of bisphenol A epoxy resin and 14 parts of active diluent are mixed and dispersed in deionized water, and homogenized to obtain component A slurry; (2) 55 parts of water-based epoxy curing agent, 11 parts of composite conductive material, 0.8 parts of defoaming agent, and 0.2 parts of leveling agent are dispersed in deionized water in sequence, and homogenized to obtain component B slurry; (3) Mix the A component slurry and the B component slurry in a ratio of 1:0.8 and mix them evenly to obtain epoxy floor paint.

Citation Information

Patent Citations

  • Graphene antistatic floor paint and preparation method thereof

    CN109096870A

  • Corrosion-resistant waterborne epoxy floor paint and preparation method thereof

    CN112409885A

  • Epoxy wear-resistant floor for underground parking garage and processing technology of epoxy wear-resistant floor

    CN112876941A