Method for recovering aluminum solid phase purification
Solid-phase purification in aluminum recycling using high-temperature molten salt electrolytes solves the problems of low purity and high energy consumption caused by the accumulation of chemical elements in scrap aluminum, achieves efficient and low-energy aluminum recycling, meets the demand for high-quality aluminum, and reduces environmental pollution.
Patent Information
- Application Number
- CN202310986620.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-07
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-08-07
AI Technical Summary
In the existing aluminum recycling technology, the accumulation of chemical elements in scrap aluminum results in low recycling purity, low recycling rate, and high energy consumption. It is difficult to meet the demand for high-quality aluminum and affects environmental protection.
High-temperature molten salt electrolyte is used for solid-phase purification of aluminum in the electrolysis reaction, and high-purity aluminum is recovered on the cathode through a redox reaction, using electrolytes such as magnesium chloride, sodium chloride, potassium chloride, and calcium chloride, combined with calcium fluoride as protection Agent, control the electrolysis temperature and current, and achieve efficient purification of aluminum.
It achieves the effects of wide recycling range, high recycling rate, high purity of recycled aluminum and low energy consumption, meets the demand for high-quality aluminum, and reduces production costs and environmental pollution.
Smart Images

Figure CN117144420B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of aluminum alloys, and in particular to a method for solid-state purification of recycled aluminum. Background Art
[0002] Aluminum alloys are widely used in aviation, aerospace, automobile transportation, construction, medical and other fields due to their low density, high strength, good plasticity, excellent thermal conductivity, electrical conductivity and corrosion resistance. With the development of the economy and society, the demand for aluminum alloys is increasing, and the consumption of aluminum alloys is also increasing year by year, becoming the main metal material at present. According to the research results of literature data, every ton of bauxite mined will consume 5 tons of minerals, destroy 1.314m2 of vegetation, produce 1 ton of alumina will produce 1 ton of red mud, and the power consumption in the electrolysis process of alumina is about 14,000 KW / h, and produce 18Kg of solid waste and 25Kg of hazardous waste. According to the statistics of the International Aluminum Association: In 2018, the global demand for aluminum has reached 95 million tons, of which 64 million tons need to be met by the production of bauxite ore. In view of the high energy consumption and high pollution generated in the production process of aluminum alloys, this will undoubtedly seriously hinder the application process of aluminum alloys and bring great pressure to human environmental protection.
[0003] Due to the energy consumption and environmental pressure brought by the production of primary aluminum, the recycling of scrap aluminum will save 14m3 of water resources per ton, save 3.4t of standard coal, reduce total energy consumption by 20 times, reduce solid waste by 20t, and reduce greenhouse gas emissions by 24 times compared with primary aluminum production. Therefore, the research and application of recycled aluminum will become an effective way to solve the high pollution and high energy consumption of aluminum alloys. In 2018, the global use of recycled aluminum reached 31 million tons. According to the forecast of the International Aluminum Association, by 2050, the global demand for aluminum will increase by 80%. This means that the supply of recycled aluminum will continue to increase, and the demand is expected to reach 70 million tons by 2050.
[0004] Aluminum is the most efficient metal for recycling and reuse. Aluminum can be recycled repeatedly and almost infinitely, making it the most reliable and efficient sustainable material. The International Aluminum Association analyzes the material flow of aluminum every year through a comprehensive global database and an original logistics analysis system. It can trace aluminum waste by product, quality, form and region, including the entire process from the source of waste to terminal consumption. Compared with the production of primary aluminum from bauxite, the energy required to produce recycled aluminum is reduced by 95%, effectively reducing and avoiding pollutant emissions including greenhouse gases. 75% of the world's aluminum is still in use today. Of the nearly 1.5 billion tons of aluminum produced worldwide to date, about 75% is still in use in various applications.
[0005] Aluminum, like iron and copper, is one of the three most widely used precious metals in society. Although aluminum is a very good recycled metal, it is inevitably downgraded by the current recycling process. This is because of the difficulty of refining post-consumer scrap aluminum. The success of aluminum recycling so far has been dependent on the strong demand for downgraded aluminum. Currently, aluminum recycling is mainly achieved through downgrading. After the scrap aluminum is recycled, it is remelted and added with raw aluminum and the alloy composition is adjusted. It is used in the production process of the next level of aluminum castings, such as housings, covers and other parts. Cast aluminum alloys become the final destination of scrap aluminum. In the process of aluminum recycling, a large amount of forged aluminum alloys are continuously downgraded to cast aluminum alloys. At the same time, the social demand for forged aluminum alloys continues to increase, which will inevitably lead to the mining of a large amount of bauxite and electrolysis at the same time to meet the demand for raw aluminum for forged aluminum alloys, which will increase the environmental burden on future society.
[0006] As the recycling and reuse process of scrap aluminum progresses, high-quality aluminum products are downgraded to cast aluminum alloys through remelting after being scrapped. This part of cast aluminum alloy can be used to produce safety parts and structural parts, such as aluminum wheels and steering knuckles. After being scrapped, aluminum safety parts and structural parts are downgraded to thin-walled appearance parts for automobile engine housings and covers through remelting. With the development and widespread application of new energy vehicles, consumers choose battery electric vehicles instead of internal combustion engine vehicles, and the demand for thin-walled appearance parts such as internal combustion engine housings and covers for automobiles has decreased. With the decline in demand for these low-grade recycled aluminum, these low-quality scrap aluminum will eventually become the low end of the aluminum cycle and a social pollutant.
[0007] In industry, aluminum is usually alloyed with silicon, copper, magnesium and other elements, where the content of alloying elements in forging alloys is usually about 5%, while the content of alloying elements in casting alloys is as high as 10-27%, which is much larger than the range of forging alloys. Due to the chemical and physical properties of aluminum, it is almost impossible to remove the alloying elements in aluminum alloys from the aluminum melt by melting, especially alloying elements such as Si, Fe, Mn, and Cu. Therefore, with continuous rounds of recycling, the accumulation of alloying elements in aluminum is inevitable, which means that the chemical composition of recycled aluminum will become more and more complex and more and more difficult to recycle. Low-quality scrap aluminum will be "waste" in the recycling process and difficult to recycle.
[0008] At present, scrap aluminum is mainly recycled by downgrading and remelting. In the recycling process, high-quality forged aluminum alloys are downgraded to low-quality cast aluminum alloys. With the popularization of electric vehicles and the shrinking of the fuel vehicle market, there are a large number of low-quality cast aluminum alloys that are difficult to be recycled. Aluminum alloys contain complex alloying elements, which react with aluminum melt to form high-temperature refractory compounds. It is difficult to remove them by refining, slag removal, etc., which causes the accumulation of these elements during the recycling process, seriously reducing the quality of recycled aluminum. With the increase in demand for high-quality aluminum, such as in the aviation, aerospace, electronics and other industries, the purity of recycled aluminum is difficult to reach the level of original aluminum, increasing dependence on original aluminum, resulting in a large amount of bauxite mining, causing energy waste and environmental pollution.
[0009] In order to meet the society's demand for high-quality aluminum, avoid the development of new bauxite mines, realize the full recycling of waste aluminum, and upgrade waste aluminum to the level of original aluminum to become the raw material of high-quality aluminum, it is necessary to invent a solid-phase purification method for recycled aluminum with a wide recycling range, high recovery rate, low energy consumption, upgrading and recycling, and environmental protection. Summary of the invention
[0010] The purpose of the present invention is to solve the problems of serious accumulation of chemical elements in the process of recycling waste materials, large amount of "waste" of low-quality waste aluminum, low recycling rate, low recycling purity, poor recycling quality, and high recycling energy consumption, and propose a solid phase purification method for recycling aluminum with a wide recycling range, high recovery rate, low energy consumption, upgraded circulation, and environmental protection. The solid phase purification method for recycling aluminum mainly includes parameters such as molten salt electrolyte, waste aluminum anode, pure aluminum cathode, and electrolytic reaction. The present invention mainly electrolyzes waste aluminum in high-temperature molten salt, and maximizes the role of electrolytic purification through parameters such as molten salt electrolyte drying process, molten salt electrolyte component ratio, molten salt electrolyte temperature, cathode and anode size specifications, electrolysis current, and electrolysis voltage, and finally achieves the effects of wide recycling range, high recovery rate, high purity of recycled aluminum, and low energy consumption. The present invention has significant effects on expanding the scope of recycled aluminum, increasing the recovery rate, improving the purity of recycled aluminum, and saving energy consumption. It is a high-quality, wide-range, and low-energy consumption method for recycling aluminum.
[0011] In the face of the difficulties and problems in the current waste aluminum recycling process, the substantial features of our company are as follows:
[0012] The present invention purifies waste aluminum in the solid phase by electrolysis. During the electrolysis process, the temperature of the molten salt electrolyte is much lower than the melting point of the aluminum alloy, thus avoiding the remelting process during the waste aluminum recovery process. In the present invention, waste aluminum does not need to be melted, and electrolysis reaction can be carried out in the solid phase to obtain high-purity aluminum on the cathode. This is the difference between the present invention and other recovery methods.
[0013] The present invention has no requirements for the material of the recycled aluminum anode, as long as the aluminum alloy waste is remelted and prepared into anode-specification thin sheets. Since the electrode potential of Si, Fe, Mn, Cu and other ions in aluminum alloys is higher than that of Al ions, the Al ions in the recycled aluminum anode can be adsorbed on the cathode through reaction under the action of current and voltage, and Si, Fe, Mn, Cu and other ions remain in the anode or molten salt electrolyte. The remaining anode can be remelted to prepare a new anode for electrolytic reaction. The aluminum content in the anode residue is less than 4%, and a high recovery rate of aluminum can be achieved. There is no restriction on the composition and type of aluminum recovered in the solid phase purification process, and any aluminum waste can be electrolytically purified. Secondly, the remaining anode can be recycled to achieve infinite circulation.
[0014] In the present invention, the aluminum recovered from the aluminum anode undergoes an oxidation-reduction reaction under the action of current and voltage, and obtains electrons on the cathode to be converted into Al atoms adsorbed on the surface. Since there are no other ions on the cathode for electrochemical reaction, high-quality aluminum with a purity greater than 99.0% can be obtained on the cathode. According to the law of conservation of energy in the electrolytic reaction, the energy of obtaining pure aluminum by solid phase purification can save more than 50% compared with obtaining raw aluminum by electrolysis of bauxite. Therefore, the requirements of high purity and low energy consumption can be met in the process of electrolytic purification of recycled aluminum.
[0015] In the present invention, the aluminum anode and pure aluminum cathode are recycled and subjected to redox reaction in electrolyte molten salt. The high temperature characteristics and electrochemical characteristics of the electrolyte molten salt can ensure that the A ions in the anode are adsorbed on the cathode during the electrolysis process, and the Fe ions, Mn ions, Si ions and other electrode potentials are higher than the Al ions and remain on the anode surface. Therefore, the electrolyte needs to fully consider the stability of the entire electrolysis reaction process and the electrolysis products. The mass percentage of electrolyte molten salts such as magnesium chloride, sodium chloride, potassium chloride, and calcium chloride and the temperature of the electrolyte molten salt are the differences between the present invention and other waste aluminum recovery methods.
[0016] In the present invention, there are problems such as high electrolysis temperature, serious corrosion to the electrolytic cell, and low electrolyte utilization rate in the solid phase electrolytic purification process of waste aluminum, and an electrolyte protective agent needs to be added to the electrolyte. The addition of calcium fluoride can prevent the boiling of the electrolyte during the electrolysis process, reduce the electrolysis temperature, and maintain a good self-heating balance of the electrolyte, reduce the occurrence of heat tanks, and improve the electrolyte flow performance, thereby improving the current efficiency of the electrolytic cell and reducing production costs. Therefore, calcium fluoride needs to be added in the solid phase purification process of recycled aluminum to ensure that the electrolyte molten salt liquid level is stable and the current efficiency is high.
[0017] In the present invention, the electrolysis reaction is carried out in a high-temperature molten salt electrolyte, so the electrolysis should be dried and mixed evenly. Since the electrolytes magnesium chloride, sodium chloride, potassium chloride, and calcium chloride are relatively easy to absorb moisture and are easily contaminated at room temperature, other ions are mixed into the electrolysis reaction, affecting the redox reaction of Al ions. In the early preparation process of the electrolyte, it is necessary to perform segmented heating and drying under vacuum conditions and mix evenly.
[0018] The beneficial effects of the present invention are:
[0019] At present, due to the mixed types of scrap aluminum, paint on the surface, insufficient pretreatment, and too many types of impurity elements, most of the recycled aluminum melts have low quality. Secondly, the dust, sludge, oil, crystal salt, fiber powder, inorganic coating, rubber, glass and other slag inclusions in the recycled aluminum raw materials are mixed with the melt during the melting process to form various compounds, which are finely dispersed in the melt. At the same time, low-melting point substances such as paint evaporate at high temperatures to produce harmful gases that dissolve in the aluminum liquid. Therefore, it is difficult to purify and improve the quality of recycled aluminum in the conventional remelting process, resulting in the degradation of recycled aluminum and the existence of "waste" aluminum that is difficult to recycle. Secondly, in the process of recycled aluminum remelting, chemical elements such as Fe, Mn, Si, and Cu are difficult to remove from the aluminum melt, resulting in a large accumulation of these elements, which ultimately affects the recycling and reuse of the recycling. At the same time, the accumulation of a large number of chemical elements makes it difficult for the recycled aluminum remelting process to achieve the purity of the original aluminum, and the aluminum waste after remelting cannot meet the demand for high-quality aluminum. Finally, in the process of remelting after the waste aluminum is recovered, the waste aluminum needs to be classified. Forged aluminum alloys and cast aluminum alloys cannot be mixed together for remelting and recycling. A large amount of original aluminum is needed to dilute the elemental components therein, and the dependence on original aluminum is high. Even cast waste aluminum needs to be melted, downgraded and remelted for use with similar chemical composition and use. In the waste aluminum recycling process, the scope of recycled aluminum waste is severely limited, resulting in a large amount of waste aluminum being difficult to recycle. During the melting process, due to the generation of a large amount of scum, the waste aluminum recovery rate is relatively low, and a large amount of hazardous waste is generated. In view of the above problems, the present invention proposes a method for solid-state purification of recycled aluminum with a wide recycling range, high recovery rate, high purity of recycled aluminum, and low energy consumption.
[0020] 1) The present invention uses the action of current and voltage in a high-temperature molten salt electrolyte medium to cause an electrochemical reaction between the anode waste aluminum and the cathode pure aluminum, and an oxidation-reduction reaction occurs on the electrode. Before the reaction begins, the anode waste aluminum mainly includes three parts: an aluminum matrix, a phase rich in (Si, Cu, Zn) and other alloy elements. As the electrolysis process proceeds, the aluminum matrix phase disappears, and the remaining two parts still exist, indicating that the aluminum in the anode can be selectively dissolved. Since the electrode potential of Fe ions, Mn ions, Si ions, etc. is higher than that of Al ions, they will remain on the anode during the electrolysis reaction. Therefore, the electrolysis reaction can achieve the purification of any recycled aluminum. At the same time, after quantitative and qualitative analysis of the anode residue, it can be concluded that more than 96% of the aluminum in the anode can participate in the electrolysis reaction and be recovered. Compared with conventional waste aluminum remelting technology, the present invention has a wider range of waste aluminum recovery, a better recovery rate, and almost no burning loss.
[0021] 2) The present invention is to recycle aluminum solid phase electrolysis and purification. Under the condition that the temperature of the electrolyte cannot be higher than the melting point of the aluminum alloy during the electrolysis process, the anode waste aluminum undergoes an electrochemical redox reaction in a high-temperature molten salt composed of magnesium chloride, sodium chloride, potassium chloride, calcium chloride and calcium fluoride. The chloride ions in the anode aluminum matrix lose electrons and are converted into free Al ions. At the same time, the free Al ions on the cathode gain electrons and are converted into aluminum atoms, so that the Al ions electrolyzed from the anode are recovered on the cathode. After analyzing the aluminum obtained by the electrolytic reaction deposited on the cathode, it was found that its purity was as high as 99.9%. Therefore, the present invention can achieve the effect of upgrading the quality of recycled aluminum and improving the purity of recycled aluminum.
[0022] 3) The purity of aluminum obtained on the cathode of the present invention is more than 99.9%, which is higher than the purity of pure aluminum obtained by electrolysis after the development of bauxite, and can better meet the needs of aviation, aerospace, electronic instruments and scientific research for high-purity aluminum. Secondly, according to the law of conservation of energy in the electrolysis reaction, the solid phase purification of the present invention can save more than 50% of the electricity consumption compared to the electrolysis of bauxite to obtain raw aluminum, and the present invention is solid-state purification and does not require remelting to consume natural gas and other energy sources. Therefore, the present invention can achieve low energy consumption and environmental protection in the process of recycling aluminum purification.
[0023] 4) The electrolyte, waste aluminum, cathode pure aluminum, electrolytic cell, etc. involved in the present invention are all conventional equipment and materials in the industry, and the production processes of these equipment and materials are mature and stable. Therefore, the present invention is easy to implement, economical and practical.
[0024] The recycled aluminum in the present invention is purified by electrolysis. Due to the high electrolysis temperature and large current during the electrolysis process, the present invention has special requirements for electrolyte components and purity that are resistant to high temperatures, have good chemical stability, and are low in corrosion. The types of electrolytes used in the solid phase purification of recycled aluminum are magnesium chloride, sodium chloride, potassium chloride, and calcium chloride, all in powder form, with purity requirements of magnesium chloride>98.0%, sodium chloride>99.0%, potassium chloride>99.6%, and calcium chloride>99.0%.
[0025] In the process of aluminum electrolysis purification, due to the high electrolysis temperature and violent electrolysis reaction, it is necessary to ensure that the electrolyte is dry and evenly mixed. The powdered magnesium chloride, sodium chloride, potassium chloride, and calcium chloride electrolytes are first kept at 180℃-250℃ under vacuum conditions for 72-80 hours, then continue to heat to 300℃-350℃ for 12-18 hours, and finally the dry electrolytes are mixed evenly.
[0026] In the solid phase electrolytic purification process of scrap aluminum, there are problems such as high electrolysis temperature, severe corrosion to the electrolytic cell, and low electrolyte utilization rate. Therefore, an electrolyte protective agent needs to be added to the electrolyte. Calcium fluoride can prevent the boiling of the electrolyte during the electrolysis process, reduce the electrolysis temperature, and maintain a good self-heating balance of the electrolyte, reduce the occurrence of heat sinks, and improve the electrolyte flow performance, thereby improving the current efficiency of the electrolytic cell and reducing production costs. Therefore, the type of electrolyte protective agent is calcium fluoride, and the addition ratio is 2%-6% of the total mass of the electrolyte.
[0027] In electrolytic purification, the electrolyte ratio and electrolysis temperature have a significant impact on the electrolysis product. The present invention is solid-phase electrolytic purification. During the electrolysis process, the temperature of the electrolyte cannot be higher than the melting point of the aluminum alloy, which can save melting costs. Therefore, a specific electrolyte ratio and electrolysis temperature are required. The electrolyte ratio is: magnesium chloride mass percentage 45%-55%, sodium chloride mass percentage 15%-20%, potassium chloride mass percentage 10%-15%, calcium chloride mass percentage 5%-10%, and the electrolyte molten salt temperature during the electrolysis process is 500°C-550°C.
[0028] The recycled aluminum in the high-temperature molten salt electrolyte undergoes an electrolytic reaction under the action of electrolysis, thereby realizing the purification of the recycled aluminum. Therefore, the anode material, cathode material, electrolysis current, and electrolysis voltage in the electrolysis process determine the product of the electrolysis reaction. The anode material is recycled aluminum, a thin sheet prepared by remelting, with a length of 100mm, a width of 30mm, and a thickness of 6mm. The cathode material is a pure aluminum (purity of 98.5%) sheet, and its size specifications are consistent with the anode. The electrolysis current is 10KA-15KA, the electrolysis voltage is 1.8V-2.8V, and the electrolysis reaction time is 2h-4h.
[0029] Therefore, according to the first aspect of the present invention, a method for solid phase purification of aluminum recovery is proposed, wherein the solid phase purification method for aluminum recovery comprises the following steps:
[0030] (a) melting the recycled waste to prepare flakes;
[0031] (b) uniformly mixing magnesium chloride, sodium chloride, potassium chloride, calcium chloride and calcium fluoride in a specific ratio and placing them in an electrolytic cell for heating; and
[0032] (c) Inserting the anode and cathode into an electrolytic cell containing a high-temperature molten salt electrolyte, and applying power when the anode and cathode are at the same temperature as the molten salt electrolyte to collect high-purity aluminum on the cathode.
[0033] According to one embodiment of the present application, before step (a), the method further comprises:
[0034] Dry appropriate amounts of powdered magnesium chloride, sodium chloride, potassium chloride and calcium chloride electrolytes, and cool them under vacuum conditions for later use.
[0035] According to one embodiment of the present application, the purity of magnesium chloride>98.0%, sodium chloride>99.0%, potassium chloride>99.6%, and calcium chloride>99.0%, the magnesium chloride, sodium chloride, potassium chloride, and calcium chloride electrolytes are kept under vacuum conditions at 220°C for 78 hours, and then the temperature is continued to be raised to 330°C and kept for 14 hours.
[0036] According to one embodiment of the present application, the purity of magnesium chloride>98.0%, sodium chloride>99.0%, potassium chloride>99.6%, and calcium chloride>99.0%, the magnesium chloride, sodium chloride, potassium chloride, and calcium chloride electrolytes are kept under vacuum conditions at 180°C for 80 hours, and then the temperature is continued to be raised to 300°C and kept for 18 hours.
[0037] According to one embodiment of the present application, the purity of magnesium chloride>98.0%, sodium chloride>99.0%, potassium chloride>99.6%, and calcium chloride>99.0%, the magnesium chloride, sodium chloride, potassium chloride, and calcium chloride electrolytes are kept at 250°C under vacuum conditions for 72 hours, and then the temperature is continued to be raised to 350°C and kept for 12 hours.
[0038] According to one embodiment of the present application, in step (a), the dimensions of the sheet are: length 100 mm, width 30 mm, thickness 6 mm, and the cathode material uses pure aluminum (purity 98.5%) sheet, and its dimensions are consistent with those of the anode.
[0039] According to one embodiment of the present application, in the step (b), dried magnesium chloride, sodium chloride, potassium chloride and calcium chloride electrolytes are weighed, and the mass percentages thereof are 45% magnesium chloride, 30% sodium chloride, 15% potassium chloride and 10% calcium chloride. At the same time, 2.0% calcium fluoride powder of the total mass of the electrolyte is weighed, and the magnesium chloride, sodium chloride, potassium chloride, calcium chloride and calcium fluoride are evenly mixed and put into an electrolytic cell for heating, and kept warm when heated to 500°C.
[0040] According to one embodiment of the present application, in the step (b), dried magnesium chloride, sodium chloride, potassium chloride and calcium chloride electrolytes are weighed, and the mass percentages thereof are 48% magnesium chloride, 22% sodium chloride, 25% potassium chloride and 5% calcium chloride. At the same time, 4.0% calcium fluoride powder of the total mass of the electrolyte is weighed, and the magnesium chloride, sodium chloride, potassium chloride, calcium chloride and calcium fluoride are evenly mixed and put into an electrolytic cell for heating, and kept warm when heated to 530°C.
[0041] According to one embodiment of the present application, in the step (b), dried magnesium chloride, sodium chloride, potassium chloride and calcium chloride electrolytes are weighed, and the mass percentages thereof are 55% magnesium chloride, 20% sodium chloride, 17% potassium chloride and 8% calcium chloride. At the same time, 6.0% calcium fluoride powder of the total mass of the electrolyte is weighed, and the magnesium chloride, sodium chloride, potassium chloride, calcium chloride and calcium fluoride are evenly mixed and put into an electrolytic cell for heating, and kept warm when heated to 550°C.
[0042] According to one embodiment of the present application, in the step (c), the temperature of the anode and the cathode is measured, and when the temperature of the anode and the cathode is consistent with that of the molten salt electrolyte, power is turned on, wherein the current is 10KA-15KA, the voltage is 1.8V-2.8V, and the electrolysis reaction time is 2h-4h. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] The technical solution of the present invention will be further described in detail below in conjunction with the accompanying drawings and embodiments. In the accompanying drawings, unless otherwise specified, the same reference numerals are used to represent the same components. Among them:
[0044] Figure 1 It is a schematic diagram of a method for solid-state purification of aluminum recovery according to a preferred embodiment of the present invention.
[0045] Figure 2 It is a schematic diagram of the steps of the method for solid-state purification of recovered aluminum according to the above preferred embodiment of the present invention. DETAILED DESCRIPTION
[0046] It should be pointed out that the embodiments shown in the drawings are only used as examples to specifically and vividly explain and illustrate the concept of the present invention. The size and structure thereof are not necessarily drawn to scale, nor do they constitute a limitation to the concept of the present invention.
[0047] The directional terms such as up, down, left, right, front, back, front, back, top, bottom, etc. mentioned or may be mentioned in this specification are defined relative to the structures shown in the various drawings. They are relative concepts and may change accordingly according to different positions and different usage conditions. Therefore, these or other directional terms should not be interpreted as restrictive terms.
[0048] Referring to the drawings of this application specification Figure 1 and Figure 2 As shown, a method for recovering aluminum from the hometown of purification according to one aspect of the present application is explained in the following description. The method for recovering aluminum from the solid phase purification comprises the following steps:
[0049] (a) melting the recycled waste to prepare flakes;
[0050] (b) uniformly mixing magnesium chloride, sodium chloride, potassium chloride, calcium chloride and calcium fluoride in a specific ratio and placing them in an electrolytic cell for heating; and
[0051] (c) Inserting the anode and cathode into an electrolytic cell containing a high-temperature molten salt electrolyte, and applying power when the anode and cathode are at the same temperature as the molten salt electrolyte to collect high-purity aluminum on the cathode.
[0052] In the method for solid phase purification of aluminum recovery described in the present application, the following steps are further included before step (a):
[0053] Dry appropriate amounts of powdered magnesium chloride, sodium chloride, potassium chloride and calcium chloride electrolytes, and cool them under vacuum conditions for later use.
[0054] In the method for solid-phase purification of aluminum recovery described in the present application, in the step (c), the temperature of the anode and the cathode is measured, and when the temperature of the anode and the cathode is consistent with that of the molten salt electrolyte, power is turned on, wherein the current is 10KA-15KA, the voltage is 1.8V-2.8V, and the electrolysis reaction time is 2h-4h. After the electrolysis reaction is completed, the power is cut off, and high-purity aluminum is collected on the cathode, and finally the solid-phase purification process of aluminum recovery is completed.
[0055] Embodiment 1:
[0056] An embodiment of the present invention provides a method for solid phase purification of aluminum recovery, which mainly consists of process parameters such as molten salt electrolyte drying process, molten salt electrolyte component ratio, electrolysis reaction protective agent, molten salt electrolyte temperature, cathode and anode size specifications, electrolysis current, electrolysis voltage, and electrolysis time.
[0057] Take appropriate amounts of powdered magnesium chloride, sodium chloride, potassium chloride and calcium chloride electrolytes, wherein the purity of magnesium chloride is >98.0%, sodium chloride is >99.0%, potassium chloride is >99.6% and calcium chloride is >99.0%, keep the magnesium chloride, sodium chloride, potassium chloride and calcium chloride electrolytes at 180°C under vacuum conditions for 80 hours, then continue to heat to 300°C and keep for 18 hours, and cool under vacuum conditions for use.
[0058] The recycled waste is melted and prepared into thin sheets with the following dimensions: length 100mm, width 30mm, thickness 6mm. The cathode material uses pure aluminum (purity 98.5%) thin sheets with the same dimensions as the anode. The surface of the anode and cathode thin sheets is guaranteed to be bright and free of foreign matter.
[0059] Use an electronic balance to weigh dried magnesium chloride, sodium chloride, potassium chloride, and calcium chloride electrolytes, the mass percentages of which are 45% magnesium chloride, 30% sodium chloride, 15% potassium chloride, and 10% calcium chloride. At the same time, weigh 2.0% of the total mass of calcium fluoride powder of the electrolyte. Mix the magnesium chloride, sodium chloride, potassium chloride, calcium chloride, and calcium fluoride evenly, put them into an electrolytic cell for heating, and keep them warm when heated to 500°C.
[0060] Insert the prepared anode and cathode into the electrolytic cell containing high-temperature molten salt electrolyte, wait for 15-20 minutes to measure the temperature of the anode and cathode, and turn on the power after the anode and cathode are consistent with the temperature of the molten salt electrolyte. The current is 10KA, the voltage is 2.8V, and the electrolysis reaction time is 4 hours. After the electrolysis reaction is completed, cut off the power supply, collect high-purity aluminum on the cathode, and finally complete the solid phase purification process of recovered aluminum.
[0061] Embodiment 2:
[0062] An embodiment of the present invention provides a method for solid phase purification of aluminum recovery, which mainly consists of process parameters such as molten salt electrolyte drying process, molten salt electrolyte component ratio, electrolysis reaction protective agent, molten salt electrolyte temperature, cathode and anode size specifications, electrolysis current, electrolysis voltage, and electrolysis time.
[0063] Take appropriate amounts of powdered magnesium chloride, sodium chloride, potassium chloride and calcium chloride electrolytes, wherein the purity of magnesium chloride is >98.0%, sodium chloride is >99.0%, potassium chloride is >99.6% and calcium chloride is >99.0%, keep the magnesium chloride, sodium chloride, potassium chloride and calcium chloride electrolytes at 220° C. under vacuum conditions for 78 hours, then continue to heat to 330° C. and keep for 14 hours, and cool under vacuum conditions for use.
[0064] The recycled waste is melted and prepared into thin sheets with the following dimensions: length 100mm, width 30mm, thickness 6mm. The cathode material uses pure aluminum (purity 98.5%) thin sheets with the same dimensions as the anode. The surface of the anode and cathode thin sheets is guaranteed to be bright and free of foreign matter.
[0065] Use an electronic balance to weigh dried magnesium chloride, sodium chloride, potassium chloride, and calcium chloride electrolytes, the mass percentages of which are 48% magnesium chloride, 22% sodium chloride, 25% potassium chloride, and 5% calcium chloride. At the same time, weigh 4.0% of the total mass of calcium fluoride powder of the electrolyte. Mix the magnesium chloride, sodium chloride, potassium chloride, calcium chloride, and calcium fluoride evenly, put them into an electrolytic cell for heating, and keep them warm when heated to 530°C.
[0066] Insert the prepared anode and cathode into the electrolytic cell containing high-temperature molten salt electrolyte, wait for 15-20 minutes to measure the temperature of the anode and cathode, and turn on the power after the anode and cathode are consistent with the temperature of the molten salt electrolyte. The current is 12KA, the voltage is 2.4V, and the electrolysis reaction time is 3 hours. After the electrolysis reaction is completed, cut off the power supply, collect high-purity aluminum on the cathode, and finally complete the solid phase purification process of recovered aluminum.
[0067] Embodiment three:
[0068] An embodiment of the present invention provides a method for solid phase purification of aluminum recovery, which mainly consists of process parameters such as molten salt electrolyte drying process, molten salt electrolyte component ratio, electrolysis reaction protective agent, molten salt electrolyte temperature, cathode and anode size specifications, electrolysis current, electrolysis voltage, and electrolysis time.
[0069] Take appropriate amounts of powdered magnesium chloride, sodium chloride, potassium chloride and calcium chloride electrolytes, wherein the purity of magnesium chloride is >98.0%, sodium chloride is >99.0%, potassium chloride is >99.6% and calcium chloride is >99.0%, keep the magnesium chloride, sodium chloride, potassium chloride and calcium chloride electrolytes at 250°C under vacuum conditions for 72 hours, then continue to heat to 350°C and keep it for 12 hours, and cool under vacuum conditions for use.
[0070] The recycled waste is melted and prepared into thin sheets with the following dimensions: length 100mm, width 30mm, thickness 6mm. The cathode material uses pure aluminum (purity 98.5%) thin sheets with the same dimensions as the anode. The surface of the anode and cathode thin sheets is guaranteed to be bright and free of foreign matter.
[0071] Use an electronic balance to weigh dried magnesium chloride, sodium chloride, potassium chloride, and calcium chloride electrolytes, the mass percentages of which are 55% magnesium chloride, 20% sodium chloride, 17% potassium chloride, and 8% calcium chloride. At the same time, weigh 6.0% of the total mass of calcium fluoride powder of the electrolyte. Mix the magnesium chloride, sodium chloride, potassium chloride, calcium chloride, and calcium fluoride evenly, put them into an electrolytic cell for heating, and keep them warm when heated to 550°C.
[0072] Insert the prepared anode and cathode into the electrolytic cell containing high-temperature molten salt electrolyte, wait for 15-20 minutes to measure the temperature of the anode and cathode, and turn on the power after the anode and cathode are consistent with the temperature of the molten salt electrolyte. The current is 15KA, the voltage is 1.8V, and the electrolysis reaction time is 2h. After the electrolysis reaction is completed, cut off the power supply, collect high-purity aluminum on the cathode, and finally complete the solid phase purification process of recovered aluminum.
[0073] Table 1 Analysis of the anode and cathode products from the solid phase purification of aluminum recovery
[0074] Solid phase purification Anode aluminum loss (%) Cathode product purity (%) Embodiment 1 96.4 99.8 Embodiment 2 96.5 99.9 Embodiment 3 97.2 99.8
[0075] Table 1 analyzes the anode and cathode products after the electrolytic reaction of Example 1, Example 2, and Example 3. The amount of aluminum transferred by the anode during the electrolysis process can be calculated by measuring the weight loss of the recovered aluminum anode. The purity of the cathode product-aluminum is analyzed by "GB / T20975.25-2020 Chemical Analysis Method for Aluminum and Aluminum Alloy Part 25: Inductively Coupled Plasma Atomic Emission Spectrometry". It can be seen from the analysis of the anode and cathode products that in the solid phase purification electrolytic reaction of Example 1, Example 2, and Example 3, 96.4%, 96.5%, and 97.2% of the aluminum loss on the anode participated in the electrolytic reaction and was transferred to the cathode, and the purity of the aluminum obtained on the cathode was 99.8%, 99.9%, and 99.8%, respectively. It can be explained that the present invention can achieve high recovery rate, high purity, and high quality recovery of waste aluminum. The present invention can achieve the effects of wide recovery range, high recovery rate, high recovery purity, and low energy consumption.
[0076] The technical scope of the present invention is not limited to the contents in the above description. Those skilled in the art can make various deformations and modifications to the above embodiments without departing from the technical idea of the present invention, and these deformations and modifications all belong to the protection scope of the present invention.
Claims
1. A method for recovering aluminum solid phase purification, wherein the method for recovering aluminum solid phase purification comprises the following steps: (a) melting the recycled waste to prepare flakes; (b) mixing magnesium chloride, sodium chloride, potassium chloride and calcium chloride as electrolytes in specific proportions and calcium fluoride as an electrolyte protective agent uniformly into an electrolytic cell for heating, wherein the purity of magnesium chloride is greater than 98.0%, sodium chloride is greater than 99.0%, potassium chloride is greater than 99.6%, and calcium chloride is greater than 99.0%, and the magnesium chloride, sodium chloride, potassium chloride and calcium chloride electrolytes are kept at 220° C. under vacuum conditions for 78 hours, and then continued to heat to 330° C. and kept for 14 hours; or the purity of magnesium chloride is greater than 98.0%, sodium chloride is greater than 99.6%, and calcium chloride is greater than 99.0%. 9.0%, potassium chloride>99.6%, calcium chloride>99.0%, magnesium chloride, sodium chloride, calcium chloride electrolyte is kept at 180°C under vacuum conditions for 80 hours, and then continued to heat to 300°C and kept for 18 hours; or the purity of magnesium chloride>98.0%, sodium chloride>99.0%, potassium chloride>99.6%, calcium chloride>99.0%, magnesium chloride, sodium chloride, potassium chloride, calcium chloride electrolyte is kept at 250°C under vacuum conditions for 72 hours, and then continued to heat to 350°C and kept for 12 hours; and (c) inserting the anode and cathode into an electrolytic cell containing a high-temperature molten salt electrolyte, and applying power when the temperature of the anode and cathode is consistent with that of the molten salt electrolyte to collect high-purity aluminum on the cathode, wherein before step (a) include: Dry appropriate amounts of powdered magnesium chloride, sodium chloride, potassium chloride and calcium chloride electrolytes, and cool them under vacuum conditions for later use.
2. The solid phase purification method for recycled aluminum according to claim 1, wherein in step (a), the dimensions of the sheet are: length 100 mm, width 30 mm, thickness 6 mm, and the cathode material uses pure aluminum sheet, and its dimensions are consistent with those of the anode.
3. The solid phase purification method for recycled aluminum according to claim 2, wherein in the step (b), weigh dried magnesium chloride, sodium chloride, potassium chloride, and calcium chloride electrolytes, the mass percentages of which are 45% magnesium chloride, 30% sodium chloride, 15% potassium chloride, and 10% calcium chloride, and weigh 2.0% of the total mass of calcium fluoride powder of the electrolyte, mix the magnesium chloride, sodium chloride, potassium chloride, calcium chloride, and calcium fluoride evenly, put them into an electrolytic cell for heating, and keep them warm when heated to 500°C.
4. The solid phase purification method for recycled aluminum according to claim 2, wherein in the step (b), weigh dried magnesium chloride, sodium chloride, potassium chloride, and calcium chloride electrolytes, the mass percentages of which are 48% magnesium chloride, 22% sodium chloride, 25% potassium chloride, and 5% calcium chloride, and weigh 4.0% of the total mass of calcium fluoride powder of the electrolyte, mix the magnesium chloride, sodium chloride, potassium chloride, calcium chloride, and calcium fluoride evenly, put them into an electrolytic cell for heating, and keep them warm when heated to 530°C.
5. The solid phase purification method for recycled aluminum according to claim 2, wherein in the step (b), weigh dried magnesium chloride, sodium chloride, potassium chloride, and calcium chloride electrolytes, the mass percentages of which are 55% magnesium chloride, 20% sodium chloride, 17% potassium chloride, and 8% calcium chloride, and weigh 6.0% of the total mass of calcium fluoride powder of the electrolyte, mix the magnesium chloride, sodium chloride, potassium chloride, calcium chloride, and calcium fluoride evenly, put them into an electrolytic cell for heating, and keep them warm when heated to 550°C.
6. The solid phase purification method for recovering aluminum according to claim 2, wherein in the step (c), the anode and the cathode are temperature measured, and power is turned on when the anode and the cathode are consistent with the temperature of the molten salt electrolyte, wherein the current is 10KA-15KA, the voltage is 1.8V-2.8V, and the electrolysis reaction time is 2h-4h.