An integrated multiphase hydrogel and its preparation method and application in flexible stretchable supercapacitors
By combining PVA/PA/PANI/HPA electrodes with PVA/SA/PA electrolyte through an integrated multiphase hydrogel structure, the problem of poor adhesion between the electrode and electrolyte interface in stretchable supercapacitors is solved, achieving high capacitance retention and high energy density, and simplifying device integration.
Patent Information
- Application Number
- CN202311123011.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-10
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2043-10-10
AI Technical Summary
Existing stretchable supercapacitors have poor interfacial adhesion between the electrodes and electrolyte, resulting in poor capacitance retention during stretching and deformation, and the electrode thickness limits the realization of high energy and high power density.
An integrated multiphase hydrogel is used, in which PVA/PA/PANI/HPA semigel electrodes are injected into PVA/SA/PA semigel electrolyte to form a parallel multiphase hydrogel structure. The PVA/SA/PA hydrogel is used as the electrolyte and elastic substrate, and the PVA/PA/PANI/HPA semigel is used as the electrode, which enhances the interfacial toughness and conductivity.
It achieves high capacitance under high strain conditions, improves interfacial adhesion strength, suppresses delamination and displacement, enhances the connection between electrodes and electrolyte, ensures high energy and power density, and simplifies the device integration process.
Smart Images

Figure CN117164892B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of hydrogel materials, and in particular to an integrated multiphase hydrogel and a preparation method thereof, and an application thereof in a flexible and stretchable supercapacitor. Background Art
[0002] Stretchable supercapacitors (SCs) have attracted great interest due to their reliable safety, high power density, fast charge and discharge rates, and long cycle life (H. Huang, C. M. Lin, Z. F. Hua, J. J. Guo, D. D. Lu, Y. H. Ni, S. L. Cao, X. J. Ma, Chem. Eng. J. 2022, 448, 137589.). Stretchable supercapacitors are usually a three-layer structure design with an electrolyte layer sandwiched between two electrode layers. Sandwich stretchable supercapacitors can maintain high energy and power density under large strain. However, series integrated supercapacitors mainly rely on a large number of conductive metal wires, which is an important obstacle to building high-voltage output stretchable devices. (Q. Gong, Y. Q. Li, X. H. Liu, Z. B. Xia, Y. Yang, Carbohydr. Polym. 2020, 245, 116611; Z. K. Wang and Q. M. Pan, Adv. Funct. Mater. 2017, 27, 1700690.). Therefore, a great challenge in the field of stretchable supercapacitors is how to optimize the interfacial connection between electrodes and electrolytes by designing innovative materials or the structure of supercapacitors.
[0003] Generally speaking, in order to overcome this challenge, a two-dimensional (2D) SC structure has been recently developed by printing current collectors and electrochemically active materials on stretchable polymer substrates. This planar structural design has no external metal interconnections, which greatly simplifies the series integration process of SC devices. However, due to the poor interfacial adhesion between the electrode and the polymer substrate, the resulting SC exhibits unsatisfactory capacitance retention during tensile deformation (P. Das, LZ Zhang, SH Zheng, XY Shi, YJ Li, Z.-S. Wu, Carbon, 2022, 196, 203-212.), although several wrinkled geometries and interface engineering strategies have been adopted. Even more frustrating is that since the interface engineering method is only applicable to eliminating the tensile strain of high modulus electrodes near the interface, but not to the bulk phase of thicker electrode coatings, the thickness of the electrode coating is very limited (LZ Zhang, D. Liu, Z.-S. Wu, WW Lei, Energy Environ. Sci. 2020, 32, 402-417.). The universal limitation of electrode thickness is the main bottleneck for constructing high energy density and high power density SCs.
[0004] Therefore, from the perspective of application, providing a flexible and stretchable supercapacitor with large strain tolerance, high energy and power density, easy integration and simple material design is a technical problem that technicians in this field urgently need to solve. Summary of the invention
[0005] In view of this, the present invention provides a scheme for an integrated multiphase hydrogel to construct a flexible and stretchable supercapacitor with good interface toughness, large strain, high energy and power density, and easy integration.
[0006] To achieve the above object, the present invention adopts the following technical solution:
[0007] A method for preparing an integrated multiphase hydrogel comprises the following steps:
[0008] (1) polyvinyl alcohol and phytic acid are dissolved in water, sulfuric acid is then added, and the mixture is stirred at 75-95° C. for 2-3 hours to obtain a homogeneous solution, which is then cooled to room temperature to form a PVA / SA / PA semi-gel electrolyte;
[0009] (2) dissolving polyvinyl alcohol in phytic acid, stirring at 75-95°C for 2-3 hours, then adding ammonium persulfate and heteropoly acid to obtain a homogeneous solution, then adding phytic acid and aniline to the solution, stirring continuously at 75-95°C for 3-4 hours, and freezing at -30--20°C for 4-6 hours to obtain a PVA / PA / PANI / HPA semi-gel electrode;
[0010] (3) Injecting the PVA / SA / PA semi-gel electrolyte into the mold, and then injecting the PVA / PA / PANI / HPA semi-gel electrode into the PVA / SA / PA semi-gel electrolyte to form parallel electrodes with controllable spacing; covering the mold with the PVA / SA / PA semi-gel electrolyte to ensure that the PVA / PA / PANI / HPA is completely embedded in the bulk phase of the PVA / SA / PA semi-gel electrolyte; finally, freezing the mold and then thawing it at room temperature to obtain an integrated multiphase hydrogel.
[0011] The integrated multiphase hydrogel described in the present invention is a multiphase hydrogel formed by injecting two parallel wavy (or other shapes, such as rectangular, V-shaped, etc.) PVA / PA / PANI / HPA semi-gel electrodes into the bulk phase of the PVA / SA / PA semi-gel electrolyte. The parallel wavy hydrogel can be directly used as the anode and cathode of the stretchable electrode of the flexible stretchable supercapacitor without any post-treatment. The PVA / SA / PA hydrogel can be used as both a stretchable electrolyte and an elastic substrate. The prepared flexible stretchable supercapacitor can maintain super strong interface toughness, has excellent charge and discharge cycle stability, and has good capacitance retention under mechanical deformation conditions such as bending, twisting, and stretching.
[0012] Furthermore, the PVA / SA / PA semi-gel electrolyte in step (1) is composed of the following raw materials in mass fraction: 13.76-26.20% polyvinyl alcohol, 58.07-80.64% phytic acid, and the rest is sulfuric acid.
[0013] The beneficial effect of adopting the above further scheme is that the PVA / SA / PA semi-gel prepared by the above scheme of the present invention can be used as a stretchable electrolyte and an elastic substrate, wherein PA can significantly enhance the hydrogen bonding between PVA and PA, thereby improving the mechanical properties of the PVA / S / PA hydrogel. Sulfuric acid (S) improves the proton conductivity of the PVA / S / PA hydrogel.
[0014] Furthermore, the PVA / PA / PANI / HPA semi-gel electrode in step (2) is composed of the following raw materials in mass fraction: the mass fraction of polyvinyl alcohol is 7.97% to 10.4%, the mass fraction of phytic acid is 53.14% to 69.84%, the mass fraction of heteropoly acid is 9.52% to 29.63%, aniline is 1.72% to 2.44%, and the rest is ammonium persulfate.
[0015] The beneficial effect of adopting the above further scheme is that the PVA / PA / PANI / HPA semi-gel prepared by the above scheme of the present invention can be directly used as the cathode and anode of the stretchable electrode of the flexible stretchable supercapacitor, wherein the multivalent HPA is a kind of inorganic nanocluster. Since HPA not only acts as a multifunctional supramolecular crosslinker to connect PANI together to form a solid network at the macroscopic level, but also has redox activity to accept and donate electrons; PANI acts as a current collector to accelerate electron transfer.
[0016] Further, the heteropoly acid in step (2) is H 6 P 2 W 18 O 62 (P 2 W 18 ), H 4 S W12 O 40 (SiW), H 3 PW 12 O 40 (PW), H 3 PMo 12 O 40 Any one or more mixtures of (PMO).
[0017] The beneficial effect of adopting the above further scheme is that the PVA / PA / PANI / HPA electrode prepared by adopting the above heteropolyacid has a wide range of applicability by replacing different types of HPA.
[0018] Furthermore, the mold in step (3) is a corrugated mold with a length of 4.0 to 5.0 cm, a width of 1.0 to 2.0 cm, and a depth of 3.0 to 3.5 mm.
[0019] Furthermore, in step (3), the freezing temperature is -30 to -20°C, the freezing time is 22 to 24 hours, and the thawing time is 2 to 3 hours.
[0020] The beneficial effect of adopting the above further scheme is that: the above scheme of the present invention can effectively fix the shape and specifications of the mold to achieve a wavy electrode with certain specifications; through freezing and thawing, the hydrogel can be better cross-linked.
[0021] The present invention also provides an application of the above-mentioned integrated multiphase hydrogel in the preparation of a flexible stretchable supercapacitor, in which: an integrated multiphase hydrogel is used to ensure that two side-by-side gel electrodes are completely placed in a gel electrolyte during the preparation process to form an integrated multiphase gel containing both electrodes and electrolytes, and then carbon cloth is connected to one end of each electrode to obtain a flexible and stretchable integrated multiphase gel supercapacitor.
[0022] Furthermore, the gel electrode has a thickness of 3.0 to 3.5 mm, a length of 3.9 to 4.2 cm, a width of 1.0 to 2.0 cm, and a distance between the gel electrodes of 2.2 to 3.0 mm.
[0023] The beneficial effect of adopting the above further scheme is that the present invention can obtain optimal, stable and repeatable experimental data by setting the shape, specifications and distance between the electrodes of the gel.
[0024] Furthermore, the two parallel gel electrodes are formed by a pair of parallel electrodes, or a plurality of parallel electrodes connected in series.
[0025] Furthermore, the electrode shape can be wavy, straight, V-shaped, rectangular or other shapes.
[0026] The beneficial effects of adopting the above further scheme are: increasing the voltage in series on multiple pairs of parallel electrodes can achieve the effect of lighting up the device, demonstrating the application prospects of this flexible integrated multiphase gel; replacing the different shapes of the electrodes shows that the multiphase gel has the characteristics of customizability, patterning and miniaturization.
[0027] The beneficial effects of the present invention are:
[0028] 1) The hydrogel electrolyte PVA / SA / PA with a lower elastic modulus around the hydrogel electrode PVA / PA / PANI / HPA can effectively disperse the tensile stress, protect the hydrogel electrode with a higher elastic modulus, and delay the cracking of the PVA / PA / PANI / HPA hydrogel electrode.
[0029] 2) The wrapping structure greatly enlarges the connection area between PVA / SA / PA and PVA / PA / PANI / HPA, which is beneficial to improve the interfacial bonding strength and inhibit delamination and displacement;
[0030] 3) When the multiphase hydrogel is stretched along the latitudinal direction parallel to the surface, the thickness of the hydrogel is greatly reduced due to the longitudinal contraction. In this case, the peripheral hydrogel electrolyte may experience a larger contraction than the electrode, promoting a close connection between the electrolyte and the electrode.
[0031] Therefore, compared with the traditional sandwich structure, the advantage of the present invention is that it can solve the problems of inevitable interface displacement and separation during repeated mechanical stretching, which are usually caused by the inherent mismatch of Young's modulus and volume strain between the electrode and the electrolyte layer of the traditional sandwich supercapacitor; compared with the newly developed two-dimensional planar capacitor, the advantage of the present invention is that it can solve the problem that the two-dimensional planar supercapacitor exhibits unsatisfactory tolerance during tensile deformation due to poor interfacial adhesion between the electrode and the polymer substrate. The present invention integrates the advantages of the above two designs at the same time. The above-mentioned flexible stretchable supercapacitor prepared by using the PVA / PA / PANI / HPA@PVA / SA / PA integrated multiphase gel has a capacitance retention rate of more than 93% during deformation such as stretching. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 This is an optical photograph of the PVA / PA / PANI / (PW-14%)-(PMO-10%)@PVA / SA / PA integrated multiphase gel in Example 1 of the present invention;
[0033] Figure 2The following are the scanning electron microscope photograph (a), the corresponding EDS image photograph (b) and the optical microscope digital photograph (c) of the interface of the PVA / PA / PANI / (PW-14%)-(PMO-10%)@PVA / SA / PA integrated multiphase gel in Example 1 of the present invention; the microscope digital photographs of the changes in the electrode and electrolyte interface of the PVA / PA / PANI / (PW-14%)-(PMO-10%)@PVA / SA / PA integrated multiphase gel (d~f) and the PVA / PA / PANI / (PW-14%)-(PMO-10%) / / PVA / SA / PA sandwich supercapacitor (g~i) under different stretching conditions (0%~800%).
[0034] Figure 3 Stress-strain curves (a) of PVA / SA / PA electrolyte, PVA / PA / PANI / (PW-14%)-(PMO-10%) electrode and PVA / PA / PANI / (PW-14%)-(PMO-10%)@PVA / SA / PA multiphase gel in Example 1 of the present invention; Loading and unloading curves of PVA / SA / PA multiphase gel at a fixed strain of 200% (b); corresponding elastic modulus (c) and toughness (d) of PVA / SA / PA electrolyte, PVA / PA / PANI / (PW-14%)-(PMO-10%) electrode and PVA / PA / PANI / (PW-14%)-(PMO-10%)@PVA / SA / PA multiphase gel, respectively.
[0035] Figure 4 The photo (a) of a multiphase gel flexible supercapacitor formed by injecting two parallel wavy semi-gels PVA / PA / PANI / (PW-14%)-(PMo-10%) as electrodes into a stretchable electrolyte PVA / SA / PA semi-gel in Example 1 of the present invention is shown in Figure 2. The supercapacitor has a capacitance of 10-100 mV S -1 Cyclic voltammetry curves of PVA / PA / PANI / (PW-14%)-(PMO-10%)@PVA / SA / PA multiphase hydrogel stretchable supercapacitors measured in the range of 0.2-1.0 mA cm -2 GCD curves of stretchable supercapacitors measured in the range (c); electrochemical impedance spectroscopy (EIS) of PVA / PA / PANI / (PW-14%)-(PMO-10%)@PVA / SA / PA multiphase hydrogel SC (d).
[0036] Figure 5Photographs of a multiphase gel flexible stretchable supercapacitor formed by injecting two parallel wavy semi-gels PVA / PA / PANI / (PW-14%)-(PMo-10%) as electrodes into a stretchable electrolyte PVA / SA / PA semi-gel in Example 1 of the present invention (a), cyclic voltammograms at different bending angles (b), constant current charge and discharge (c) and capacitance retention graphs under different bending conditions (d).
[0037] Figure 6 The stretching photograph (a) of a multiphase gel flexible stretchable supercapacitor formed by two parallel wavy semi-gels PVA / PA / PANI / (PW-14%)-(PMO-10%)@PVA / SA / PA as electrodes injected into PVA / SA / PA semi-gel as a stretchable electrolyte in Example 1 of the present invention, the cyclic voltammetry curves at different stretching ratios (b), constant current charge and discharge curves (c), capacitance retention rate (d), cyclic voltammetry curves at different stretching times (e); GCD curves at different stretching times (f); and capacitance retention rate at different stretching times (g).
[0038] Figure 7 CV and GCD when four groups of identical multiphase gel supercapacitors are assembled in series in Example 1 of the present invention. DETAILED DESCRIPTION
[0039] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0040] Example 1
[0041] Preparation of PVA / PA / PANI / (PW-14%)-(PMO-10%)@PVA / SA / PA integrated multiphase gel:
[0042] (1) Polyvinyl alcohol (PVA, 3.0 g) and phytic acid (PA, 19.9 g) were dissolved in deionized water (5.4 mL), and then 1 mL of sulfuric acid (SA) was added. The mixture was stirred at 85 °C for 2 h to obtain a homogeneous solution, which was then cooled to room temperature to form a PVA / SA / PA semi-gel electrolyte.
[0043] The PVA / SA / PA semi-gel was frozen at -30oC for 24 hours and then thawed at room temperature for 2 hours to obtain a stretchable hydrogel electrolyte.
[0044] (2) PVA (2.0 g) was dissolved in PA (13.3 g) and stirred at 95 °C for 2 h to form a uniform solution. Then, 0.67 g of PA and 0.47 g of aniline were mixed in 2 mL of deionized water. 3 PW 12 O 40 (PW, 3.5 g) and H 3 PMo 12 O 40 1 mL aqueous solution of (PMO, 2.5 g) was quickly added to the PVA / PA solution and stirred continuously at 85 °C for 4 h. The mixed solution gradually changed from white to dark green, indicating that ammonium persulfate (APS) oxidized the aniline monomer to generate PANI. The dark green solution was frozen at -20 °C for 4 h to obtain PVA / PA / PANI / (PW-14%)-(PMO-10%) semi-gel.
[0045] Finally, the PVA / PA / PANI / (PW-14%)-(PMO-10%) semi-gel was frozen at -20 °C for 24 h and then thawed at room temperature for 2 h to obtain a stretchable hydrogel electrode.
[0046] (3) The PVA / SA / PA semi-gel electrolyte was injected into the mold (a wavy mold with a length of 4.0 cm, a width of 2.0 cm, and a depth of 3.0 mm). Then, the PVA / PA / PANI / (PW-14%)-(PMO-10%) semi-gel electrode was injected into the PVA / SA / PA semi-gel electrolyte to form parallel electrodes with controllable spacing (the coating thickness was 3.0 mm, the length was 3.9 cm, the width was 1.0 cm, and the distance between the two waves was 2.2 mm). Subsequently, the mold was covered with the PVA / SA / PA semi-gel electrolyte to ensure that the PVA / PA / PANI / (PW-14%)-(PMO-10%) was completely embedded in the bulk phase of the PVA / SA / PA semi-gel electrolyte. Finally, the mold was frozen at -20oC for 24 h and then thawed at room temperature for 2 h to form a PVA / PA / PANI / (PW-14%)-(PMO-10%)@PVA / SA / PA integrated multiphase hydrogel.
[0047] Figure 1 This is a digital photo of PVA / PA / PANI / (PW-14%)-(PMO-10%)@PVA / SA / PA integrated multiphase hydrogel; from the picture, it can be seen that the PVA / SA / PA electrolyte surrounds the PVA / PA / PANI / (PW-14%)-(PMO-10%) electrode, explaining the structure of its integrated multiphase gel.
[0048] Experimental Example 1Interfacial Properties of PVA / PA / PANI / (PW-14%)-(PMO-10%)@PVA / SA / PA Integrated Multiphase Gel
[0049] The freeze-dried PVA / PA / PANI / (PW-14%)-(PMO-10%)@PVA / SA / PA integrated multiphase gel (30 mm in length, 8 mm in width, and 3 mm in thickness) in Example 1 was bonded to a cross-section table (30 mm in diameter) used for a scanning electron microscope, and the fusion of the electrode and electrolyte interface regions in the multiphase gel was detected using a scanning electron microscope; the PVA / PA / PANI / (PW-14%)-(PMO-10%)@PVA / SA / PA integrated multiphase gel (30 mm in length, 8 mm in width, and 3 mm in thickness) and a sandwich-type supercapacitor (30 mm in length, 8 mm in width, and 3 mm in thickness) were placed under a microscope to observe changes in the electrode and electrolyte interface regions at different stretching ratios (0% to 800%).
[0050] like Figure 2 Shown are scanning electron microscope photos of the fusion of the electrode and electrolyte interface region in the PVA / PA / PANI / (PW-14%)-(PMO-10%)@PVA / SA / PA multiphase gel (for example, whether there is a seamless connection in the interface region); and microscope digital photos of the changes in the electrode and electrolyte interface region of the multiphase gel and sandwich gel at a stretching ratio of 0% to 800% (for example, whether there is stratification, rupture, etc. in the interface region).
[0051] From the cross-sectional scanning electron microscopy images of the multiphase hydrogel ( Figure 2 As can be seen in a), there is a seamless interface connection in the interface region. The corresponding W image ( Figure 2 b) Clearly reveals the interfacial diffusion between the PVA / PA / PANI / (PW-14%)-(PMO-10%) electrode and the PVA / SA / PA electrolyte due to local material exchange during the preparation process. The optical microscopy image shows (2c) that there is a dark blue diffusion zone between the dark green PVA / PA / PANI / (PW-14%)-(PMO-10%) phase and the white PVA / SA / PA phase, further supporting the existence of seamless interfacial diffusion. The interpenetration or entanglement of multivalent polymers at the interface is conducive to strengthening the adhesion of the material between the electrode and the electrolyte. Figure 2 d is the photo of the interface change of PVA / PA / PANI / (PW-14%)-(PMO-10%)@PVA / SA / PA multiphase hydrogel under different stretching conditions. Figure 2d It can be seen that: 1) At a high stretching ratio (500%), the existence of the interfacial diffusion layer indicates that the initial stress is first applied to the PVA / SA / PA electrolyte, resulting in stress dispersion and protection of the interfacial layer and the PVA / PA / PANI / (PW-14%)-(PMO-10%) gel electrode. With the further increase of the stretching ratio to 800%, the stress gradually transfers to the interface, causing the diffusion layer to become thinner or even disappear. 2) No interfacial fracture was found during the entire stretching process, indicating that the wrapped structure of the multiphase hydrogel can effectively maintain a close interfacial connection between the electrode and the electrolyte. In contrast, at a stretching ratio of 500%, the sandwich hydrogel ( Figure 2 e) Cracks appeared at the interface between PVA / PA / PANI / (PW-14%)-(PMO-10%) and PVA / SA / PA. As the stretching ratio increased to 800%, the degree of interfacial cracks increased significantly, eventually leading to interfacial delamination and displacement.
[0052] Experimental Example 2 Mechanical Properties of PVA / PA / PANI / (PW-14%)-(PMo-10%)@PVA / SA / PA Integrated Multiphase Gel
[0053] The two ends of the PVA / PA / PANI / (PW-14%)-(PMo-10%)@PVA / SA / PA integrated multiphase gel with a length of 30mm, a width of 8mm, and a thickness of 3mm were fixed vertically on an electronic universal material testing machine and longitudinally stretched at a speed of 20mm / min and a temperature of 25°C. The applied force (the additional internal force per unit area) and the strain generated (when an object is deformed by force, the degree of deformation at each point in the body is generally not the same. A mechanical quantity used to describe the degree of deformation at a point) were recorded until fracture occurred. The two parameter data are then plotted on an XY graph to obtain the familiar stress-strain curve. The stress-strain curve is data that shows how stress changes with increasing strain. The slope of the stress-strain curve is used to obtain the Young's modulus to evaluate its strength; the area under the stress-strain curve is used to calculate its toughness and evaluate its ductility.
[0054] The two ends of an integrated multiphase gel with a length of 30 mm, a width of 8 mm and a thickness of 3 mm were vertically fixed on an electronic universal material testing machine and the loading (when the stress changes (0-200%), the sample has new plastic deformation, and this stress change is called loading) and unloading (when the stress changes, the sample returns to the initial (200-0%) state and no new plastic deformation occurs. At this time, the stress change becomes unloading) curves of the PVA / PA / PANI / (PW-14%)-(PMo-10%)@PVA / SA / PA integrated multiphase gel as the strain increases (0-200%) at a speed of 20 mm / min and a fixed maximum strain of 200%. The area of the loading and unloading curves is the area of the hysteresis loop, and the energy dissipation is evaluated by the size of the area of the hysteresis loop.
[0055] Figure 3 The present invention relates to a novel multiphase hydrogel having a plurality of phases, a plurality of phases, and a plurality of phases. The present invention relates to a multiphase hydrogel having a plurality of phases, a plurality of phases, and a plurality of phases. The present invention relates to a multiphase hydrogel having a plurality of phases, a plurality of phases, and a plurality of phases. The present invention relates to a multiphase hydrogel having a plurality of phases, a plurality of phases, and a plurality of phases. The present invention relates to a multiphase hydrogel having a plurality of phases, a plurality of phases, and a plurality of phases. The present invention relates to a multiphase hydrogel having a plurality of phases, a plurality of phases, and a plurality of phases. The present invention relates to a multiphase hydrogel having a plurality of phases, a plurality of phases, and a plurality of phases. The present invention relates to a multiphase hydrogel having a plurality of phases, a plurality of phases, and a plurality of phases. The present invention relates to a multiphase hydrogel having a plurality of phases, a plurality of phases, and a plurality of phases. The present invention relates to a multiphase hydrogel having a plurality of phases, a plurality of phases, and a plurality of phases.
[0056] The mechanical properties of PVA / PA / PANI / (PW-14%)-(PMO-10%)@PVA / SA / PA multiphase hydrogel were tested using typical tensile stress-strain curves. Figure 3 As shown in a, the tensile strain (614%) and tensile strength (1.83 MPa) of PVA / PA / PANI / (PW-14%)-(PMO-10%)@PVA / SA / PA phase hydrogel are higher than those of PVA / SA / PA hydrogel (737%, 0.90 MPa), but lower than those of PVA / PA / PANI / (PW-14%)-(PMo-10%) hydrogel (660%, 1.49 MPa). Figure 3 The apparent hysteresis loops of PVA / SA / PA hydrogel, PVA / PA / PANI / (PW-14%)-(PMO-10%) and PVA / PA / PANI / (PW-14%)-(PMO-10%)@PVA / SA / PA in b indicate that the hydrogel cross-linked network brought by dynamic reversible hydrogen bonds can effectively dissipate the stretching energy. The elastic modulus of the multiphase hydrogel is 0.282MPa( Figure 3 c), toughness is 6.62MJ m -3 ( Figure 3 d). Apparently, multiphase hydrogels can integrate mismatched hydrogel phases into an integrated platform, thereby improving the tensile strength of PVA / SA / PA hydrogels and enhancing the toughness of PVA / PA / PANI / (PW-14%)-(PMo-10%) hydrogels.
[0057] Experimental Example 3 Comprehensive performance of PVA / PA / PANI / (PW-14%)-(PMO-10%)@PVA / SA / PA integrated multiphase gel flexible and stretchable supercapacitor
[0058] Put two parallel waves (such as Figure 1 As shown, the thickness of the electrode is 3.0-3.5 mm, the pattern length is 3.9-4.2 cm, the width is 1.0-2.0 cm, and the distance between the two waves is 2.2-3.0 mm) PVA / PA / PANI / (PW-14%)-(PMO-10%) semi-gel electrode is injected into the bulk phase of PVA / SA / PA semi-gel electrolyte to form a multiphase hydrogel. The parallel-arranged wavy hydrogel can be directly used as the anode and cathode of the flexible stretchable supercapacitor electrode without any post-treatment. The PVA / SA / PA hydrogel can be used as both a stretchable electrolyte and an elastic substrate. The cyclic voltammetry (CV) curve of PVA / PA / PANI / (PW-14%)-(PMO-10%)@PVA / SA / PA integrated stretchable super electrical appliance was tested at 10-100 mV / s using Chenhua electrochemical workstation to evaluate the rate performance of PVA / PA / PANI / (PW-14%)-(PMO-10%)@PVA / SA / PA integrated stretchable super electrical appliance; according to the PVA / PA / PANI / (PW-14%)-(PMO-10%)@PVA / SA / PA integrated stretchable super electrical appliance at 0.2-1.0 mA cm -2The constant current charge and discharge (GCD) curve under current density is used to evaluate its capacitance, energy density and power density; the electrochemical impedance spectroscopy (EIS) curve of the PVA / PA / PANI / (PW-14%)-(PMO-10%)@PVA / SA / PA integrated stretchable super-electrical device is used to evaluate the conductivity and diffusion behavior of its electrodes. The CV and GCD curves of the PVA / PA / PANI / (PW-14%)-(PMO-10%)@PVA / SA / PA integrated stretchable super-electrical device under different stretching ratios (0% to 250%) were tested, and the capacitance retention was judged by analyzing the CV and GCD curves. The PVA / PA / PANI / (PW-14%)-(PMO-10%)@PVA / SA / PA integrated multiphase gel can well integrate the bottom-up approach and the top-down technology to conveniently construct a processable, integrable, and patternable stretchable supercapacitor device. This multiphase design has no external metal interconnection when connected in series, which greatly simplifies the series integration process of supercapacitor devices. The capacitors obtained in series were subjected to CV and GCD tests at different stretching ratios to evaluate the performance of the flexible capacitors obtained in series.
[0059] Figure 4 A multiphase gel flexible stretchable supercapacitor (PVA / PA / PANI / (PW-14%)-(PMO-10%) semi-gel electrode was injected into a PVA / SA / PA semi-gel electrolyte. Figure 4 a) From Figure 4 b It can be seen that with the increase of scanning speed, the shape of the cyclic voltammetry curve remains unchanged, but the current intensity increases significantly, which indicates that the PVA / PA / PANI / (PW-14%)-(PMO-10%)@PVA / SA / PA multiphase hydrogel has high rate capability. GCD test ( Figure 4 c) shows a nonlinear but symmetrical curve, which indicates that the Faradaic behavior of the multiphase hydrogel is consistent with the cyclic voltammetry curve. -2 When the specific capacitance (Cs) of PVA / PA / PANI / (PW-14%)-(PMO-10%)@PVA / SA / PA multiphase gel is 258.5, 209.4, 181.5, 178.0 and 167.5 F cm -2 At a power density of 576.0 μW cm -2 The maximum energy density of the single-electrode PVA / PA / PANI / (PW-14%)-(PMO-10%)@PVA / SA / PA multiphase hydrogel can reach 82.7 μWh cm -2 Even at 2880.0 μW cm -2At the maximum power density, the energy density can also be maintained at 53.6 μWh cm -2 .Electrochemical impedance spectroscopy (EIS) shows no semicircular pattern in the high frequency range ( Figure 4 d), which indicates that the PVA / PA / PANI / (PW-14%)-(PMO-10%) hydrogel electrode has high conductivity and low charge transfer resistance during charge and discharge. The straight line in the low frequency range corresponds to the diffusion process of ions into the electrode, indicating good capacitive behavior. The low impedance value at 1 Hz (11Ω) indicates that ions are easily inserted into the PVA / PA / PANI / (PW-14%)-(PMO-10%) hydrogel electrode.
[0060] Figure 5 It is a PVA / PA / PANI / (PW-14%)-(PMO-10%)@PVA / SA / PA integrated multiphase gel flexible stretchable supercapacitor ( Figure 5 a) Cyclic voltammetry curves, GCD and capacitance retention at different bending angles. From the figure, we can see the CV ( Figure 5 b) and GCD curve ( Figure 5 c) remains almost unchanged. The capacitance retention rate of PVA / PA / PANI / (PW-14%)-(PMO-10%)@PVA / SA / PA stretchable supercapacitor during bending deformation exceeds 99% ( Figure 5 d), indicating that the multiphase hydrogel structure has reliable adaptability to mechanical deformation.
[0061] Figure 6 The PVA / PA / PANI / (PW-14%)-(PMO-10%) semi-gel electrode was injected into the PVA / SA / PA semi-gel to form a multiphase gel flexible stretchable supercapacitor ( Figure 6 a) Cyclic voltammetry curves and capacitance retention under different stretching conditions. From the figure, we can see that the CV and GCD curves of the PVA / PA / PANI / (PW-14%)-(PMO-10%)@PVA / SA / PA stretchable supercapacitor under stretching are as follows: Figure 6 b and 6c. The capacitance calculated from the GCD curve reaches 93.0% at 250% strain ( Figure 6 d). In order to further analyze the mechanical stability and durability of the multiphase structure supercapacitor, a long-term deformation test with 3000 consecutive 300% stretching cycles was carried out. After repeated stretching for 3000 times, the cyclic voltammetry curve of the stretchable supercapacitor ( Figure 6 e) and GCD( Figure 6 f) The curve has no obvious change, and the initial capacity is maintained at 95.0% ( Figure 6 g), indicating that the multiphase hydrogel SC has good anti-deformation performance.
[0062] Figure 7 Four groups of PVA / PA / PANI / (PW-14%)-(PMO-10%)@PVA / SA / PA are connected in series to form a flexible and stretchable supercapacitor. From the CV curve and GCD curve, it can be seen that the series-connected PVA / PA / PANI / (PW-14%)-(PMO-10%)@PVA / SA / PA flexible and stretchable supercapacitor can output higher current or voltage, demonstrating the application prospects of this flexible integrated PVA / PA / PANI / (PW-14%)-(PMO-10%)@PVA / SA / PA multiphase gel.
[0063] Example 2
[0064] The same as Example 1, other conditions remain unchanged, 4g PW and 2g PMO (H 3 PW 12 O 40 , molecular weight is 2880.05g / mol, H 3 PMo 12 O 40 , molecular weight 1825.25 g / mol) was changed to 1 g PW and 5 g PMO (H 3 PW 12 O 40 , molecular weight is 2880.05g / mol, H 3 PMo 12 O 40 , molecular weight of 1825.25g / mol), and then prepared PVA / PA / PANI / (PW-4%)-(PMo-20%)@PVA / SA / PA multiphase hydrogel. According to the operating steps of Example 1, the PVA / PA / PANI / (PW-4%)-(PMo-20%) semi-gel electrode was injected into the PVA / SA / PA semi-gel stretchable electrolyte to form an integrated multiphase gel and then assembled into a flexible stretchable supercapacitor. Then the cyclic voltammetry curves and charge-discharge curves of the prepared flexible stretchable supercapacitor were measured at different bending angles and different stretching ratios (stretching ratio 0-250%). The results show that whether it is bent or stretched (stretching ratio 0-250%), the capacitance retention rate reaches more than 92%, which indicates that the prepared flexible stretchable supercapacitor has good tensile resistance.
[0065] Example 3
[0066] The same as Example 1, other conditions remain unchanged, 4g PW and 2g PMO (H 3 PW 12 O 40 , molecular weight is 2880.05g / mol, H 3 PMo 12 O 40 , molecular weight 1825.25 g / mol) was changed to 2 g PW and 4 g PMO (H 3 PW 12 O 40 , molecular weight is 2880.05g / mol, H 3 PMo 12 O 40 , molecular weight of 1825.25g / mol), and then prepared PVA / PA / PANI / (PW-8%)-(PMo-16%)@PVA / SA / PA multiphase hydrogel. According to the operating steps of Example 1, the PVA / PA / PANI / (PW-8%)-(PMo-16%) semi-gel was injected into the PVA / SA / PA semi-gel stretchable electrolyte to form an integrated multiphase gel and then assembled into a flexible supercapacitor. The cyclic voltammetry curves and charge-discharge curves of the prepared flexible stretchable supercapacitor were then measured at different bending angles and different stretching ratios (stretching ratio 0-250%). The results show that whether it is bent or stretched (stretching ratio 0-250%), the capacitance retention rate reaches more than 91%, which indicates that the prepared flexible stretchable supercapacitor has good tensile resistance.
[0067] Example 4
[0068] The same as Example 1, other conditions remain unchanged, 4g PW and 2g PMO (H 3 PW 12 O 40 , molecular weight is 2880.05g / mol, H 3 PMo 12 O 40 , molecular weight 1825.25 g / mol) was changed to 3 g PW and 3 g PMO (H 3 PW 12 O 40 , molecular weight is 2880.05g / mol, H 3 PMo 12 O 40, molecular weight of 1825.25g / mol), and then prepared PVA / PA / PANI / (PW-12%)-(PMo-12%)@PVA / SA / PA multiphase hydrogel. According to the operating steps of Example 1, the PVA / PA / PANI / (PW-12%)-(PMo-12%) semi-gel was injected into the PVA / SA / PA semi-gel stretchable electrolyte to form an integrated multiphase gel and then assembled into a flexible stretchable supercapacitor. The cyclic voltammetry curve and charge-discharge curve of the prepared flexible supercapacitor were then measured at different bending angles and different stretching ratios (stretching ratio 0-250%). The results show that whether it is bent or stretched (stretching ratio 0-250%), the capacitance retention rate reaches more than 90%, which indicates that the prepared flexible stretchable supercapacitor has good tensile resistance.
[0069] Example 5
[0070] The same as Example 1, other conditions remain unchanged, 4g PW and 2g PMO (H 3 PW 12 O 40 , molecular weight is 2880.05g / mol, H 3 PMo 12 O 40 , molecular weight 1825.25 g / mol) was changed to 5 g PW and 1 g PMO (H 3 PW 12 O 40 , molecular weight is 2880.05g / mol, H 3 PMo 12 O 40 , molecular weight of 1825.25g / mol), and then prepared PVA / PA / PANI / (PW-20%)-(PMo-4%)@PVA / SA / PA multiphase hydrogel. According to the operating steps of Example 1, the PVA / PA / PANI / (PW-20%)-(PMo-4%) semi-gel was injected into the PVA / SA / PA semi-gel stretchable electrolyte to form an integrated multiphase gel and then assembled into a flexible stretchable supercapacitor. The cyclic voltammetry curves and charge-discharge curves of the prepared flexible stretchable supercapacitor were then measured at different bending angles and different stretching ratios (stretching ratio 0-250%). The results show that whether it is bent or stretched (stretching ratio 0-250%), the capacitance retention rate reaches more than 87%, which indicates that the prepared flexible stretchable supercapacitor has good tensile resistance.
[0071] Example 6
[0072] The same as Example 1, other conditions remain unchanged, 4g PW and 2g PMO (H 3 PW12 O 40 , molecular weight is 2880.05g / mol, H 3 PMo 12 O 40 , molecular weight 1825.25 g / mol) was changed to 4 g PW and 2 g H 6 P 2 W 18 O 62 (H 3 PW 12 O 40 , molecular weight is 2880.05g / mol, H 6 P 2 W 18 O 62 , molecular weight 4369.62g / mol), and then PVA / PA / PANI / (PW-16%)-(P 2 W 18 -8%)@PVA / SA / PA multiphase hydrogel. According to the operation steps of Example 1, PVA / PA / PANI / (PW-16%)-(P 2 W 18 -8%) semi-gel was injected into the PVA / SA / PA semi-gel stretchable electrolyte to form an integrated multiphase gel and then assembled into a flexible stretchable supercapacitor. The cyclic voltammetry curve and charge-discharge curve of the prepared flexible stretchable supercapacitor were then measured at different bending angles and different stretching ratios (stretching ratio 0-250%). The results showed that whether it was bent or stretched (stretching ratio 0-250%), its capacitance retention rate reached more than 86%, which indicates that the prepared flexible stretchable supercapacitor has good tensile resistance.
[0073] Example 7
[0074] The same as Example 1, other conditions remain unchanged, 4g PW and 2g PMO (H 3 PW 12 O 40 , molecular weight is 2880.05g / mol, H 3 PMo 12 O 40 , molecular weight is 1825.25 g / mol) is changed to 2g PW and 4g H 6 P 2 W 18 O 62 (H 3 PW 12 O 40 , molecular weight is 2880.05g / mol, H 6 P 2 W 18O 62 , molecular weight 4369.62g / mol), and then PVA / PA / PANI / (PW-8%)-(P 2 W 18 -16%)@PVA / SA / PA multiphase hydrogel. According to the operation steps of Example 1, PVA / PA / PANI / (PW-8%)-(P 2 W 18 -16%) semi-gel electrodes were injected into PVA / SA / PA semi-gel stretchable electrolytes to form an integrated multiphase gel and then assembled into a flexible stretchable supercapacitor. The cyclic voltammetry curves and charge-discharge curves of the prepared flexible stretchable supercapacitor were then measured at different bending angles and different stretching ratios (stretching ratio 0-250%). The results showed that whether it was bent or stretched (stretching ratio 0-250%), the capacitance retention rate reached more than 88%, which indicates that the prepared flexible stretchable supercapacitor has good tensile resistance.
[0075] Example 8
[0076] The same as Example 1, other conditions remain unchanged, 4g PW and 2g PMO (H 3 PW 12 O 40 , molecular weight is 2880.05g / mol, H 3 PMo 12 O 40 , molecular weight 1825.25 g / mol) was changed to 4 g PMO and 2 g H 6 P 2 W 18 O 62 (H 3 PMo 12 O 40 , molecular weight is 1825.25 g / mol, H 6 P 2 W 18 O 62 , molecular weight 4369.62g / mol), and then PVA / PA / PANI / (PMO-16%)-(P 2 W 18 -8%)@PVA / SA / PA multiphase hydrogel. According to the operation steps of Example 1, PVA / PA / PANI / (PMO-16%)-(P 2 W 18-8%) semi-gel electrodes were injected into PVA / SA / PA semi-gel stretchable electrolytes to form an integrated multiphase gel and then assembled into a flexible stretchable supercapacitor. The cyclic voltammetry curves and charge-discharge curves of the prepared flexible stretchable supercapacitor were then measured at different bending angles and different stretching ratios (stretching ratio 0-250%). The results showed that whether it was bent or stretched (stretching ratio 0-250%), its capacitance retention rate reached more than 87%, which indicates that the prepared flexible stretchable supercapacitor has good tensile resistance.
[0077] Example 9
[0078] The same as Example 1, other conditions remain unchanged, 4g PW and 2g PMO (H 3 PW 12 O 40 , molecular weight is 2880.05g / mol, H 3 PMo 12 O 40 , molecular weight 1825.25 g / mol) was changed to 2 g PMO and 4 g H 6 P 2 W 18 O 62 (H 3 PMo 12 O 40 , molecular weight is 1825.25 g / mol, H 6 P 2 W 18 O 62 , molecular weight of 4369.62 g / mol), and then PVA / PA / PANI / (PMO-8%)-(P 2 W 18 -16%)@PVA / SA / PA multiphase hydrogel. According to the operation steps of Example 1, PVA / PA / PANI / (PMO-8%)-(P 2 W 18 -16%) semi-gel was injected into the PVA / SA / PA semi-gel stretchable electrolyte to form an integrated multiphase gel and then assembled into a flexible stretchable supercapacitor. The cyclic voltammetry curve and charge-discharge curve of the prepared flexible stretchable supercapacitor were then measured at different bending angles and different stretching ratios (stretching ratio 0-250%). The results showed that whether it was bent or stretched (stretching ratio 0-250%), the capacitance retention rate reached more than 85%, which indicates that the prepared flexible stretchable supercapacitor has good tensile resistance.
[0079] Example 10
[0080] The same as Example 1, other conditions remain unchanged, 4g PW and 2g PMO (H 3 PW 12 O 40 , molecular weight is 2880.05g / mol, H 3 PMo 12 O 40 , molecular weight 1825.25 g / mol) was changed to 2 g PMO and 4 g H 4 S W 12 O 40 (H 3 PW 12 O 40 , molecular weight is 2880.05g / mol, H 4 S W 12 O 40 , molecular weight is 2878.17g / mol), and then PVA / PA / PANI / (PMO-8%)-(SiW-16%)@PVA / SA / PA multiphase hydrogel is prepared. According to the operating steps of Example 1, the PVA / PA / PANI / (PMO-8%)-(SiW-16%) semi-gel electrode is injected into the PVA / SA / PA semi-gel stretchable electrolyte to form an integrated multiphase gel and then assembled into a flexible stretchable supercapacitor. Then the cyclic voltammetry curves and charge-discharge curves of the prepared flexible stretchable supercapacitor were measured at different bending angles and different stretching ratios (stretching ratio 0-250%). The results show that whether it is bent or stretched (stretching ratio 0-250%), the capacitance retention rate reaches more than 86%, which indicates that the prepared flexible stretchable supercapacitor has good tensile resistance.
[0081] Embodiment 11
[0082] The same as Example 1, other conditions remain unchanged, 4g PW and 2g PMO (H 3 PW 12 O 40 , molecular weight is 2880.05g / mol, H 3 PMo 12 O 40 , molecular weight 1825.25 g / mol) was changed to 4 g PMO and 2 g H 4 S W 12 O 40 (H 3 PMo 12 O 40 , molecular weight is 1825.25 g / mol, H 4 S W 12 O 40, molecular weight is 2878.17g / mol), and then PVA / PA / PANI / (PMO-16%)-(SiW-8%)@PVA / SA / PA multiphase hydrogel is prepared. According to the operating steps of Example 1, the PVA / PA / PANI / (PMO-16%)-(SiW-8%) semi-gel electrode is injected into the PVA / SA / PA semi-gel stretchable electrolyte to form an integrated multiphase gel and then assembled into a flexible stretchable supercapacitor. Then the cyclic voltammetry curve and charge-discharge curve of the prepared flexible stretchable supercapacitor were measured at different bending angles and different stretching ratios (stretching ratio 0-250%). The results show that whether it is bent or stretched (stretching ratio 0-250%), the capacitance retention rate reaches more than 88%, which indicates that the prepared flexible stretchable supercapacitor has good tensile resistance.
[0083] Example 12
[0084] The same as Example 1, other conditions remain unchanged, 4g PW and 2g PMO (H 3 PW 12 O 40 , molecular weight is 2880.05g / mol, H 3 PMo 12 O 40 , molecular weight is 1825.25 g / mol) is changed to 2g PW and 4g H 4 S W 12 O 40 (H 3 PW 12 O 40 , molecular weight is 2880.05g / mol, H 4 S W 12 O 40 , molecular weight is 2878.17g / mol), and then PVA / PA / PANI / (PW-8%)-(SiW-16%)@PVA / SA / PA multiphase hydrogel is prepared. According to the operating steps of Example 1, the PVA / PA / PANI / (PW-8%)-(SiW-16%) semi-gel electrode is injected into the PVA / SA / PA semi-gel stretchable electrolyte to form an integrated multiphase gel and then assembled into a flexible stretchable supercapacitor. Then the cyclic voltammetry curves and charge-discharge curves of the prepared flexible stretchable supercapacitor were measured at different bending angles and different stretching ratios (stretching ratio 0-250%). The results show that whether it is bent or stretched (stretching ratio 0-250%), the capacitance retention rate reaches more than 83%, which indicates that the prepared flexible stretchable supercapacitor has good tensile resistance.
[0085] Embodiment 13
[0086] The same as Example 1, other conditions remain unchanged, 4g PW and 2g PMO (H 3 PW 12 O 40 , molecular weight is 2880.05g / mol, H 3 PMo 12 O 40 , molecular weight 1825.25 g / mol) was changed to 4 g PW and 2 g H 4 S W 12 O 40 (H 3 PW 12 O 40 , molecular weight is 2880.05g / mol, H 4 S W 12 O 40 , molecular weight is 2878.17g / mol), and then PVA / PA / PANI / (PW-16%)-(SiW-8%)@PVA / SA / PA multiphase hydrogel is prepared. According to the operating steps of Example 1, the PVA / PA / PANI / (PW-16%)-(SiW-8%) semi-gel electrode is injected into the PVA / SA / PA semi-gel stretchable electrolyte to form an integrated multiphase gel and then assembled into a flexible stretchable supercapacitor. Then the cyclic voltammetry curves and charge-discharge curves of the prepared flexible stretchable supercapacitor were measured at different bending angles and different stretching ratios (stretching ratio 0-250%). The results show that whether it is bent or stretched (stretching ratio 0-250%), the capacitance retention rate reaches more than 85%, which indicates that the prepared flexible stretchable supercapacitor has good tensile resistance.
[0087] Embodiment 14
[0088] Basically the same as Example 1, other conditions remain unchanged, the wavy PVA / PA / PANI / (PW-14%)-(PMO-10%) electrode is changed to a rectangular PVA / PA / PANI / (PW-14%)-(PMO-10%) electrode, and then a rectangular PVA / PA / PANI / (PW-14%)-(PW-10%)@PVA / SA / PA multiphase hydrogel is prepared. According to the operating steps of Example 1, the rectangular PVA / PA / PANI / (PW-14%)-(PMO-10%) semi-gel electrode is injected into the PVA / SA / PA semi-gel stretchable electrolyte to form an integrated multiphase gel and then assembled into a flexible stretchable supercapacitor. Then, the cyclic voltammetry curve and charge-discharge curve of the prepared flexible stretchable supercapacitor are measured at different bending angles and different stretching ratios (stretching ratio 0 to 140%). The results show that whether it is bent or stretched (stretching ratio 0-140%), the capacitance retention rate reaches more than 77%, which indicates that the prepared flexible stretchable supercapacitor has good tensile resistance.
[0089] Embodiment 15
[0090] Basically the same as Example 1, other conditions remain unchanged, the wavy PVA / PA / PANI / (PW-14%)-(PMO-10%) electrode is changed to a V-shaped PVA / PA / PANI / (PW-14%)-(PMO-10%) electrode, and then a V-shaped PVA / PA / PANI / (PW-14%)-(PW-10%)@PVA / SA / PA multiphase hydrogel is prepared. According to the operating steps of Example 1, the rectangular PVA / PA / PANI / (PW-14%)-(PMO-10%) semi-gel electrode is injected into the PVA / SA / PA semi-gel stretchable electrolyte to form an integrated multiphase gel and then assembled into a flexible stretchable supercapacitor. Then, the cyclic voltammetry curve and charge-discharge curve of the prepared flexible stretchable supercapacitor are measured at different bending angles and different stretching ratios (stretching ratio 0 to 200%). The results show that whether it is bent or stretched (stretching ratio 0-200%), the capacitance retention rate reaches more than 89%, which indicates that the prepared flexible stretchable supercapacitor has good tensile resistance.
[0091] Example 16
[0092] Basically the same as Example 1, other conditions remain unchanged, the wavy PVA / PA / PANI / (PW-14%)-(PMO-10%) electrode is changed to a linear PVA / PA / PANI / (PW-14%)-(PMO-10%) electrode, and then a linear PVA / PA / PANI / (PW-14%)-(PW-10%)@PVA / SA / PA multiphase hydrogel is prepared. According to the operating steps of Example 1, the rectangular PVA / PA / PANI / (PW-14%)-(PMO-10%) semi-gel electrode is injected into the PVA / SA / PA semi-gel stretchable electrolyte to form an integrated multiphase gel and then assembled into a flexible stretchable supercapacitor. Then, the cyclic voltammetry curve and charge-discharge curve of the prepared flexible stretchable supercapacitor are measured at different bending angles and different stretching ratios (stretching ratio 0 to 150%). The results show that whether it is bent or stretched (stretching ratio 0-150%), the capacitance retention rate reaches more than 78%, which indicates that the prepared flexible stretchable supercapacitor has good tensile resistance.
[0093] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A method for preparing an integrated multiphase hydrogel, characterized in that: The following steps are involved: (1) Dissolving polyvinyl alcohol and phytic acid in water, then adding sulfuric acid, stirring at 75 to 95° C. for 2 to 3 h to obtain a homogeneous solution, and then cooling to room temperature to form a PVA / SA / PA semi-gel electrolyte; the PVA / SA / PA semi-gel electrolyte is composed of the following raw materials by mass fraction: polyvinyl alcohol 13.76 to 26.20%, phytic acid 58.07 to 80.64%, and the rest sulfuric acid; (2) Dissolve polyvinyl alcohol in phytic acid, stir at 75-95°C for 2-3 h, then add ammonium persulfate and heteropoly acid to obtain a homogeneous solution, then add phytic acid and aniline to the solution, stir continuously at 75-95°C for 3-4 h, and freeze at -30--20°C for 4-6 h to obtain a PVA / PA / PANI / HPA semi-gel electrode; the heteropoly acid is H3PW 12 O 40 and H3PMo 12 O 40 The PVA / PA / PANI / HPA semi-gel electrode is composed of the following raw materials by mass fraction: polyvinyl alcohol 7.97 ~ 10.4%, phytic acid 53.14 ~ 69.84%, heteropoly acid 9.52 ~ 29.63%, aniline 1.72% ~ 2.44%, and the rest is ammonium persulfate; (3) Inject the PVA / SA / PA semi-gel electrolyte into the mold, and then inject the PVA / PA / PANI / HPA semi-gel electrode into the PVA / SA / PA semi-gel electrolyte to form parallel electrodes with controllable spacing; cover the mold with the PVA / SA / PA semi-gel electrolyte to ensure that the PVA / PA / PANI / HPA is completely embedded in the bulk phase of the PVA / SA / PA semi-gel electrolyte; finally, freeze the mold and then thaw it at room temperature to obtain an integrated multiphase hydrogel.
2. The method for preparing an integrated multiphase hydrogel according to claim 1, characterized in that: In step (3), the freezing temperature is -30 to -20°C, the freezing time is 22 to 24 hours, and the thawing time is 2 to 3 hours.
3. An integrated multiphase hydrogel, characterized in that: Prepared by the method of claim 1 or 2.
4. The use of an integrated multiphase hydrogel in preparing a flexible stretchable supercapacitor according to claim 3, characterized in that: In the flexible and stretchable supercapacitor: an integrated multiphase hydrogel is used to ensure that two side-by-side gel electrodes are completely placed in the gel electrolyte during the preparation process to form an integrated multiphase gel containing both electrodes and electrolytes, and then a carbon cloth is connected to one end of each electrode to obtain a flexible and stretchable integrated multiphase gel supercapacitor.
5. The use of the integrated multiphase hydrogel in preparing a flexible stretchable supercapacitor according to claim 4, characterized in that: The gel electrode has a thickness of 3.0-3.5 mm, a length of 3.9-4.2 cm, a width of 1.0-2.0 cm, and a distance between the gel electrodes of 2.2-3.0 mm.
6. The use of the integrated multiphase hydrogel in preparing a flexible stretchable supercapacitor according to claim 4, characterized in that: The two side-by-side gel electrodes are formed by a pair of parallel electrodes, or a plurality of parallel electrodes connected in series.
Citation Information
Cited By
A two-dimensional stretchable supercapacitor based on a viscous electrolyte and a preparation method thereof
CN120709081B