Aluminum-wood-plastic composite door and window material and preparation method thereof
By using specific raw materials and preparation methods, the problem of insufficient mechanical and aging resistance of aluminum wood-plastic composite doors and windows is solved, and the high mechanical and mechanical properties and stability of the material are achieved, and the service life is extended.
Patent Information
- Application Number
- CN202311155775.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-08
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-09-08
AI Technical Summary
Traditional aluminum wood-plastic composite door and window materials have limited mechanical properties, poor performance stability, prone to cracking, insufficient product reliability and aging resistance, resulting in short service life.
Use plant fiber powder, end amino polypropylene, 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methacrylate/isopropenyl boric acid Pinna alcohol Ester/glycidyl methacrylate copolymer, glass fiber, 1,4-diamino-2,3-dicyanoanthraquinone, bis(3-aminophenyl) 3,5-bis(trifluoromethyl) The raw materials such as phenyl phosphine oxide are formed by the preparation method of extrusion molding and rolling composite of aluminum alloy members to form aluminum wood-plastic composite door and window materials.
It improves the mechanical and mechanical properties, aging resistance and performance stability of the material, extends the service life, the material is not easy to crack, and has good decorative effects and mechanical properties.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of building door and window manufacturing, and in particular to an aluminum-wood-plastic composite door and window material and a preparation method thereof. Background Art
[0002] In recent years, with the rapid development of economy and the continuous progress of society, the construction industry has also achieved unprecedented development, and high-rise buildings have sprung up. Behind these high-rise buildings, the use of doors and windows is indispensable. Doors and windows are an important part of the building envelope, and their materials directly affect the decorative effect, service life and mechanical properties. It can be seen that it is particularly important to develop door and window materials with good comprehensive performance and performance stability.
[0003] At present, the materials for doors and windows are generally made of plastic, wood or aluminum alloy. Aluminum alloy door and window materials have the characteristics of flame retardancy, insect resistance, and non-water absorption, but poor thermal insulation, heavy weight, and high cost. Wood door and window materials have good thermal insulation and light weight, but poor flame retardancy, easy to absorb water, deform, and cannot prevent insects. In addition, excessive logging of wood will have a huge impact on the environment. Although plastic door and window materials have good thermal insulation performance, they have poor weather resistance. In the natural environment, the surface loses its original gloss after a period of time, fades quickly, and the exposed part is prone to aging after a period of use. It is in this situation that aluminum-wood-plastic composite door and window materials came into being. Aluminum-wood-plastic composite door and window materials can combine and give full play to the advantages of aluminum and plastic wood to the maximum extent, and occupy an advantageous position in terms of UV resistance, aging resistance, thermal insulation, decorativeness, water tightness, air tightness, etc. However, the mechanical properties of traditional aluminum-wood-plastic composite door and window materials are limited, the performance stability is poor, and cracking is prone to occur due to compatibility issues. The product reliability needs to be further improved.
[0004] In order to solve the above problems, the Chinese invention patent with the authorization announcement number CN103467841B discloses an aluminum-plastic-wood composite material, including a plastic-wood component and an aluminum component. The raw materials and mass percentages of the plastic-wood component are: 55-75% polypropylene plastic, 10%-20% wood powder, 2-30% magnetic powder, 1-3% polyethylene grafted maleic anhydride and 0.5-3% dioctyl phthalate, and the surface of the aluminum component is nickel-plated. At the same time, the invention also discloses a preparation method of the aluminum-plastic-wood composite material. The aluminum-plastic-wood composite material prepared by the preparation method of the invention has strong compression and bending resistance. However, its aging resistance is insufficient, and due to compatibility issues, the product reliability and performance stability still need to be further improved.
[0005] It can be seen that the development of an aluminum-wood-plastic composite door and window material with good mechanical properties, sufficient aging resistance, good reliability, sufficient performance stability, not easy to crack, and long service life and its preparation method meet the market demand, have broad market value and application prospects, and are of great significance to promoting the development of the aluminum-wood-plastic composite material field. Summary of the invention
[0006] The main purpose of the present invention is to provide an aluminum-wood-plastic composite door and window material with good mechanical properties, sufficient aging resistance, good reliability, sufficient performance stability, not easy to crack, and long service life, and a preparation method thereof.
[0007] To achieve the above purpose, the present invention provides an aluminum-wood-plastic composite door and window material, comprising a door and window material body and an aluminum alloy component matched therewith, wherein the aluminum alloy component plays a role of a skeleton; the door and window material body is made of the following raw materials in parts by weight: 35-45 parts of plant fiber powder, 40-50 parts of amino-terminated polypropylene, 5-10 parts of 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methacrylate / isopropenylboronic acid pinacol ester / methacrylate glycidyl ester copolymer, 5-8 parts of glass fiber, 3-5 parts of 1,4-diamino-2,3-dicyanoanthraquinone, 1-3 parts of bis(3-aminophenyl) 3,5-bis(trifluoromethyl)phenylphosphine oxide, 1-3 parts of a coupling agent, 0.8-1.2 parts of an antioxidant, 1-3 parts of a lubricant, and 2-4 parts of an environmentally friendly plasticizer.
[0008] Preferably, the environmentally friendly plasticizer is epoxidized soybean oil.
[0009] Preferably, the lubricant is at least one of paraffin and ethylenebisoleamide; the antioxidant is one or more of antioxidant 1010, antioxidant 1076, and antioxidant 168.
[0010] Preferably, the coupling agent is at least one of silane coupling agent KH550, silane coupling agent KH560, and silane coupling agent KH570.
[0011] Preferably, the glass fiber is alkali-free chopped glass fiber, with a single fiber diameter of 3-9 microns and a length of 1-3 mm.
[0012] Preferably, the preparation method of the 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methacrylate / isopropenylboronic acid pinacol ester / glycidyl methacrylate copolymer comprises the following steps: adding 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methacrylate, isopropenylboronic acid pinacol ester, glycidyl methacrylate, and an initiator to a high boiling point solvent, stirring and reacting at 50-65° C. in an inert gas atmosphere for 3-5 hours, then precipitating in water, washing the precipitated polymer with ethanol for 3-6 times, and finally drying in a vacuum drying oven at 85-95° C. to constant weight.
[0013] Preferably, the mass ratio of the 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methacrylate, isopropenylboronic acid pinacol ester, glycidyl methacrylate, initiator, and high boiling point solvent is 1:1:(2-3):(0.04-0.06):(15-25).
[0014] Preferably, the initiator is azobisisobutyronitrile; the high boiling point solvent is at least one of dimethyl sulfoxide, N,N-dimethylformamide, and N-methylpyrrolidone; and the inert gas is any one of nitrogen, helium, neon, and argon.
[0015] Preferably, the molecular weight of the amino-terminated polypropylene is 13000-90000 g / mol, and the amino-terminated functionality is 0.80-0.92.
[0016] More preferably, the amino-terminated polypropylene is prepared according to the method of Example 8 in Chinese invention patent CN101812147B.
[0017] Preferably, the plant fiber powder is at least one of wood fiber powder, hemp fiber powder, bamboo fiber powder, grass fiber powder, bran powder or straw fiber powder.
[0018] Preferably, the particle size of the plant fiber powder is 50-200 mesh.
[0019] Another object of the present invention is to provide a method for preparing the aluminum-wood-plastic composite door and window material, comprising the following steps: drying the plant fiber powder at 100-120°C for 1-3 hours, then mixing it evenly with other raw materials, adding it to an extruder, and extruding it through a mold to obtain a blank; then rolling and compounding an aluminum alloy component matching the blank to obtain the aluminum-plastic-wood composite door and window material.
[0020] Preferably, the temperature of the extruder is 175-195° C., and the head pressure of the extruder is 13-18 MPa.
[0021] Due to the application of the above technical solution, the present invention has the following beneficial effects:
[0022] The preparation method of the aluminum-wood-plastic composite door and window material disclosed by the invention has simple process, convenient operation and control, low energy consumption, high preparation efficiency and finished product qualification rate, is suitable for continuous large-scale production, and has high promotion and application value.
[0023] The aluminum-wood-plastic composite door and window material disclosed in the present invention comprises a door and window material body and an aluminum alloy component matched therewith, wherein the aluminum alloy component plays a role of a skeleton; through such a structural design, the advantages of aluminum alloy, plastic and wood are integrated into one, and the material has good decorative effect, good mechanical properties, is not easy to deform, is excellent in aging resistance and has a long service life; through the reasonable selection of raw materials for preparing the door and window material body and the content thereof, the material body is well combined with the aluminum alloy component, the structural stability is improved and the service life is prolonged.
[0024] The aluminum-wood-plastic composite door and window material disclosed by the present invention is made of the following raw materials by weight: 35-45 parts of plant fiber powder, 40-50 parts of amino-terminated polypropylene, 5-10 parts of 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methacrylate / isopropenylboric acid pinacol ester / methacrylate glycidyl copolymer, 5-8 parts of glass fiber, 3-5 parts of 1,4-diamino-2,3-dicyanoanthraquinone, 1-3 parts of bis(3-aminophenyl) 3,5-bis(trifluoromethyl)phenylphosphine oxide, 1-3 parts of coupling agent, 0.8-1.2 parts of antioxidant, 1-3 parts of lubricant, and 2-4 parts of environmentally friendly plasticizer. Through the mutual cooperation and joint action between the raw materials, the manufactured door and window material has good mechanical properties, sufficient aging resistance, good reliability, sufficient performance stability, is not easy to crack, and has a long service life.
[0025] The aluminum-wood-plastic composite door and window material disclosed by the present invention, the epoxy group on the copolymer of 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methacrylate / isopropenyl boric acid pinacol ester / methacrylate glycidyl ester can react with the amino groups on the amino-terminated polypropylene, 1,4-diamino-2,3-dicyanoanthraquinone and bis(3-aminophenyl) 3,5-bis(trifluoromethyl)phenylphosphine oxide to form an interpenetrating network structure, which effectively improves the mechanical properties, aging resistance and performance stability of the product and prolongs its service life. Through the above raw materials, benzotriazole, boric acid pinacol ester, cyanoanthraquinone and trifluoromethylphenylphosphine oxide structures are simultaneously introduced into the material, and these structures, under the multiple effects of electronic effect, steric effect and conjugation effect, further improve the above performance of the manufactured product, thereby effectively improving the reliability of the product. DETAILED DESCRIPTION
[0026] The following description is used to disclose the present invention so that those skilled in the art can implement the present invention. The preferred embodiments described below are only examples, and those skilled in the art may think of other obvious variations. Example 1
[0027] An aluminum-wood-plastic composite door and window material comprises a door and window material body and an aluminum alloy component matched therewith, wherein the aluminum alloy component acts as a skeleton; the door and window material body is made of the following raw materials in parts by weight: 35 parts of plant fiber powder, 40 parts of amino-terminated polypropylene, 5 parts of 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methacrylate / isopropenylboronic acid pinacol ester / methacrylate glycidyl ester copolymer, 5 parts of glass fiber, 3 parts of 1,4-diamino-2,3-dicyanoanthraquinone, 1 part of bis(3-aminophenyl) 3,5-bis(trifluoromethyl)phenylphosphine oxide, 1 part of coupling agent, 0.8 part of antioxidant, 1 part of lubricant, and 2 parts of environmentally friendly plasticizer.
[0028] The environmentally friendly plasticizer is epoxidized soybean oil; the lubricant is paraffin; the antioxidant is antioxidant 1010; the coupling agent is silane coupling agent KH550; and the glass fiber is alkali-free chopped glass fiber, with a single filament diameter of 3 microns and a length of 1 mm.
[0029] The preparation method of the 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methacrylate / isopropenylboronic acid pinacol ester / glycidyl methacrylate copolymer comprises the following steps: adding 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methacrylate, isopropenylboronic acid pinacol ester, glycidyl methacrylate and an initiator into a high boiling point solvent, stirring and reacting at 50° C. for 3 hours in an inert gas atmosphere. The precipitated polymer was washed with ethanol for 3 times and then dried in a vacuum oven at 85°C to constant weight. The mass ratio of 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methacrylate, isopropenylboronic acid pinacol ester, glycidyl methacrylate, initiator and high boiling point solvent was 1:1:2:0.04:15. The initiator was azobisisobutyronitrile. The high boiling point solvent was dimethyl sulfoxide. The inert gas was nitrogen. The M of the copolymer was tested by GPC. n =15163g / mol,M W / M n =1.337; quantitative element analysis confirmed that the mass ratio of the structural units introduced by 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methacrylate, isopropenylboronic acid pinacol ester, and glycidyl methacrylate in the copolymer was 0.99:0.97:1.98.
[0030] The amino-terminated polypropylene is prepared according to the method of Example 8 in Chinese invention patent CN101812147B; the plant fiber powder is wood fiber powder; and the particle size of the plant fiber powder is 50 meshes.
[0031] A preparation method of the aluminum-wood-plastic composite door and window material comprises the following steps: drying the plant fiber powder at 100°C for 1 hour, then uniformly mixing it with other raw materials, adding it into an extruder, and extruding it through a mold to obtain a blank; then rolling and compounding an aluminum alloy component matching the blank to obtain the aluminum-plastic-wood composite door and window material; the temperature of the extruder is 175°C, and the head pressure of the extruder is 13MPa. Example 2
[0032] An aluminum-wood-plastic composite door and window material comprises a door and window material body and an aluminum alloy component matched therewith, wherein the aluminum alloy component acts as a skeleton; the door and window material body is made of the following raw materials in parts by weight: 38 parts of plant fiber powder, 42 parts of amino-terminated polypropylene, 6 parts of 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methacrylate / isopropenylboronic acid pinacol ester / methacrylate glycidyl ester copolymer, 6 parts of glass fiber, 3.5 parts of 1,4-diamino-2,3-dicyanoanthraquinone, 1.5 parts of bis(3-aminophenyl) 3,5-bis(trifluoromethyl)phenylphosphine oxide, 1.5 parts of coupling agent, 0.9 parts of antioxidant, 1.5 parts of lubricant, and 2.5 parts of environmentally friendly plasticizer.
[0033] The environmentally friendly plasticizer is epoxy soybean oil; the lubricant is ethylene bisoleamide; the antioxidant is antioxidant 1076; the coupling agent is silane coupling agent KH560; the glass fiber is alkali-free chopped glass fiber, with a single filament diameter of 6 microns and a length of 1.5 mm.
[0034] The preparation method of the 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methacrylate / isopropenylboronic acid pinacol ester / glycidyl methacrylate copolymer comprises the following steps: adding 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methacrylate, isopropenylboronic acid pinacol ester, glycidyl methacrylate and an initiator into a high boiling point solvent, stirring and reacting at 55° C. for 3.5 hours in an inert gas atmosphere, and then The polymer was precipitated in water, and the precipitated polymer was washed with ethanol for 4 times, and finally dried in a vacuum drying oven at 88° C. to constant weight; the mass ratio of 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methacrylate, isopropenylboronic acid pinacol ester, glycidyl methacrylate, initiator, and high boiling point solvent was 1:1:2.3:0.045:18; the initiator was azobisisobutyronitrile; the high boiling point solvent was N,N-dimethylformamide; and the inert gas was helium.
[0035] The amino-terminated polypropylene is prepared according to the method of Example 8 in Chinese invention patent CN101812147B; the plant fiber powder is hemp fiber powder; and the particle size of the plant fiber powder is 100 meshes.
[0036] A preparation method of the aluminum-wood-plastic composite door and window material comprises the following steps: drying the plant fiber powder at 105°C for 1.5 hours, then mixing it evenly with other raw materials, adding it into an extruder, and extruding it through a mold to obtain a blank; then rolling and compounding an aluminum alloy component matching the blank to obtain the aluminum-plastic-wood composite door and window material; the temperature of the extruder is 180°C, and the head pressure of the extruder is 15MPa. Example 3
[0037] An aluminum-wood-plastic composite door and window material comprises a door and window material body and an aluminum alloy component matched therewith, wherein the aluminum alloy component acts as a skeleton; the door and window material body is made of the following raw materials in parts by weight: 40 parts of plant fiber powder, 45 parts of amino-terminated polypropylene, 8 parts of 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methacrylate / isopropenylboronic acid pinacol ester / methacrylate glycidyl ester copolymer, 6.5 parts of glass fiber, 4 parts of 1,4-diamino-2,3-dicyanoanthraquinone, 2 parts of bis(3-aminophenyl) 3,5-bis(trifluoromethyl)phenylphosphine oxide, 2 parts of coupling agent, 1 part of antioxidant, 2 parts of lubricant, and 3 parts of environmentally friendly plasticizer.
[0038] The environmentally friendly plasticizer is epoxidized soybean oil; the lubricant is paraffin; the antioxidant is antioxidant 168; the coupling agent is silane coupling agent KH570; and the glass fiber is alkali-free chopped glass fiber, with a single filament diameter of 7 microns and a length of 2 mm.
[0039] The preparation method of the 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methacrylate / isopropenylboronic acid pinacol ester / glycidyl methacrylate copolymer comprises the following steps: adding 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methacrylate, isopropenylboronic acid pinacol ester, glycidyl methacrylate and an initiator into a high boiling point solvent, stirring and reacting at 59° C. for 4 hours in an inert gas atmosphere, and then The polymer was precipitated in water, washed with ethanol for 5 times, and finally dried in a vacuum drying oven at 90°C to constant weight; the mass ratio of 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methacrylate, isopropenylboronic acid pinacol ester, glycidyl methacrylate, initiator, and high boiling point solvent was 1:1:2.5:0.05:20; the initiator was azobisisobutyronitrile; the high boiling point solvent was N-methylpyrrolidone; and the inert gas was neon.
[0040] The amino-terminated polypropylene is prepared according to the method of Example 8 in Chinese invention patent CN101812147B; the plant fiber powder is bamboo fiber powder; and the particle size of the plant fiber powder is 130 meshes.
[0041] A preparation method of the aluminum-wood-plastic composite door and window material comprises the following steps: drying the plant fiber powder at 110°C for 2 hours, then mixing it evenly with other raw materials, adding it into an extruder, and extruding it through a mold to obtain a blank; then rolling and compounding an aluminum alloy component matching the blank to obtain the aluminum-plastic-wood composite door and window material; the temperature of the extruder is 185°C, and the head pressure of the extruder is 16MPa. Example 4
[0042] An aluminum-wood-plastic composite door and window material comprises a door and window material body and an aluminum alloy component matched therewith, wherein the aluminum alloy component acts as a skeleton; the door and window material body is made of the following raw materials in parts by weight: 43 parts of plant fiber powder, 48 parts of amino-terminated polypropylene, 9 parts of 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methacrylate / isopropenylboronic acid pinacol ester / methacrylate glycidyl ester copolymer, 7.5 parts of glass fiber, 4.5 parts of 1,4-diamino-2,3-dicyanoanthraquinone, 2.5 parts of bis(3-aminophenyl) 3,5-bis(trifluoromethyl)phenylphosphine oxide, 2.5 parts of coupling agent, 1.1 parts of antioxidant, 2.5 parts of lubricant, and 3.5 parts of environmentally friendly plasticizer.
[0043] The environmentally friendly plasticizer is epoxy soybean oil; the lubricant is a mixture of paraffin and ethylene bisoleamide in a mass ratio of 3:5; the antioxidant is a mixture of antioxidant 1010, antioxidant 1076, and antioxidant 168 in a mass ratio of 1:2:4; the coupling agent is a mixture of silane coupling agent KH550, silane coupling agent KH560, and silane coupling agent KH570 in a mass ratio of 2:1:3; the glass fiber is alkali-free chopped glass fiber, and the single fiber diameter is 8 microns and the length is 2.5 mm.
[0044] The preparation method of the 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methacrylate / isopropenylboronic acid pinacol ester / glycidyl methacrylate copolymer comprises the following steps: adding 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methacrylate, isopropenylboronic acid pinacol ester, glycidyl methacrylate and an initiator into a high boiling point solvent, stirring and reacting at 63°C in an inert gas atmosphere for 4.5 hours, then precipitating in water, washing the precipitated polymer with ethanol for 3-6 times, and finally drying in a vacuum drying oven at 93°C to constant weight.
[0045] The mass ratio of the 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methacrylate, isopropenylboronic acid pinacol ester, glycidyl methacrylate, initiator, and high boiling point solvent is 1:1:2.8:0.055:23; the initiator is azobisisobutyronitrile; the high boiling point solvent is a mixture of dimethyl sulfoxide, N,N-dimethylformamide, and N-methylpyrrolidone in a mass ratio of 1:3:4; and the inert gas is argon.
[0046] The amino-terminated polypropylene is made according to the method of Example 8 in Chinese invention patent CN101812147B; the plant fiber powder is a mixture of wood fiber powder, hemp fiber powder, bamboo fiber powder, grass fiber powder, bran powder, and straw fiber powder in a mass ratio of 1:1:2:1:3:1; the particle size of the plant fiber powder is 180 meshes.
[0047] A preparation method of the aluminum-wood-plastic composite door and window material comprises the following steps: drying the plant fiber powder at 115°C for 2.5 hours, then mixing it evenly with other raw materials, adding it into an extruder, and extruding it through a mold to obtain a blank; then rolling and compounding an aluminum alloy component matching the blank to obtain the aluminum-plastic-wood composite door and window material; the temperature of the extruder is 190°C, and the head pressure of the extruder is 17MPa. Example 5
[0048] An aluminum-wood-plastic composite door and window material comprises a door and window material body and an aluminum alloy component matched therewith, wherein the aluminum alloy component acts as a skeleton; the door and window material body is made of the following raw materials in parts by weight: 45 parts of plant fiber powder, 50 parts of amino-terminated polypropylene, 10 parts of 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methacrylate / isopropenylboronic acid pinacol ester / methacrylate glycidyl ester copolymer, 8 parts of glass fiber, 5 parts of 1,4-diamino-2,3-dicyanoanthraquinone, 3 parts of bis(3-aminophenyl) 3,5-bis(trifluoromethyl)phenylphosphine oxide, 3 parts of coupling agent, 1.2 parts of antioxidant, 3 parts of lubricant, and 4 parts of environmentally friendly plasticizer.
[0049] The environmentally friendly plasticizer is epoxy soybean oil; the lubricant is ethylene bisoleamide; the antioxidant is antioxidant 1010; the coupling agent is silane coupling agent KH560; the glass fiber is alkali-free chopped glass fiber, with a single filament diameter of 9 microns and a length of 3 mm.
[0050] The preparation method of the 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methacrylate / isopropenylboronic acid pinacol ester / glycidyl methacrylate copolymer comprises the following steps: adding 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methacrylate, isopropenylboronic acid pinacol ester, glycidyl methacrylate and an initiator into a high boiling point solvent, stirring and reacting at 65° C. for 5 hours in an inert gas atmosphere, and then The polymer was precipitated in water, washed with ethanol for 6 times, and finally dried in a vacuum drying oven at 95° C. to constant weight; the mass ratio of 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methacrylate, isopropenylboronic acid pinacol ester, glycidyl methacrylate, initiator, and high boiling point solvent was 1:1:3:0.06:25; the initiator was azobisisobutyronitrile; the high boiling point solvent was N,N-dimethylformamide; and the inert gas was nitrogen.
[0051] The amino-terminated polypropylene is prepared according to the method of Example 8 in Chinese invention patent CN101812147B; the plant fiber powder is wood fiber powder; and the particle size of the plant fiber powder is 200 meshes.
[0052] A preparation method of the aluminum-wood-plastic composite door and window material comprises the following steps: drying the plant fiber powder at 120°C for 3 hours, then mixing it evenly with other raw materials, adding it into an extruder, and extruding it through a mold to obtain a blank; then rolling and compounding an aluminum alloy component matching the blank to obtain the aluminum-plastic-wood composite door and window material; the temperature of the extruder is 195°C, and the head pressure of the extruder is 18MPa.
[0053] Comparative Example 1
[0054] An aluminum-wood-plastic composite door and window material is substantially the same as Example 1, except that 1,4-diamino-2,3-dicyanoanthraquinone and isopropenylboronic acid pinacol ester are not added.
[0055] Comparative Example 2
[0056] An aluminum-wood-plastic composite door and window material is substantially the same as Example 1, except that bis(3-aminophenyl) 3,5-bis(trifluoromethyl)phenylphosphine oxide and 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methacrylate are not added.
[0057] In order to further illustrate the beneficial technical effects of the aluminum-wood-plastic composite door and window materials involved in each embodiment of the present invention, the aluminum-wood-plastic composite door and window materials involved in Examples 1-5 and Comparative Examples 1-2 were subjected to relevant performance tests. The test results are shown in Table 1. The test method is as follows: According to GB / T7106-2019, the wind pressure resistance, air tightness and water tightness tests were carried out. The aging resistance test was carried out by placing the aluminum-wood-plastic composite door and window materials involved in each example in hot air at 90°C for artificial accelerated aging for 150 hours, cooling to room temperature, and then referring to GB / T7106-2019 for wind pressure resistance test again, and calculating the wind pressure resistance classification index value retention rate. The larger the value, the better the heat aging resistance. The wind pressure resistance, air tightness and water tightness values in the table are all classification index values. For the comparability of experimental data, the overall size structure of each door and window is guaranteed to be consistent during the test process.
[0058] Table 1
[0059] project Wind pressure resistance Airtightness Water tightness Aging resistance unit KPa <![CDATA[m 3 / (m·h)]]> Pa % Example 1 4.5 1.1 500 93.33 Example 2 4.8 0.8 600 95.83 Example 3 5.0 0.7 600 97.00 Example 4 5.1 0.5 700 98.04 Example 5 5.5 0.4 700 99.10 Comparative Example 1 4.0 1.7 350 87.50 Comparative Example 2 3.8 2.0 400 84.21
[0060] As can be seen from Table 1, the aluminum-wood-plastic composite door and window material disclosed in the embodiment of the present invention has better mechanical properties, air tightness and water tightness than the comparative example product, and has better aging resistance. The addition of 1,4-diamino-2,3-dicyanoanthraquinone, isopropenylboronic acid pinacol ester, bis(3-aminophenyl) 3,5-bis(trifluoromethyl)phenylphosphine oxide and 2-[3-(2H-benzotriazol-2-yl)-4-hydroxyphenyl]ethyl 2-methacrylate is beneficial to improving the above properties.
[0061] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The above embodiments and descriptions only describe the principles of the present invention. The present invention may be subject to various changes and improvements without departing from the spirit and scope of the present invention. These changes and improvements fall within the scope of the present invention. The scope of protection claimed by the present invention is defined by the attached claims and their equivalents.
Claims
1. A kind of aluminum-wood-plastic composite door and window material, It is characterized in that The invention comprises a door and window material body and an aluminum alloy component matched therewith, wherein the aluminum alloy component plays a role of a skeleton; the door and window material body is made of the following raw materials in parts by weight: 35-45 parts of plant fiber powder, 40-50 parts of amino-terminated polypropylene, 5-10 parts of 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methacrylate / isopropenylboronic acid pinacol ester / methacrylate glycidyl ester copolymer, 5-8 parts of glass fiber, 3-5 parts of 1,4-diamino-2,3-dicyanoanthraquinone, 1-3 parts of bis(3-aminophenyl) 3,5-bis(trifluoromethyl)phenylphosphine oxide, 1-3 parts of a coupling agent, 0.8-1.2 parts of an antioxidant, 1-3 parts of a lubricant, and 2-4 parts of an environmentally friendly plasticizer; The preparation method of the 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methacrylate / isopropenylboronic acid pinacol ester / glycidyl methacrylate copolymer comprises the following steps: adding 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methacrylate, isopropenylboronic acid pinacol ester, glycidyl methacrylate and an initiator into a high boiling point solvent, stirring and reacting at 50-65° C. for 3-5 hours in an inert gas atmosphere, then precipitating in water, and The precipitated polymer is washed with ethanol for 3-6 times, and finally placed in a vacuum drying oven at 85-95° C. to dry to constant weight; the mass ratio of the 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methacrylate, isopropenylboronic acid pinacol ester, glycidyl methacrylate, initiator, and high boiling point solvent is 1:1:(2-3):(0.04-0.06):(15-25); the high boiling point solvent is at least one of dimethyl sulfoxide, N,N-dimethylformamide, and N-methylpyrrolidone.
2. According to claim 1, the aluminum-wood-plastic composite door and window material, It is characterized in that The environmentally friendly plasticizer is epoxidized soybean oil; the lubricant is at least one of paraffin wax and ethylene bisoleamide; the antioxidant is one or more of antioxidant 1010, antioxidant 1076, and antioxidant 168.
3. The aluminum-wood-plastic composite door and window material according to claim 1, It is characterized in that The coupling agent is at least one of silane coupling agent KH550, silane coupling agent KH560 and silane coupling agent KH570; the glass fiber is alkali-free chopped glass fiber, with a single fiber diameter of 3-9 μm and a length of 1-3 mm.
4. The aluminum-wood-plastic composite door and window material according to claim 1, It is characterized in that The initiator is azobisisobutyronitrile; the inert gas is any one of nitrogen, helium, neon and argon.
5. The aluminum-wood-plastic composite door and window material according to claim 1, It is characterized in that The molecular weight of the amino-terminated polypropylene is 13000-90000 g / mol, and the amino-terminated functionality is 0.80-0.
92.
6. The aluminum-wood-plastic composite door and window material according to claim 1, It is characterized in that The plant fiber powder is at least one of wood fiber powder, hemp fiber powder, bamboo fiber powder, grass fiber powder, bran powder or straw fiber powder; the particle size of the plant fiber powder is 50-200 meshes.
7. A method for preparing the aluminum-wood-plastic composite door and window material according to any one of claims 1 to 6, It is characterized in that The method comprises the following steps: drying the plant fiber powder at 100-120°C for 1-3 hours, then uniformly mixing the plant fiber powder with other raw materials, adding the powder into an extruder, extruding the powder through a mold to obtain a blank; and then rolling and compounding an aluminum alloy component matching the blank to obtain an aluminum-wood-plastic composite door and window material.
8. The method for preparing the aluminum-wood-plastic composite door and window material according to claim 7, It is characterized in that The temperature of the extruder is 175-195° C., and the head pressure of the extruder is 13-18 MPa.
Citation Information
Patent Citations
Amino-terminated polypropylene and preparation method thereof
CN101812147B
A kind of aluminum plastic wood composite material and preparation method thereof
CN103467841B
High-temperature resistant adhesive containing phosphonyl polyimide and preparation method thereof
CN101709212A
Composite film containing 4-methyl-1-pentene polymer and demoulding film comprising same
CN112793271A
Double-component thermosetting epoxy glue with low water absorption rate as well as preparation method and application thereof