A kind of wear-resistant, corrosion-resistant and high-temperature resistant bearing lubricating oil and preparation method thereof
By connecting anti-wear agents and adding anti-corrosion additives to the surface of mercapto-sepiolite, the problem of insufficient anti-wear and anti-corrosion properties of traditional lubricating oils at high temperatures is solved, and the excellent anti-wear, friction-reducing and corrosion-resistant properties of lubricating oils at high temperatures are achieved. properties, extending service life.
Patent Information
- Application Number
- CN202311137863.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-05
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-09-05
AI Technical Summary
The extreme pressure anti-wear agents in traditional lubricants contain sulfur, phosphorus, and chloride. Although they are hard, they are fragile and easy to fall off, causing corrosion of machine parts and consumption of additives. They have a short service life and are difficult to maintain anti-wear and anti-corrosion properties at high temperatures.
It uses anti-wear and corrosion-resistant lubricating oil that does not contain sulfur, phosphorus and chloride. It is prepared by connecting an anti-wear agent on the surface of mercapto-sepiolite. It combines the anti-wear agent formed by the reaction of fatty alcohol amine, boric acid and diethyl phosphite. Naphthalene-containing polyaramid and phenylene ether amide are added as anti-corrosion additives to enhance the anti-wear and anti-corrosion properties of the lubricating oil.
The anti-wear, anti-friction and anti-corrosion properties of lubricating oil are significantly improved at high temperatures, extending the service life. It is suitable for high-speed machinery and industrial gears, and reduces the friction coefficient and corrosion risk.
Smart Images

Figure BDA0004432464990000101
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of lubricants, and in particular to a wear-resistant, corrosion-resistant and high-temperature-resistant bearing lubricating oil and a preparation method thereof. Background Art
[0002] Lubricating oil is a liquid or semi-solid lubricant used in various types of automobiles and mechanical equipment to reduce friction and protect machinery and processed parts. It mainly plays the role of lubrication and buffering. When the engine is running or stored, the moisture in the atmosphere, lubricating oil, fuel, and acidic gases produced by combustion will cause corrosion and rust to the parts, thereby increasing the damage to the friction surface. The oil film formed by lubricating oil on the surface of the parts can prevent the parts from direct contact with water and acidic gases, preventing corrosion and rust.
[0003] The extreme pressure anti-wear agents in traditional lubricating oils are often sulfur, phosphorus, and chlorides, which generate metal compounds with friction pairs through instantaneous high temperature and high pressure of boundary lubrication to improve hardness and wear resistance. Although this compound is hard, it is very brittle. It constantly falls off and forms during the friction process, which not only corrodes the parts, but also consumes additives. The service life of both the machinery and the lubricating oil is very short. Therefore, the present invention studies and prepares a wear-resistant, corrosion-resistant, and high-temperature bearing lubricating oil that does not contain sulfur, phosphorus, and chlorides. It has excellent wear resistance and corrosion resistance at high temperatures and is suitable for the lubrication of high-speed wire mills, plate mills, and thin plate cold rolling units in steel plants. It can also be used for the lubrication of rough and medium continuous rolling units and rolling mill support roller bearings and other parts. It can also be used for the lubrication of various high-speed, medium-speed, and low-speed industrial gears, worm gears, rolling bearings, and anti-friction bearings. It is suitable for the lubrication of the circulation system of large rolling mills and high-speed rolling mills in the steel and metallurgical industry. Summary of the invention
[0004] The object of the present invention is to provide a wear-resistant, corrosion-resistant and high-temperature-resistant bearing lubricant and a preparation method thereof, so as to solve the problems raised in the above-mentioned background technology.
[0005] In order to solve the above technical problems, the present invention provides the following technical solutions: a wear-resistant, corrosion-resistant and high-temperature resistant bearing lubricant, which comprises a base oil, an extreme pressure anti-wear agent, an anti-corrosion additive and a viscosity index improver.
[0006] Preferably, the extreme pressure anti-wear agent is obtained by connecting an anti-wear agent to the surface of mercapto sepiolite; the anti-wear agent is obtained by reacting fatty alcohol amine, boric acid and diethyl phosphite; the fatty alcohol amine is obtained by reacting oleic acid and diisopropanolamide.
[0007] Preferably, the base oil is selected from one or more of trimellitic acid esters and / or saturated polyol esters; the viscosity index improver is any one or more of Evonik VISCOPLEX 3-200, Evonik VISCOPLEX 3-201, and Evonik VISCOPLEX 3-220.
[0008] Preferably, the anti-corrosion additive is prepared by mixing naphthalene-containing polyaromatic amide and ether phenylamide; the naphthalene-containing polyaromatic amide is prepared by reacting naphthalene dicarboxylic acid with 2,2-bis[4-(4-aminophenoxy)phenyl]propane; and the phenyl ether amide is prepared by reacting polyperfluoromethyl ethyl ether carboxylic acid with aniline.
[0009] Preferably, the method for preparing the anti-wear, corrosion and high temperature resistant bearing lubricating oil comprises the following specific steps:
[0010] (1) In a nitrogen atmosphere, boric acid, fatty alcohol amine and diethyl phosphite are mixed in a mass ratio of 1:1.2 to 1.5:1, the temperature is raised to 150 to 170° C., and the reaction is carried out for 8 to 12 hours to obtain an anti-wear agent;
[0011] (2) Immerse the mercapto sepiolite in the anti-wear agent at 10-30 mW / cm 2 Irradiate with 365nm ultraviolet light for 20-40min, remove and wash with anhydrous ethanol and deionized water for 2-4 times, dry, and obtain an extreme pressure anti-wear agent;
[0012] (3) N-methylpyrrolidone and naphthalene-containing polyaromatic amide are mixed in a mass ratio of 20 to 40:3, stirred evenly, and then 0.4 to 0.8 times the mass of ether benzamide of the naphthalene-containing polyaromatic amide is added, the temperature is raised to 80 to 90° C., stirred at 300 to 500 rpm for reaction for 3 to 6 hours, the temperature is raised to 220 to 240° C., and the temperature is kept for 16 to 18 hours to prepare an anti-corrosion additive;
[0013] (4) The base oil is heated to 150-180° C., and under continuous stirring, the extreme pressure anti-wear agent, the anti-corrosion additive and the viscosity index improver are stirred evenly and then defoamed, and stirring is continued for 20-40 minutes to obtain an anti-wear, corrosion and high temperature resistant bearing lubricant.
[0014] Preferably, in the above step (1): the preparation method of the fatty alcohol amine is: heating oleic acid to 50-60° C., adding diisopropanolamine in an amount 1-1.5 times the mass of oleic acid, heating to 130-180° C., reacting for 2-6 hours, to obtain the fatty alcohol amine.
[0015] Preferably, in the above step (2): the preparation method of mercapto sepiolite is: sepiolite powder, ethanol and deionized water are mixed in a mass ratio of 1:8 to 10:2, the pH is adjusted to 3 to 4 with hydrochloric acid, ultrasonicated at 60 to 80 kHz for 50 to 80 min, and then 0.5 to 0.6 times the mass of sepiolite powder (3-mercaptopropyl) trimethoxysilane is added, the temperature is raised to 65 to 75° C., stirred at 100 to 300 rpm for reaction for 10 to 14 hours, filtered and washed with anhydrous ethanol and deionized water for 2 to 4 times in sequence, and finally dried and ground to obtain mercapto sepiolite.
[0016] Preferably, in the above step (3): the preparation method of naphthalene-containing polyaromatic amide: under a nitrogen atmosphere, 1,4-naphthalene dicarboxylic acid, 2,2-bis[4-(4-aminophenoxy)phenyl]propane and N-methyl-pyrrolidone are stirred and dissolved in a mass ratio of 2:3 to 3.4:30, and then lithium chloride (2 to 2.2 times the mass of 1,4-naphthalene dicarboxylic acid), triphenyl phosphite (4 to 5 times the mass of 1,4-naphthalene dicarboxylic acid) and pyridine (5 to 6 times the mass of 1,4-naphthalene dicarboxylic acid) are added, the temperature is raised to 108 to 110° C., the reaction is carried out for 6 to 8 hours, the mixture is transferred to methanol and soaked for 24 to 48 hours, and then the mixture is boiled with deionized water and methanol respectively, filtered for 3 to 5 times, and finally dried in a vacuum drying oven at 100 to 120° C. to obtain naphthalene-containing polyaromatic amide.
[0017] Preferably, in the above step (3): the preparation method of phenyl ether amide is: add 4-8% phosphoric acid with a mass fraction of 0.02-0.04 times the mass of the polyperfluoromethyl ether carboxylic acid at a rate of 1-3 mL / min, heat to 60-80° C. and react for 3-4 hours, cool to room temperature, add aniline with a mass fraction of 1-1.2 times the mass of the polyperfluoromethyl ether carboxylic acid under a nitrogen atmosphere, heat to 75-85° C., react for 10-12 hours, and distill under reduced pressure to obtain phenyl ether amide.
[0018] Preferably, in the above step (4), the mass ratio of the base oil, the extreme pressure anti-wear agent, the anti-corrosion additive and the viscosity index improver is 50-60:2-4:1-2:1.
[0019] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0020] The wear-resistant, corrosion-resistant and high-temperature-resistant bearing lubricating oil prepared by the present invention is prepared by adding an extreme pressure anti-wear agent and an anti-corrosion additive into a base oil;
[0021] The extreme pressure anti-wear agent is prepared by connecting the anti-wear agent to the surface of mercapto sepiolite; the anti-wear agent is prepared by the reaction of fatty alcohol amine, boric acid and diethyl phosphite, and the fatty alcohol amine is prepared by the reaction of oleic acid and diisopropanolamide; sepiolite has a strong adsorption capacity, and can be quickly adsorbed and deposited on the wear surface during the friction process, and grind, polish, fill and repair the micro-protrusions, pits and micro-damages on the wear surface, thereby reducing the roughness and enhancing the wear resistance of the extreme pressure anti-wear agent; the fatty alcohol amine can react with boric acid and diethyl phosphite to form an anti-wear agent with borate and phosphate, and the fatty alcohol amine generated by the reaction of oleic acid and diisopropanolamide has a strong steric hindrance effect, which tightly connects the borate and phosphate on the surface of mercapto sepiolite, and the borate can generate a layered boron nitride compound on the friction surface, which can form a protective film on the wear surface, reduce the friction coefficient, and improve the anti-wear and friction-reducing properties of the lubricating oil;
[0022] The anti-corrosion additive is a mixture of naphthalene-containing polyaromatic amide and phenyl ether amide. The naphthalene-containing polyaromatic amide is prepared by the reaction of naphthalene dicarboxylic acid and 2,2-bis[4-(4-aminophenoxy)phenyl]propane, and phenyl ether amide is prepared by the reaction of polyperfluoromethyl ether carboxylic acid and aniline. When polyperfluoromethyl ether carboxylic acid reacts with aniline to introduce a benzene ring, benzamide is formed, which can accept electrons from oxygen free radicals to prevent the reaction of oxygen free radicals, and can also give electrons to form a chemical adsorption film with metals to prevent metal catalytic decomposition and corrosion of metals. It can produce an anti-corrosion effect in the oil. Naphthalenedicarboxylic acid reacts with 2,2-bis[4-(4-aminophenoxy)phenyl]propane to undergo a phosphating reaction, introducing bisphenol A groups into the polymer molecular chains to increase the chain spacing. The phenyl ether bonds can also increase the flexibility of the chain segments, allowing the phenyl ether amide to entangle with the polar molecules of the naphthalene-containing polyaromatic amide to form a steric hindrance, and evenly disperse the extreme pressure anti-wear agent in the base oil. Under the combined action of the base oil trimellitic acid ester and the anti-corrosion additive, the anti-wear and friction-reducing properties of the lubricating oil at high temperatures are improved. DETAILED DESCRIPTION
[0023] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. In the embodiments of the present invention and the comparative examples, the base oil is Ruijie TMT-5, the viscosity index improver is Evonik VISCOPLEX 3-200, and the polyperfluoromethyl ether carboxylic acid is purchased from Great Wall Lubricant Group Co., Ltd., and the remaining reagents are all commercially available products.
[0024] In order to more clearly illustrate the method provided by the present invention, the following examples are used to describe in detail the various index testing methods of the anti-wear, corrosion and high temperature resistant bearing lubricating oils prepared in the examples and comparative examples as follows:
[0025] Wear resistance: After the wear-resistant, corrosion-resistant and high-temperature resistant bearing lubricants prepared in the examples and comparative examples were heat treated at 150°C for 8 hours, a four-ball load capacity test was performed before and after the heat treatment in accordance with GB / T3142 "Determination of the load-bearing capacity of lubricants - Four-ball method".
[0026] Corrosion resistance: After the wear-resistant, corrosion-resistant and high-temperature resistant bearing lubricating oils prepared in the examples and comparative examples were heat-treated at 150° C. for 8 hours, the copper sheet corrosion level test before and after the heat treatment was carried out in accordance with GB / T5096.
[0027] Coking property: The wear-resistant, corrosion-resistant and high-temperature resistant bearing lubricating oils prepared in the examples and comparative examples were tested for their coking quality at 150° C. for 20 hours using a lubricating oil high-temperature coking performance tester.
[0028] Example 1
[0029] (1) Raising the temperature of oleic acid to 50° C., adding diisopropanolamine (1 times the mass of oleic acid), raising the temperature to 130° C., and reacting for 2 hours to obtain a fatty alcohol amine; in a nitrogen atmosphere, mixing boric acid, fatty alcohol amine, and diethyl phosphite in a mass ratio of 1:1.2:1, raising the temperature to 150° C., and reacting for 8 hours to obtain an anti-wear agent;
[0030] (2) Mix sepiolite powder, ethanol and deionized water in a mass ratio of 1:8:2, adjust the pH to 3 with hydrochloric acid, perform ultrasonic treatment at 60 kHz for 50 min, add (3-mercaptopropyl)trimethoxysilane in an amount of 0.5 times the mass of the sepiolite powder, heat to 65° C., stir at 100 rpm for 10 h, filter and wash twice with anhydrous ethanol and deionized water in sequence, and finally dry and grind to obtain mercapto sepiolite; immerse the mercapto sepiolite in an anti-wear agent and perform ultrasonic treatment at 10 mW / cm 2 The mixture was irradiated with 365 nm ultraviolet light for 20 min, taken out and washed twice with anhydrous ethanol and deionized water in sequence, and dried to obtain an extreme pressure anti-wear agent;
[0031] (3) Under nitrogen atmosphere, 1,4-naphthalene dicarboxylic acid, 2,2-bis[4-(4-aminophenoxy)phenyl]propane and N-methyl-pyrrolidone were stirred and dissolved in a mass ratio of 2:3:30, and then lithium chloride (2 times the mass of 1,4-naphthalene dicarboxylic acid), triphenyl phosphite (4 times the mass of 1,4-naphthalene dicarboxylic acid) and pyridine (5 times the mass of 1,4-naphthalene dicarboxylic acid) were added, the temperature was raised to 108°C, the reaction was carried out for 6 hours, and the mixture was transferred to methanol and soaked for 24 hours. The mixture was then boiled and filtered three times with deionized water and methanol respectively, and finally dried in a vacuum drying oven at 100°C to obtain naphthalene-containing polyaromatic amide; and polyperfluoromethyl ethyl ether carboxylic acid was added with Add 4% phosphoric acid with a mass fraction of 0.02 times the mass of polyperfluoromethyl ethyl ether carboxylic acid at a rate of 1 mL / min, heat to 60°C for reaction for 3 hours, cool to room temperature, add aniline with a mass fraction of 1 times the mass of polyperfluoromethyl ethyl ether carboxylic acid under a nitrogen atmosphere, heat to 75°C, react for 10 hours, and distill under reduced pressure to obtain phenyl ether amide; mix N-methyl pyrrolidone and naphthalene-containing polyaromatic amide in a mass ratio of 20:3, stir evenly, add ether benzamide with a mass fraction of 0.4 times the mass of naphthalene-containing polyaromatic amide, heat to 80°C, stir at 300 rpm for reaction for 3 hours, heat to 220°C, and keep warm for 16 hours to obtain an anti-corrosion additive;
[0032] (4) The base oil is heated to 150° C., and under continuous stirring, the extreme pressure anti-wear agent, the anti-corrosion additive and the viscosity index improver are added in a mass ratio of 50:2:1:1, the base oil, the extreme pressure anti-wear agent, the anti-corrosion additive and the viscosity index improver, and the mixture is stirred evenly to remove the foam, and the stirring is continued for 20 minutes to obtain an anti-wear, corrosion and high temperature resistant bearing lubricant.
[0033] Example 2
[0034] (1) Raising the temperature of oleic acid to 55°C, adding diisopropanolamine (1.25 times the mass of oleic acid), raising the temperature to 1550°C, and reacting for 4 hours to obtain a fatty alcohol amine; in a nitrogen atmosphere, mixing boric acid, fatty alcohol amine, and diethyl phosphite in a mass ratio of 1:1.4:1, raising the temperature to 160°C, and reacting for 10 hours to obtain an anti-wear agent;
[0035] (2) Sepiolite powder, ethanol and deionized water were mixed in a mass ratio of 1:9:2, the pH value was adjusted to 3.5 with hydrochloric acid, ultrasonicated at 70 kHz for 70 min, and then (3-mercaptopropyl)trimethoxysilane (0.55 times the mass of the sepiolite powder) was added, the temperature was raised to 70°C, stirred at 200 rpm for 12 h, filtered and washed three times with anhydrous ethanol and deionized water in sequence, and finally dried and ground to obtain mercapto sepiolite; the mercapto sepiolite was immersed in an anti-wear agent and heated at 20 mW / cm 2 The mixture was irradiated with 365 nm ultraviolet light for 30 min, removed and washed three times with anhydrous ethanol and deionized water in sequence, and dried to obtain an extreme pressure anti-wear agent;
[0036] (3) Under nitrogen atmosphere, 1,4-naphthalene dicarboxylic acid, 2,2-bis[4-(4-aminophenoxy)phenyl]propane and N-methyl-pyrrolidone were stirred and dissolved in a mass ratio of 2:3.2:30, and then 2.1 times the mass of 1,4-naphthalene dicarboxylic acid lithium chloride, 4.5 times the mass of 1,4-naphthalene dicarboxylic acid triphenyl phosphite and 5.5 times the mass of 1,4-naphthalene dicarboxylic acid pyridine were added, the temperature was raised to 109°C, the reaction was carried out for 7 hours, and the mixture was transferred to methanol and soaked for 36 hours. The mixture was then boiled with deionized water and methanol, filtered 4 times, and finally dried in a vacuum drying oven at 110°C to obtain naphthalene-containing polyaromatic amide; and the mixture was added to polyperfluoromethyl ethyl ether carboxylic acid. Phosphoric acid with a mass fraction of 6% and a mass fraction of 0.03 times the mass of polyperfluoromethyl ethyl ether carboxylic acid is added dropwise at a rate of 2 mL / min, the temperature is raised to 70° C. and reacted for 3.5 hours, then the temperature is lowered to room temperature, and aniline with a mass fraction of 1.1 times the mass of polyperfluoromethyl ethyl ether carboxylic acid is added under a nitrogen atmosphere, the temperature is raised to 80° C., the reaction is carried out for 11 hours, and reduced pressure distillation is performed to obtain phenyl ether amide; N-methyl pyrrolidone and naphthalene-containing polyaromatic amide are mixed in a mass ratio of 30:3, stirred evenly, and ether phenyl amide with a mass fraction of 0.6 times the mass of naphthalene-containing polyaromatic amide is added, the temperature is raised to 85° C., stirred at 400 rpm for 4.5 hours, the temperature is raised to 230° C., and the temperature is kept for 17 hours to obtain an anti-corrosion additive;
[0037] (4) The base oil is heated to 165° C., and under continuous stirring, the extreme pressure anti-wear agent, the anti-corrosion additive and the viscosity index improver are added in a mass ratio of 55:3:1.5:1, the base oil, the extreme pressure anti-wear agent, the anti-corrosion additive and the viscosity index improver are stirred evenly and then defoamed, and stirring is continued for 30 minutes to obtain an anti-wear, corrosion and high temperature resistant bearing lubricant.
[0038] Example 3
[0039] (1) Raising the temperature of oleic acid to 60° C., adding diisopropanolamine (1.5 times the mass of oleic acid), raising the temperature to 180° C., and reacting for 6 hours to obtain a fatty alcohol amine; in a nitrogen atmosphere, mixing boric acid, fatty alcohol amine, and diethyl phosphite in a mass ratio of 1:1.5:1, raising the temperature to 170° C., and reacting for 12 hours to obtain an anti-wear agent;
[0040] (2) Mix sepiolite powder, ethanol and deionized water in a mass ratio of 1:10:2, adjust the pH to 4 with hydrochloric acid, perform ultrasonic treatment at 80 kHz for 80 min, add (3-mercaptopropyl)trimethoxysilane in an amount of 0.6 times the mass of the sepiolite powder, heat to 75°C, stir at 300 rpm for 14 h, filter and wash with anhydrous ethanol and deionized water four times in sequence, finally dry and grind to obtain mercapto sepiolite; immerse the mercapto sepiolite in an anti-wear agent and heat at 30 mW / cm 2 The mixture was irradiated with 365 nm ultraviolet light for 40 min, removed and washed four times with anhydrous ethanol and deionized water in sequence, and dried to obtain an extreme pressure anti-wear agent;
[0041] (3) Under nitrogen atmosphere, 1,4-naphthalene dicarboxylic acid, 2,2-bis[4-(4-aminophenoxy)phenyl]propane and N-methyl-pyrrolidone were stirred and dissolved in a mass ratio of 2:3.4:30, and then 2.2 times the mass of 1,4-naphthalene dicarboxylic acid lithium chloride, 5 times the mass of 1,4-naphthalene dicarboxylic acid triphenyl phosphite and 6 times the mass of 1,4-naphthalene dicarboxylic acid pyridine were added, the temperature was raised to 110°C, the reaction was carried out for 8 hours, the mixture was transferred to methanol and soaked for 48 hours, and then the mixture was boiled and filtered 5 times with deionized water and methanol respectively, and finally dried in a vacuum drying oven at 120°C to obtain naphthalene-containing polyaromatic amide; and the mixture was added to polyperfluoromethyl ethyl ether carboxylic acid. Phosphoric acid with a mass fraction of 8% and a mass fraction of 0.04 times the mass of polyperfluoromethyl ethyl ether carboxylic acid is added dropwise at a rate of 3 mL / min, the temperature is raised to 80° C. and reacted for 4 hours, then the temperature is lowered to room temperature, and aniline with a mass fraction of 1.2 times the mass of polyperfluoromethyl ethyl ether carboxylic acid is added under a nitrogen atmosphere, the temperature is raised to 85° C., the reaction is carried out for 12 hours, and reduced pressure distillation is performed to obtain phenyl ether amide; N-methyl pyrrolidone and naphthalene-containing polyaromatic amide are mixed in a mass ratio of 40:3, stirred evenly, and ether phenyl amide with a mass fraction of 0.8 times the mass of naphthalene-containing polyaromatic amide is added, the temperature is raised to 90° C., stirred at 500 rpm for 6 hours, the temperature is raised to 240° C., and the temperature is kept for 18 hours to obtain an anti-corrosion additive;
[0042] (4) The base oil is heated to 180° C., and under continuous stirring, the extreme pressure anti-wear agent, the anti-corrosion additive and the viscosity index improver are added in a mass ratio of 60:4:2:1, the base oil, the extreme pressure anti-wear agent, the anti-corrosion additive and the viscosity index improver, and the mixture is stirred evenly to remove the foam, and the stirring is continued for 40 minutes to obtain an anti-wear, corrosion and high temperature resistant bearing lubricant.
[0043] Comparative Example 1
[0044] The composition of comparative example 1 is the same as that of example 2. The difference between the method for preparing the wear-resistant, corrosion-resistant and high-temperature bearing lubricating oil and example 2 is that step (1) is different, and step (1) is modified as follows: heating oleic acid to 60° C., adding diisopropanolamine with a mass of 1.5 times that of oleic acid, heating to 180° C., reacting for 6 hours, and obtaining fatty alcohol amine; in a nitrogen atmosphere, mixing fatty alcohol amine and diethyl phosphite in a mass ratio of 1.5:1, heating to 170° C., and reacting for 12 hours, and obtaining an anti-wear agent.
[0045] Comparative Example 2
[0046] The composition of comparative example 2 is the same as that of example 2. The difference between the method for preparing the anti-wear, corrosion-resistant and high-temperature bearing lubricating oil and example 2 lies in the difference in step (1), which is modified as follows: heating oleic acid to 60°C, adding diisopropanolamine with a mass of 1.5 times that of oleic acid, heating to 180°C, reacting for 6 hours, and obtaining fatty alcohol amine; in a nitrogen atmosphere, mixing boric acid and fatty alcohol amine in a mass ratio of 1:1.5, heating to 170°C, and reacting for 12 hours, and obtaining an anti-wear agent.
[0047] Comparative Example 3
[0048] The composition of comparative example 3 is the same as that of example 2. The difference between the method for preparing the anti-wear, corrosion-resistant and high-temperature bearing lubricating oil and example 2 is only the difference in step (1), which is modified as follows: heating oleic acid to 60° C., adding diisopropanolamine with a mass of 1.5 times that of oleic acid, heating to 180° C., reacting for 6 hours, and obtaining fatty alcohol amine, which is an anti-wear agent.
[0049] Comparative Example 4
[0050] The composition of Comparative Example 4 is the same as that of Example 2. The difference between the method for preparing the anti-wear, corrosion-resistant and high-temperature resistant bearing lubricating oil and that of Example 2 is that the extreme pressure anti-wear agent is mercapto sepiolite.
[0051] Comparative Example 5
[0052] The composition of comparative example 5 is the same as that of example 2. The difference between the method for preparing the anti-wear, corrosion and high temperature bearing lubricating oil and that of example 2 is that the anti-corrosion additive is only naphthalene-containing polyaromatic amide.
[0053] Comparative Example 6
[0054] The composition of Comparative Example 6 is the same as that of Example 2. The difference between the method for preparing the anti-wear, corrosion, and high-temperature resistant bearing lubricating oil and that of Example 2 is that the anti-corrosion additive is only phenyl ether amide.
[0055] Comparative Example 7
[0056] The composition of comparative example 7 is the same as that of example 2. The difference between the method for preparing the anti-wear, corrosion and high temperature bearing lubricating oil and that of example 2 is that the anti-wear, corrosion and high temperature bearing lubricating oil further comprises base oil, extreme pressure anti-wear agent and viscosity index improver.
[0057] Effect example
[0058] Table 1 below shows the performance analysis results of the anti-wear, corrosion and high temperature resistant bearing lubricants of Examples 1 to 3 of the present invention and Comparative Examples 1 to 7:
[0059] Table 1
[0060]
[0061] By comparing the experimental data of the embodiments and the comparative examples in Table 1 and testing on the gearbox oil test platform, it can be clearly found that the wear-resistant, corrosion-resistant and high-temperature resistant bearing lubricants prepared using Examples 1, 2 and 3 have excellent anti-wear and anti-corrosion properties at high temperatures.
[0062] From the comparison of the experimental data of Example 1, Example 2, Example 3 and Comparative Example 1, Comparative Example 2, Comparative Example 3, Comparative Example 4, Comparative Example 7, it can be found that the anti-wear agent prepared by the reaction of fatty alcohol amine, boric acid and diethyl phosphite is connected to the surface of mercapto sepiolite to obtain an extreme pressure anti-wear agent, forming an anti-wear agent with borate and phosphate, and the fatty alcohol amine generated by the reaction of oleic acid and diisopropanolamide has a strong steric hindrance effect, which tightly connects the borate and phosphate on the surface of mercapto sepiolite. The borate can generate layered boron nitride compounds on the friction surface, which can form a protective film on the wear surface, reduce the friction coefficient, and improve the anti-wear and friction-reducing properties of the lubricating oil.
[0063] From the comparison of the experimental data of Example 1, Example 2, Example 3 and Comparative Example 5, Comparative Example 6, Comparative Example 7, it can be found that when polyperfluoromethyl ethyl ether carboxylic acid reacts with aniline to introduce benzene rings, benzamide is formed, which can not only accept electrons from oxygen free radicals to prevent oxygen free radical reactions, but also donate electrons to form a chemical adsorption film with metals to prevent metal catalytic decomposition and corrosion of metals. Adding it to the base oil can produce an anti-corrosion effect. Naphthalenedicarboxylic acid reacts with 2,2-bis[4-(4-aminophenoxy)phenyl]propane to introduce bisphenol A groups into the polymer molecular chains to increase the chain spacing. The phenyl ether bond can also increase the flexibility of the chain segments, so that the phenyl ether amide can be entangled with the polar molecules of the naphthalene-containing polyaromatic amide to form a steric hindrance, and the extreme pressure anti-wear agent is evenly dispersed in the base oil to improve the anti-wear and friction-reducing properties of the lubricating oil.
[0064] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.
Claims
1. A wear-resistant, corrosion-resistant and high-temperature resistant bearing lubricant, It is characterized in that The anti-wear, corrosion and high temperature resistant bearing lubricating oil comprises base oil, extreme pressure anti-wear agent, anti-corrosion additive and viscosity index improver. The extreme pressure anti-wear agent is prepared by connecting the anti-wear agent to the surface of mercapto sepiolite; the anti-wear agent is prepared by reacting fatty alcohol amine, boric acid and diethyl phosphite; The preparation method of the fatty alcohol amine is as follows: heating oleic acid to 50-60° C., adding diisopropanolamine in an amount of 1-1.5 times the mass of the oleic acid, heating to 130-180° C., reacting for 2-6 hours, and obtaining the fatty alcohol amine; The anti-corrosion additive is prepared by mixing naphthalene-containing polyaromatic amide and ether benzamide; the naphthalene-containing polyaromatic amide is prepared by reacting naphthalene dicarboxylic acid with 2,2-bis[4-(4-aminophenoxy)phenyl]propane; the ether benzamide is prepared by reacting polyperfluoromethyl ethyl ether carboxylic acid with aniline; The preparation method of the mercapto sepiolite is as follows: sepiolite powder, ethanol and deionized water are mixed in a mass ratio of 1:8-10:2, the pH value is adjusted to 3-4 with hydrochloric acid, ultrasonication is performed at 60-80 kHz for 50-80 minutes, (3-mercaptopropyl)trimethoxysilane is added in an amount of 0.5-0.6 times the mass of the sepiolite powder, the temperature is raised to 65-75° C., the reaction is stirred at 100-300 rpm for 10-14 hours, filtering and washing with anhydrous ethanol and deionized water for 2-4 times in sequence, and finally drying and grinding to obtain the mercapto sepiolite; The preparation method of the naphthalene-containing polyaromatic amide comprises the following steps: in a nitrogen atmosphere, 1,4-naphthalene dicarboxylic acid, 2,2-bis[4-(4-aminophenoxy)phenyl]propane and N-methylpyrrolidone are stirred and dissolved in a mass ratio of 2:3-3.4:30, and then lithium chloride 2-2.2 times the mass of 1,4-naphthalene dicarboxylic acid, triphenyl phosphite 4-5 times the mass of 1,4-naphthalene dicarboxylic acid and pyridine 5-6 times the mass of 1,4-naphthalene dicarboxylic acid are added, the temperature is raised to 108-110° C., reacted for 6-8 hours, transferred to methanol and soaked for 24-48 hours, boiled with deionized water and methanol respectively, filtered 3-5 times, and finally dried in a vacuum drying oven at 100-120° C. to obtain the naphthalene-containing polyaromatic amide; The preparation method of the ether benzamide is as follows: adding 4-8% phosphoric acid, which is 0.02-0.04 times the mass of the polyperfluoromethyl ethyl ether carboxylic acid, dropwise at a rate of 1-3 mL / min, heating to 60-80° C. for reaction for 3-4 hours, cooling to room temperature, adding aniline, which is 1-1.2 times the mass of the polyperfluoromethyl ethyl ether carboxylic acid, under a nitrogen atmosphere, heating to 75-85° C., reacting for 10-12 hours, and performing reduced pressure distillation to obtain the ether benzamide.
2. The anti-wear, corrosion and high temperature resistant bearing lubricant according to claim 1, It is characterized in that The base oil is selected from one or more of trimellitic acid esters and / or saturated polyol esters; the viscosity index improver is any one or more of Evonik VISCOPLEX 3-200, Evonik VISCOPLEX 3-201, and Evonik VISCOPLEX 3-220.
3. A method for preparing the anti-wear, corrosion and high temperature resistant bearing lubricating oil according to claim 1, It is characterized in that The specific steps include: (1) In a nitrogen atmosphere, boric acid, fatty alcohol amine and diethyl phosphite are mixed in a mass ratio of 1:1.2-1.5:1, the temperature is raised to 150-170°C, and the reaction is carried out for 8-12 hours to obtain an anti-wear agent; (2) Immerse the mercapto sepiolite in the anti-wear agent at 10~30mW / cm 2 Irradiate with 365nm ultraviolet light for 20-40min, remove and wash with anhydrous ethanol and deionized water 2-4 times in sequence, dry, and obtain an extreme pressure anti-wear agent; (3) N-methylpyrrolidone and naphthalene-containing polyaromatic amide are mixed in a mass ratio of 20-40:3, stirred evenly, and then 0.4-0.8 times the mass of ether benzamide of the naphthalene-containing polyaromatic amide is added, the temperature is raised to 80-90° C., stirred at 300-500 rpm for reaction for 3-6 hours, the temperature is raised to 220-240° C., and the temperature is kept for 16-18 hours to obtain an anti-corrosion additive; (4) Heat the base oil to 150-180°C, add the extreme pressure anti-wear agent, anti-corrosion additive and viscosity index improver under continuous stirring, stir evenly and remove the foam, continue stirring for 20-40 minutes, and obtain the anti-wear, corrosion and high temperature resistant bearing lubricant.
4. The method for preparing a wear-resistant, corrosion-resistant and high-temperature-resistant bearing lubricant according to claim 3, It is characterized in that In the above step (4), the mass ratio of base oil, extreme pressure anti-wear agent, anti-corrosion additive and viscosity index improver is 50-60:2-4:1-2:1.