A method for preparing a large-size high-temperature alloy long-neck flange pipe

Through the two extrusion process and stainless steel coating method, the problem of small processing temperature range of high-temperature alloy long-neck flange pipe at high temperature is solved, and the preparation of large-sized pipe fittings is realized, which reduces the construction cost of conveying pipelines and increases the Laying efficiency.

CN117181972BActive Publication Date: 2024-11-26XIAN WESTERN ENERGY MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311092379.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-08-29
Publication Date
2024-11-26
Estimated Expiration
2043-08-29

AI Technical Summary

Technical Problem

The existing high-temperature alloy long-neck flange pipe has a small processing temperature range at high temperatures, resulting in defects such as cracking, limiting the length of the pipe fittings, increasing the connection points of the conveying pipeline, improving construction costs and affecting laying efficiency.

Method used

Using two extrusion processes, first prepare step tube blanks in a small extrusion cylinder, and then perform upsetting treatment in a large extrusion cylinder. Stainless steel coating and heat treatment are used to ensure full utilization of extrusion pressure and increase deformation and structure. Uniformity.

Benefits of technology

The preparation of large-size high-temperature alloy long-neck flange pipe is realized, which reduces the connection points, reduces the construction cost of conveying pipes, improves the laying efficiency, and improves the mechanical properties of the flange.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117181972B_ABST
    Figure CN117181972B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for preparing a large-size high-temperature alloy long-neck flange pipe, comprising: 1) firstly coating a high-temperature alloy hollow ingot with stainless steel, then heating it and then extruding it once, and reserving a set length of residual pressure during the first extrusion to obtain a long-neck step pipe; 2) heating the long-neck step pipe, replacing a large-size extrusion cylinder and a special mold, and then performing a second extrusion upsetting treatment on the residual pressure reserved for the first extrusion to obtain a long-neck flange pipe; 3) sequentially heat treating and machining the long-neck flange pipe to obtain a target product; and simultaneously controlling parameters such as temperature, extrusion speed, extrusion ratio, and extrusion pressure in each step. The present invention adopts a double hot extrusion process, and can prepare a large-size high-temperature alloy long-neck flange pipe with a smaller extrusion force of existing equipment, and significantly increases the deformation of the flange, and improves the structural uniformity and mechanical properties of the flange.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of high-temperature alloy pipe processing, and in particular relates to a method for preparing a large-size high-temperature alloy long-neck flange pipe. Background Art

[0002] High-temperature alloy, also known as heat-resistant alloy or superalloy, refers to an alloy material with iron, nickel and cobalt as the base materials. It can show good anti-oxidation, anti-corrosion and anti-creep properties under high temperature conditions of 600℃~1200℃, and has good fatigue performance. At the same time, it can work for a long time under certain stress load conditions.

[0003] Long-neck flange pipe refers to a flange with a long tube at one end, which can be regarded as a combination of flange and pipe fittings, such as Figure 1 As shown, the long-neck flange pipe made of high-temperature alloy is mainly used in high-temperature and high-pressure environments, such as pipeline connections in nuclear power, chemical, petroleum, natural gas and other industries. Due to its harsh service conditions, in order to avoid stress corrosion or creep failure caused by stress concentration, it is usually formed in one piece by forging or ring rolling. However, since the processing temperature range of high-temperature alloys at high temperatures is small, cracking and other defects may occur after the temperature is lowered. Therefore, the length of flange pipe fittings prepared by forging or ring rolling is limited. Usually, the length of the pipe fittings is less than 1000mm. After use, it will cause too many connection points in the entire transmission pipeline (in actual connection, flanges can be set at both ends, Figure 1 Only for example), if high temperature and high pressure media are to be transported, special treatment must be done on each connection. Therefore, a relatively short flange pipe will not only greatly increase the construction cost of the pipeline, but also affect the laying efficiency of the pipeline.

[0004] In view of this, the inventor proposes a method for preparing a large-size high-temperature alloy long-neck flange pipe to overcome the defects of the prior art. Summary of the invention

[0005] The purpose of the present invention is to overcome the shortcomings of the above-mentioned prior art and to propose a method for preparing a large-sized high-temperature alloy long-neck flange pipe. The preparation method can achieve the goal of preparing a large-sized high-temperature alloy long-neck flange pipe through two extrusion processes and using a smaller extrusion force of existing equipment.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] The present invention provides a method for preparing a large-size high-temperature alloy long-neck flange pipe, the preparation method comprising the following steps:

[0008] Step 1: First, a high-temperature alloy hollow ingot is coated with stainless steel, and then the coated high-temperature alloy hollow ingot is heated and then loaded into an extrusion die for a first extrusion process, and a set length of excess pressure is reserved during the first extrusion process to obtain a long-necked step tube billet;

[0009] Step 2: heat the long-neck step tube blank obtained in step 1, replace the large-size extrusion cylinder and extrusion die, and then perform secondary extrusion upsetting treatment on the remaining pressure part reserved for the first extrusion to obtain the long-neck flange tube blank;

[0010] Step 3, heat treating the long neck flange tube blank obtained in step 2;

[0011] Step 4: machining the long-neck flange tube blank after the heat treatment in step 3 to obtain a high-temperature alloy long-neck flange tube of a target size.

[0012] Furthermore, in the step 1, the thickness of the stainless steel coating the high-temperature alloy hollow ingot is 2 mm to 5 mm, and the stainless steel completely coats the inner and outer surfaces and end faces of the high-temperature alloy hollow ingot during coating.

[0013] Furthermore, in the step 1, when the coated high-temperature alloy hollow ingot is heated, the heating method used is induction heating or resistance furnace heating;

[0014] When induction heating is used, the heating temperature is set to 1000℃~1200℃ and the holding time is 2min~5min;

[0015] When using a resistance furnace for heating, set a heat preservation platform at 700℃~900℃, and then raise the temperature to 1000℃~1200℃, with a heat preservation time of 1h~3h.

[0016] Furthermore, in the step 1, during the primary extrusion treatment of the high-temperature alloy hollow ingot, glass powder is used as a lubricant, and a steel pad with a temperature of more than 900° C. is placed at the tail of the high-temperature alloy hollow ingot to reduce the temperature drop of the high-temperature alloy hollow ingot.

[0017] Furthermore, in the step 1, when the high-temperature alloy hollow ingot is subjected to a single extrusion process, the extrusion parameters set are as follows: the extrusion ratio is 3 to 10, the extrusion speed is 50 mm / s to 150 mm / s, and the length of the remaining extrusion portion reserved during extrusion is 50 mm to 200 mm.

[0018] Furthermore, in the step 2, when the long-necked step tube blank is heated, the entire long-necked step tube is heated or only the reserved residual portion is heated, and the heating temperature is less than or equal to the heating temperature in the step 1.

[0019] Furthermore, the inner diameter of the extrusion cylinder used in the step 2 is 5mm to 20mm larger than the target flange diameter, the length of the extrusion excess portion should be 5mm to 10mm larger than the target flange thickness, and the secondary extrusion upsetting ratio is controlled to 2 to 4, and the extrusion speed is set to 5mm / s to 30mm / s.

[0020] Furthermore, the heat treatment method in step three is annealing + aging, the specific annealing temperature is 700° C. to 900° C., and the heat preservation time is 2h to 3h.

[0021] Furthermore, in the step 4, the single-side removal allowance of the long-neck flange tube blank during machining is 2 mm to 10 mm.

[0022] Furthermore, the preparation method is used to prepare high-temperature alloy long-neck flange pipes with flange diameters ranging from 195 mm to 780 mm, pipe diameters ranging from 56 mm to 290 mm, and pipe lengths ranging from 1000 mm to 3000 mm.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] 1. The preparation method provided by the present invention uses an extruder to first prepare a step tube blank in a smaller extrusion barrel, and then replaces the large extrusion barrel for upsetting to complete the preparation of the flange, making full use of the small extrusion force in the extrusion filling (upsetting) stage, and realizing the preparation of large-size high-temperature alloy long-neck flange pipes on conventional extrusion equipment. This is because the high-temperature alloy has extremely high strength during hot extrusion, and is limited by the extrusion force, and it is impossible to directly prepare a large extrusion ratio pipe. For example, when the flange diameter is 300mm, the pipe diameter is 100mm, and the wall thickness is 10mm, if the direct extrusion method is used, an extrusion barrel with an inner diameter greater than 300mm is required, the extrusion ratio is greater than 23, and the theoretical extrusion force is about 50MN; limited by the allowable stress of the extrusion shaft, the extrusion force configured with an extrusion barrel with an inner diameter of 300mm is usually 40MN (i.e. less than 50MN), so the extrusion force is not enough to deform the high-temperature alloy. The present invention first obtains a long-necked stepped tube blank by the first extrusion, and then performs extrusion upsetting on the flange side by the second extrusion, which significantly increases the deformation of the flange and improves the structural uniformity and mechanical properties of the flange.

[0025] 2. The preparation method provided by the present invention firstly coats the inner and outer surfaces and the ends of the high-temperature alloy tube blank with a stainless steel layer, so that when the high-temperature alloy tube blank is heated and extruded once, the stainless steel can be used to have good ductility and lubricity at high temperature to isolate the high-temperature alloy from the extrusion die, thereby ensuring the surface quality of the long-necked step tube blank after extrusion; then the long-necked step tube blank is heated, and after replacing the large-size extrusion cylinder and the extrusion die, the reserved pressure surplus part of the first extrusion is subjected to secondary extrusion upsetting treatment to obtain the long-necked flange tube blank; finally, the long-necked flange tube blank is heat-treated and machined in sequence to obtain the target product. Compared with the prior art, the preparation method of the present invention can obtain a high-temperature alloy long-necked flange pipe with a flange diameter of 195mm to 780mm, a pipe diameter of 56mm to 290mm, and a pipe length of 1000mm to 3000mm, thereby reducing the connection points when constructing a high-temperature and high-pressure transmission pipeline, thereby reducing the construction cost of the transmission pipeline and improving the laying efficiency of the transmission pipeline. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] The accompanying drawings are incorporated in and constitute a part of this specification and, together with the description, serve to explain the principles of the present invention.

[0027] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.

[0028] Figure 1 This is a schematic diagram of the long neck flange pipe structure;

[0029] Figure 2 is a flow chart of the preparation method of the present invention;

[0030] Figure 3 This is a schematic diagram of the structure of the preparation method of the present invention before the first extrusion;

[0031] Figure 4 This is a schematic diagram of the structure of the preparation method of the present invention after one extrusion;

[0032] Figure 5 It is a schematic diagram of the preparation method of the present invention before secondary extrusion upsetting;

[0033] Figure 6 This is a schematic diagram of the preparation method of the present invention after secondary extrusion upsetting.

[0034] Among them: 1 is the extrusion shaft; 2 is the extrusion cylinder; 3 is the extrusion pad; 4 is the steel pad; 5 is the high-temperature alloy tube blank; 6 is the extrusion die; 7 is the die pad; 8 is the extrusion needle; 9 is the die sleeve. DETAILED DESCRIPTION

[0035] Here, exemplary embodiments will be described in detail, and the embodiments described in the following exemplary embodiments do not represent all embodiments consistent with the present invention. Instead, they are only examples of devices consistent with some aspects of the present invention as detailed in the appended claims.

[0036] See also Figures 2 to 6 The present invention provides a method for preparing a large-size high-temperature alloy long-neck flange pipe, the preparation method comprising the following steps:

[0037] Step 1: First, a high-temperature alloy hollow ingot is coated with stainless steel, and then the coated high-temperature alloy hollow ingot is heated and then loaded into an extrusion die for a first extrusion process, and a set length of excess pressure is reserved during the first extrusion process to obtain a long-necked step tube billet;

[0038] Specifically, firstly, the inner and outer surfaces and the end surface of the high-temperature alloy hollow ingot are completely covered with stainless steel with a thickness of 2 mm to 5 mm.

[0039] Then the coated high-temperature alloy hollow ingot is heated by induction heating or resistance furnace heating. When induction heating is adopted, the heating temperature is set at 1000℃~1200℃, and the holding time is 2min~5min; when resistance furnace heating is adopted, a holding platform is set at 700℃~900℃, and then the temperature is raised to 1000℃~1200℃, and the holding time is 1h~3h.

[0040] Finally, the heated and stainless steel coated high temperature alloy hollow ingot is loaded into the extrusion die. Figure 2 As shown, glass powder is used as a lubricant, and a steel pad with a temperature of more than 900°C is placed at the tail of the high-temperature alloy hollow ingot; then the high-temperature alloy hollow ingot is subjected to a first extrusion process, and the extrusion parameters set during the first extrusion process are as follows: the extrusion ratio is 3 to 10, the extrusion speed is 50 mm / s to 150 mm / s, and the length of the remaining pressure portion reserved during extrusion is 50 mm to 200 mm. Figure 4 shown.

[0041] The present invention places a high-temperature steel pad at the tail of the hollow ingot to reduce the temperature drop of the high-temperature alloy. This is because the high-temperature alloy has high strength at high temperatures. Using a smaller extrusion ratio is beneficial to reducing the resistance to extrusion deformation, while reducing the risk of product cracking or surface grooves. A 50mm to 200mm long hollow ingot is reserved without extrusion, and a step-type tube billet can be prepared, that is, a long-necked step tube billet is obtained.

[0042] Step 2: heat the long-neck step tube blank obtained in step 1, replace the large-size extrusion cylinder and extrusion die, and then perform secondary extrusion upsetting treatment on the remaining pressure part reserved for the first extrusion to obtain the long-neck flange tube blank;

[0043] Specifically, in this step, only the reserved residual portion can be heated, or the entire long-necked step tube billet can be heated, and the heating temperature is less than or equal to the heating temperature in step 1. This is because appropriately lowering the heating temperature is conducive to reducing compound precipitation and avoiding abnormal grain growth. After heating, the long-necked step tube billet is placed in a special mold, such as Figure 5 As shown, after secondary extrusion and upsetting, Figure 6 As shown, a long-neck flange tube blank is obtained.

[0044] Among them, the inner diameter of the extrusion barrel replaced during the secondary extrusion upsetting process should be 5mm to 20mm larger than the target flange diameter, and the length of the extrusion surplus should be 5mm to 10mm larger than the target flange thickness. At the same time, the secondary extrusion upsetting ratio is controlled to be 2 to 4, and the extrusion speed is set to 5mm / s to 30mm / s. The above-set inner diameter of the extrusion barrel and the extrusion surplus setting values ​​can ensure that qualified flanges can be processed, and the utilization rate of high-temperature alloy materials can be improved; at the same time, a reasonable extrusion ratio can be set to fully deform the flange part, while avoiding obvious defects during upsetting; and the extrusion speed is slow extrusion, which is convenient for accurate control of the extrusion surplus thickness.

[0045] Step 3, heat treating the long neck flange tube blank obtained in step 2;

[0046] The specific heat treatment method is annealing + aging. The specific process is determined according to the material and purpose of the product. Generally, the annealing temperature is set at 700℃~900℃ and kept warm for 2h~3h.

[0047] Step 4: machining the long-neck flange tube blank after the heat treatment in step 3 to obtain a high-temperature alloy long-neck flange tube of a target size. Specifically, during machining, the single-side removal allowance of the long-neck flange tube blank is 2 mm to 10 mm.

[0048] In order to further illustrate the effect of the preparation method of the present invention, the inventors carried out the following specific examples:

[0049] Example 1 (Specifications of preparing long-neck flange pipes: pipe fittings of Ø56×6×1000 mm and flanges of Ø195×30 mm)

[0050] The preparation method of this embodiment comprises the following steps:

[0051] 1) The high-temperature alloy material is GH4720. First, 304 stainless steel with a thickness of 3 mm is used to cover the entire high-temperature alloy hollow ingot. The specification of the high-temperature alloy hollow ingot after covering is Ф外 117×Ф 内 43×320mm; the coated high-temperature alloy billet is heated in a resistance furnace to 700℃ and kept in the furnace for 1h, and then heated to 1150℃ and kept in temperature for 1.5-2.5h; after the insulation, it is quickly transferred to the extruder for the first extrusion. Glass powder is used as a lubricant during extrusion, and a steel pad with a temperature of 950℃ is placed at the tail of the high-temperature alloy hollow ingot. The inner diameter of the extrusion barrel is 120mm, the extrusion ratio is 6, the extrusion speed is 50mm / s, and the extrusion residual length is set to 120mm, that is, the hollow ingot with a reserved length of 120mm is not extruded. The measured peak extrusion force is 14MN. After the first extrusion, a long-necked step billet is obtained. The specification of the pipe fittings in the long-necked step billet is Ф60×10×1000mm.

[0052] 2) During the secondary extrusion upsetting, the long-necked step tube blank obtained in step 1) is heated to 1130°C by a resistance heating furnace and kept warm for 1h to 1.5h; and the extrusion cylinder with an inner diameter of 200mm and the corresponding extrusion die are replaced, and a steel pad with a temperature of 950°C is placed at the tail of the long-necked step tube blank, the residual thickness is set to 40mm, the extrusion upsetting ratio is 3, the extrusion speed is set to 5mm / s, the measured upsetting force is 9MN, and the long-necked flange tube blank is obtained after extrusion upsetting.

[0053] 3) The long-neck flange tube blank obtained in step 2) is annealed at 700°C for 2 hours; after annealing, it is cooled to room temperature and machined, and the inner and outer surfaces are removed 2 mm on one side to obtain a finished product of Ф56×6×1000mm pipe fitting + Ф195×30mm flange.

[0054] Example 2 (Specifications of preparing long-neck flange pipes: pipe fittings of Ф176×16×2000 mm and flanges of Ф340×30 mm)

[0055] The preparation method of this embodiment comprises the following steps:

[0056] 1) The high-temperature alloy material is GH4169. First, 2mm thick 304 stainless steel is used to cover the entire high-temperature alloy hollow ingot. The specification of the high-temperature alloy hollow ingot after coating is Ф 外 252×Ф 内143×740mm; the coated high-temperature alloy billet is heated by induction, heated to 1100℃, and then kept warm for 5 minutes; after the insulation is completed, it is quickly transferred to the extruder for the first extrusion. Glass powder is used as a lubricant during extrusion, and a steel pad with a temperature of 950℃ is placed at the tail of the high-temperature alloy hollow ingot. The inner diameter of the extrusion barrel is 260mm, the extrusion ratio is 3.6, the extrusion speed is 100mm / s, and the extrusion residual setting length is 90mm, that is, the hollow ingot with a reserved length of 90mm is not extruded. The measured peak extrusion force is 42MN. After the first extrusion, a long-necked step billet is obtained. The specification of the pipe fittings in the long-necked step billet is Ф180×20×2000mm.

[0057] 2) During the secondary extrusion upsetting, the long-necked step tube blank obtained in step 1) is heated to 1100°C by induction heating and kept warm for 5 minutes; and the extrusion cylinder with an inner diameter of 350 mm and the corresponding extrusion die are replaced, and a steel pad with a temperature of 950°C is placed at the tail of the long-necked step tube blank, the residual thickness is set to 40 mm, the extrusion upsetting ratio is 2.2, the extrusion speed is set to 10 mm / s, the measured upsetting force is 23 MN, and the long-necked flange tube blank is obtained after extrusion upsetting.

[0058] 3) The long-neck flange tube blank obtained in step 2) is annealed at 800°C for 2.5 hours; after annealing, it is cooled to room temperature and machined, with a single-side removal of 2 mm on the inner and outer surfaces to obtain a finished product of Ф176×16×1000mm pipe fitting + Ф340×30mm flange.

[0059] Example 3 (Specifications of preparing long-neck flange pipes: pipe fittings of 290 × 20 × 1000 mm and flanges of 780 × 30 mm)

[0060] The preparation method of this embodiment comprises the following steps:

[0061] 1) The high-temperature alloy material is N06690. First, 3mm thick 304 stainless steel is used to cover the entire high-temperature alloy hollow ingot. The specification of the high-temperature alloy hollow ingot after coating is Ф 外 440×Ф 内243×920mm; the coated high-temperature alloy hollow ingot is heated in a resistance furnace to 800℃ and kept in the furnace for 2h, and then heated to 1200℃ for 3.0-5.0h; after the insulation, it is quickly transferred to the extruder for the first extrusion. Glass powder is used as a lubricant during extrusion, and a steel pad with a temperature of 950℃ is placed at the tail of the high-temperature alloy tube. The inner diameter of the extrusion barrel is 450mm, the extrusion ratio is 4.4, the extrusion speed is 150mm / s, and the extrusion pressure setting length is 160mm, that is, the hollow ingot with a reserved length of 160mm is not extruded. The measured peak extrusion force is 60MN. After the first extrusion, a long-necked step tube is obtained. The specification of the pipe fittings in the long-necked step tube is Ф300×30×3000mm.

[0062] 2) During the secondary extrusion upsetting, the long-necked step tube blank obtained in step 1) is heated to 1160°C in a resistance heating furnace and kept warm for 2h to 3h; and the extrusion cylinder with an inner diameter of 800mm and the corresponding extrusion die are replaced, and a steel pad with a temperature of 950°C is placed at the tail of the long-necked step tube blank, the residual thickness is set to 40mm, the extrusion upsetting ratio is 4, the extrusion speed is set to 30mm / s, the measured upsetting force is 35MN, and the long-necked flange tube blank is obtained after extrusion upsetting.

[0063] 3) The long-neck flange tube blank obtained in step 2) is annealed at 900°C for 3 hours; after annealing, it is cooled to room temperature and machined, and the inner and outer surfaces are removed by 5 mm on one side to obtain a finished product of Ф290×20×3000mm pipe fitting + Ф780×30mm flange.

[0064] Tables 1 and 2 below are comparisons of the parameters of the primary extrusion and secondary extrusion upsetting processes in Examples 1 to 3:

[0065] Table 1 Comparison of primary extrusion process parameters

[0066]

[0067] Table 2 Comparison of secondary extrusion upsetting process parameters

[0068]

[0069] The above description is only a specific embodiment of the present invention, so that those skilled in the art can understand or implement the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present invention.

[0070] It should be understood that the present invention is not limited to what has been described above and that various modifications and changes may be made without departing from its scope. The scope of the present invention is limited only by the appended claims.

Claims

1. A method for preparing a large-size high-temperature alloy long-neck flange pipe, characterized in that: The preparation method comprises the following steps: Step 1: First, a high-temperature alloy hollow ingot is coated with stainless steel, and then the coated high-temperature alloy hollow ingot is heated and then loaded into an extrusion die for a first extrusion process, and a set length of excess pressure is reserved during the first extrusion process to obtain a long-necked step tube billet; Step 2: heat the long-neck step tube blank obtained in step 1, replace the large-size extrusion cylinder and extrusion die, and then perform secondary extrusion upsetting treatment on the remaining pressure part reserved for the first extrusion to obtain the long-neck flange tube blank; Step 3, heat treating the long neck flange tube blank obtained in step 2; Step 4: machining the long-neck flange tube blank after the heat treatment in step 3 to obtain a high-temperature alloy long-neck flange tube of a target size; Wherein, the thickness of the stainless steel coating the high-temperature alloy hollow ingot in the step 1 is 2 mm to 5 mm, and the stainless steel completely coats the inner and outer surfaces and end faces of the high-temperature alloy hollow ingot during coating; during the primary extrusion treatment of the coated high-temperature alloy hollow ingot: a steel pad with a temperature of more than 900° C. is placed at the tail of the high-temperature alloy hollow ingot, and the set extrusion parameters are as follows: the extrusion ratio is 3 to 10, the extrusion speed is 50 mm / s to 150 mm / s, and the length of the remaining pressing portion reserved during extrusion is 50 mm to 200 mm; The inner diameter of the extrusion cylinder used in the step 2 is 5mm to 20mm larger than the target flange diameter, the length of the extrusion excess portion should be 5mm to 10mm larger than the target flange thickness, and the secondary extrusion upsetting ratio is controlled to be 2 to 4, and the extrusion speed is set to 5mm / s to 30mm / s.

2. The method for preparing a large-size high-temperature alloy long-neck flange pipe according to claim 1, characterized in that: In the step 1, when the coated high-temperature alloy hollow ingot is heated, the heating method used is induction heating or resistance furnace heating; When induction heating is used, the heating temperature is set to 1000℃~1200℃ and the holding time is 2min~5min; When using a resistance furnace for heating, set a heat preservation platform at 700℃~900℃, and then raise the temperature to 1000℃~1200℃, with a heat preservation time of 1h~5h.

3. The method for preparing a large-size high-temperature alloy long-neck flange pipe according to claim 1, characterized in that: In the step 1, glass powder is used as a lubricant during the primary extrusion process of the high-temperature alloy hollow ingot.

4. The method for preparing a large-size high-temperature alloy long-neck flange pipe according to claim 1, characterized in that: In the step 2, when the long-necked step tube blank is heated, the entire long-necked step tube is heated or only the reserved residual portion is heated, and the heating temperature is less than or equal to the heating temperature in the step 1.

5. The method for preparing a large-size high-temperature alloy long-neck flange pipe according to claim 1, characterized in that: The heat treatment method in step three is annealing + aging, the specific annealing temperature is 700° C. to 900° C., and the heat preservation is 2h to 3h.

6. The method for preparing a large-size high-temperature alloy long-neck flange pipe according to claim 1, characterized in that: During machining in step 4, the single-side removal allowance of the long-neck flange tube blank is 2 mm to 10 mm.

7. The method for preparing a large-size high-temperature alloy long-neck flange pipe according to any one of claims 1 to 6, characterized in that: The preparation method is used for preparing high-temperature alloy long-neck flange pipes with flange diameters ranging from 195 mm to 780 mm, pipe diameters ranging from 56 mm to 290 mm, and pipe lengths ranging from 1000 mm to 3000 mm.