A flame retardant diaphragm material for lithium battery and preparation method thereof
By coating the lithium-ion battery separator with a flame-retardant coating containing zeolite-based reinforcing agents and POSS-based cross-linking agents, the problems of separator flame retardancy and low liquid absorption rate are solved, and high thermal stability and excellent flame retardant properties are achieved. .
Patent Information
- Application Number
- CN202311366258.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-20
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-10-20
AI Technical Summary
The existing lithium-ion battery separators have poor flame retardancy, which leads to safety hazards under high-power charging and discharging. At the same time, due to the high crystallinity and weak polarity of polyvinylidene fluoride, the electrolyte solution has poor swelling properties, resulting in low liquid absorption rate and affecting ions. Conductivity.
A flame-retardant coating is coated on a polyolefin-based film. Self-made zeolite-based reinforcing agent and POSS-based cross-linking agent are introduced into the coating. The amino-terminated nitrogen-phosphorus POSS polymer is formed through the Michael addition reaction and the elimination reaction of chlorine and amino groups to form The flame retardant coating with high thermal stability and porous structure improves the liquid absorption rate and flame retardancy of the separator.
It significantly improves the thermal stability, flame retardancy and liquid absorption rate of the lithium battery separator, enhances the affinity between the electrolyte and the separator, reduces the shrinkage of the separator and the volatilization of small molecules produced by combustion, and improves the flame retardant performance.
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium batteries, and in particular relates to a flame retardant diaphragm material for lithium batteries and a preparation method thereof. Background Art
[0002] Lithium-ion batteries are widely used in various portable devices, electric vehicles and energy storage systems because of their high energy density, high power, low self-discharge rate and long life. Lithium-ion batteries are mainly composed of four parts: positive electrode material, negative electrode material, electrolyte solution and diaphragm. In the battery system, the main function of the diaphragm is to separate the positive and negative electrodes of the battery to prevent the two electrodes from directly contacting and short-circuiting. The diaphragm is an electronically insulating polymer functional material with a large number of tortuous micropores. The ions in the electrolyte can pass freely through the micropores and migrate between the positive and negative electrodes to form a circuit, while the electrons form an electric current through the external circuit, improving the utilization of electrical equipment. The performance of the diaphragm determines the interface structure, liquid retention and internal resistance of the battery, which in turn affects the battery capacity, battery charge and discharge rate, cycle life and safety performance.
[0003] At present, polyolefin microporous membranes prepared by dry and wet processes are widely popular, such as polyethylene (PE) membranes, polypropylene (PP) membranes, etc., which have good mechanical properties and excellent chemical stability and have become the main membranes for lithium-ion batteries. However, polyolefin microporous membranes have poor flame retardancy and pose safety hazards when electric vehicles face high-power charging and discharging requirements. In this regard, Chinese patent CN116231228B discloses a flame-retardant lithium battery coated membrane and a preparation method and application thereof, including a base membrane and a coating layer coated on at least one side of the base membrane, wherein the coating layer has composite flame-retardant particles and vinylidene fluoride polymers, and the composite flame-retardant particles include porous dioxygen as an outer shell. Although the barrier film finally obtained has excellent temperature resistance and flame retardancy, polyvinylidene fluoride is a polymer with high crystallinity and weak polarity, so that the electrolyte solution can swell into the polymer matrix very little, and the microporous structure of the introduced composite flame retardant particles is blocked, which further hinders the close contact between the electrolyte and the barrier film, and hinders the shuttle of ions in the electrolyte in the barrier film, resulting in the barrier film finally having a liquid absorption rate of only 18.9-25.5%, which is not conducive to the improvement of ion conductivity. Therefore, it is necessary to provide a lithium battery flame retardant diaphragm material with high liquid absorption rate. Summary of the invention
[0004] One of the purposes of the present invention is to provide a flame retardant diaphragm material for a lithium battery, wherein the diaphragm not only has excellent temperature resistance and flame retardancy, but also has a high liquid absorption rate.
[0005] A second object of the present invention is to provide a method for preparing the flame-retardant lithium battery coating barrier film.
[0006] The purpose of the present invention can be achieved through the following technical solutions:
[0007] A flame retardant diaphragm material for a lithium battery comprises a base film and a flame retardant coating arranged on one side or both sides of the base film.
[0008] Furthermore, the base film is one of a single-layer polypropylene porous film, a single-layer polyethylene porous film, a multi-layer polyethylene microporous film, and a polypropylene-polyethylene multi-layer composite film.
[0009] Furthermore, the flame retardant coating is obtained by drying and curing the flame retardant paint.
[0010] A method for preparing a flame retardant diaphragm material for a lithium battery comprises the following steps:
[0011] (1) adding a polyvinylidene fluoride polymer, a zeolite-based reinforcing agent, a POSS-based crosslinking agent and deionized water into a stirrer, stirring at a speed of 500-1000 r / min for 0.5-1 h, adding an initiator and stirring for 0.5 h, then adding a wetting agent, and continuing to stir for 0.5-1 h to obtain a flame retardant coating;
[0012] (2) The flame retardant coating is uniformly coated on one side or both sides of the base film, with a single-side coating thickness of 1-3 μm, and the base film is placed in a 50-60° C. environment to dry for 6-8 hours, and rolled up to obtain a lithium battery flame retardant diaphragm material.
[0013] Furthermore, the flame retardant coating comprises the following raw materials in parts by weight:
[0014] 18-23 parts of polyvinylidene fluoride polymer, 20-25 parts of zeolite-based reinforcing agent, 3-5 parts of POSS-based crosslinking agent, 0.2-0.6 parts of initiator, 0.5-1 parts of wetting agent and 55-65 parts of deionized water.
[0015] Further, the zeolite-based reinforcing agent is obtained by the following steps:
[0016] Pentaerythritol triallyl ether and 3-aminopropyltriethoxysilane are added to anhydrous tetrahydrofuran, reacted at 50°C for 12 hours under closed conditions, and the anhydrous tetrahydrofuran is removed under reduced pressure to obtain an intermediate product. The intermediate product and nano zeolite are placed in a solution consisting of tetrahydrofuran and deionized water, ultrasonicated for 30 minutes, and reacted at 50°C for 12 hours. After the reaction, the tetrahydrofuran is centrifuged and washed three times, and vacuum dried at 50°C for 24 hours to obtain a zeolite-based enhancer.
[0017] The mass ratio of pentaerythritol triallyl ether to 3-aminopropyltriethoxysilane is 7.7-8.0:6.6, and the dosage ratio of the intermediate product, nano zeolite, tetrahydrofuran and deionized water is 2g:1-2g:60-80mL:5-10mL.
[0018] Zeolite is a framework structure composed of silicon-oxygen tetrahedrons and aluminum-oxygen tetrahedrons, which is loose and porous, relatively low in price, and has high chemical stability and thermal stability. The present invention first uses pentaerythritol triallyl ether and 3-aminopropyltriethoxysilane as raw materials, and obtains a terminal vinyl hyperbranched polymer (the molecular structure also contains numerous hydrophilic hydroxyl groups, hydrophilic ether bonds, and a siloxane structure), i.e., the above-mentioned intermediate product, by Michael addition reaction. The intermediate product is then grafted onto zeolite by coupling reaction to obtain a zeolite-based reinforcing agent, which is introduced into the coating layer to significantly improve the heat resistance and liquid absorption rate of the barrier film.
[0019] Further, the POSS-based cross-linking agent is obtained by the following steps:
[0020] S1, hexachlorocyclotriphosphazene and octa-p-aminophenyl-POSS were mixed and ground, and then transferred to a hydrothermal reactor, reacted at 160° C. for 12 h, and then cooled to room temperature, centrifuged the product, and washed alternately with anhydrous methanol and deionized water. The centrifuged product was placed in an oven at 120° C. and dried to constant weight to obtain an amino-terminated nitrogen-phosphorus POSS polymer;
[0021] S2. Add acrylic acid, EDC·HCl and NHS to dimethyl sulfoxide, stir for 0.5 h, add amino-terminated nitrogen and phosphorus POSS polymer, stir and react for 24 h. After the reaction is completed, pour the reaction product into acetone for precipitation, wash it with acetone for 3 times, filter it, and vacuum dry it at 60°C to constant weight to obtain a POSS-based cross-linking agent.
[0022] Polyhedral oligomeric silsesquioxane (POSS) is an organic / inorganic nano hybrid molecule with a special structure. The main molecular skeleton is composed of Si-O-Si bonds in a three-dimensional structure. It has good flame retardancy and heat resistance and a multi-faceted microporous structure. However, the flame retardant effect of the polyhedral oligomeric silsesquioxane alone as a flame retardant is relatively low. Therefore, the present invention uses hexachlorocyclotriphosphazene and octa-p-aminophenyl-POSS as raw materials, obtains an amino-terminated nitrogen-phosphorus POSS polymer through an elimination reaction between chlorine and amino groups, and then, under the catalysis of EDC·HCl and NHS, the amino group of the amino-terminated nitrogen-phosphorus POSS polymer is subjected to an amide reaction with the carboxyl group of acrylic acid to obtain the above-mentioned POSS-based crosslinking agent.
[0023] Furthermore, the mass ratio of hexachlorocyclotriphosphazene to octa-p-aminophenyl-POSS in S1 is 0.7:2.6-3.0.
[0024] Furthermore, the usage ratio of acrylic acid, EDC·HCl, NHS, dimethyl sulfoxide and amino-terminated nitrogen-phosphorus POSS polymer in S2 is 0.4-0.6 g: 0.96 g: 0.56 g: 200 mL: 4.4-5.2 g.
[0025] Furthermore, the initiator is one or both of dicumyl peroxide and benzoyl peroxide.
[0026] Furthermore, the wetting agent is one or more of sodium dodecyl sulfonate, sodium dodecyl sulfate and polyoxyethylene alkylphenol ether.
[0027] Further, the polyvinylidene fluoride polymer is one or more of polyvinylidene fluoride, a vinylidene fluoride-tetrafluoroethylene copolymer and a vinylidene fluoride-hexafluoroacrylic acid copolymer.
[0028] Beneficial effects of the present invention:
[0029] 1. The present invention provides a flame-retardant diaphragm material for a lithium battery and a preparation method thereof. A flame-retardant coating is formed by coating a flame-retardant coating on a polyolefin base film, thereby improving the thermal stability and flame retardancy of the barrier film and giving it a good liquid absorption rate.
[0030] 2. The present invention introduces a self-made zeolite-based reinforcing agent into the flame-retardant coating, which is a nano-scale zeolite modified by a terminal vinyl hyperbranched polymer. Based on the low viscosity characteristics of the hyperbranched polymer, it has good dispersibility in the coating, so that zeolite particles with continuously distributed well-developed pores are obtained in the flame-retardant coating. Combined with the nano-scale voids inside the hyperbranched polymer, the introduced porous structure is beneficial to improving the storage capacity of the barrier film for the electrolyte, and improving the liquid absorption and liquid retention of the barrier film. Since the molecular structure of the hyperbranched polymer also contains many hydrophilic hydroxyl groups and hydrophilic ether bonds, the polarity of the flame-retardant coating is enhanced, thereby improving the affinity between the base film and the electrolyte, which is beneficial for the electrolyte to wetting and swelling the barrier, and further improving the liquid absorption rate of the electrolyte. In addition, the terminal vinyl of the hyperbranched polymer It can also undergo polymerization reaction with cross-linking agents and polyvinylidene fluoride polymers to improve the stability of zeolite in the coating and reduce the degree of zeolite loss over time. In addition, based on the high thermal stability of zeolite and silicon-oxygen-silicon bonds, the skeleton of the flame-retardant coating will not shrink at high temperatures. When the barrier film shrinks due to heat, it can hinder the shrinkage of the barrier film and reduce the degree of shrinkage. More importantly, during the combustion process, the porous structure in the zeolite can effectively adsorb small molecular weight substances produced by combustion, reduce the volatilization of these substances and promote carbonization. The free water and crystal water in the zeolite will gradually evaporate, absorb heat, and reduce the surface temperature of the material. The silicon-oxygen-silicon bonds decompose under heat to produce a Si-OC insulating layer, which increases the density and strength of the residual carbon layer and the carbon layer, and effectively improves the flame retardancy of the barrier film.
[0031] 3. The present invention introduces a homemade POSS-based cross-linking agent into the flame-retardant coating, which can react with the polyvinylidene fluoride polymer to form an interpenetrating network structure. Nitrogen, phosphorus, and silicon flame-retardant elements are introduced into the flame-retardant coating to further improve the flame retardancy of the barrier film. The microporous structure in the POSS-based cross-linking agent further increases the porosity of the coating, giving the barrier film excellent flame retardancy while improving its liquid absorption rate. DETAILED DESCRIPTION
[0032] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] Example 1
[0034] A zeolite-based reinforcing agent is obtained by the following steps:
[0035] 7.7 g of pentaerythritol triallyl ether and 6.6 g of 3-aminopropyltriethoxysilane were added to 150 mL of anhydrous tetrahydrofuran, and reacted at 50°C for 12 h under closed conditions. After removing the anhydrous tetrahydrofuran under reduced pressure, an intermediate product was obtained. 2 g of the intermediate product and 1 g of nano zeolite were placed in a solution consisting of 60 mL of tetrahydrofuran and 5 mL of deionized water, and the mixture was ultrasonicated for 30 min and reacted at 50°C for 12 h. After the reaction, the mixture was centrifuged and washed three times with tetrahydrofuran, and vacuum dried at 50°C for 24 h to obtain a zeolite-based enhancer. The nano zeolite had a particle size of 300 nm and a pore size of 0.4 nm, and was purchased from Sinopharm Chemical Reagent Co., Ltd.
[0036] Example 2
[0037] A zeolite-based reinforcing agent is obtained by the following steps:
[0038] 8.0 g of pentaerythritol triallyl ether and 6.6 g of 3-aminopropyltriethoxysilane were added to 150 mL of anhydrous tetrahydrofuran, and reacted at 50°C for 12 h under closed conditions. After removing the anhydrous tetrahydrofuran under reduced pressure, an intermediate product was obtained. 2 g of the intermediate product and 2 g of nano zeolite were placed in a solution consisting of 80 mL of tetrahydrofuran and 10 mL of deionized water, and the mixture was ultrasonicated for 30 min and reacted at 50°C for 12 h. After the reaction, the mixture was centrifuged and washed three times with tetrahydrofuran, and vacuum dried at 50°C for 24 h to obtain a zeolite-based enhancer. The nano zeolite had a particle size of 300 nm and a pore size of 0.4 nm, and was purchased from Sinopharm Chemical Reagent Co., Ltd.
[0039] Comparative Example 1
[0040] A zeolite-based reinforcing agent is prepared on the substrate of Example 1, wherein the pentaerythritol triallyl ether in Example 1 is replaced with 30 mmol of trimethylolpropane triacrylate.
[0041] Example 3
[0042] A POSS-based cross-linking agent is obtained by the following steps:
[0043] S1, 0.7g hexachlorocyclotriphosphazene and 2.6g octa-p-aminophenyl-POSS (purchased from Shanghai Hanhong Technology Co., Ltd.) were mixed and ground, and then transferred to a hydrothermal reactor, reacted at 160°C for 12h, and then cooled to room temperature, the product was centrifuged, and washed alternately with anhydrous methanol and deionized water. The centrifuged product was placed in an oven at 120°C and dried to constant weight to obtain an amino-terminated nitrogen-phosphorus POSS polymer;
[0044] S2. Add 0.4 g acrylic acid, 0.96 g EDC·HCl and 0.56 g NHS into 200 mL dimethyl sulfoxide, stir for 0.5 h, add 4.4 g amino-terminated nitrogen-phosphorus POSS polymer, stir and react for 24 h. After the reaction, pour the reaction product into acetone for precipitation, wash with acetone for 3 times, filter, and vacuum dry at 60°C to constant weight to obtain a POSS-based cross-linking agent.
[0045] Example 4
[0046] A POSS-based cross-linking agent is obtained by the following steps:
[0047] S1, 0.7g hexachlorocyclotriphosphazene and 3.0g octa-p-aminophenyl-POSS (purchased from Shanghai Hanhong Technology Co., Ltd.) were mixed and ground, and then transferred to a hydrothermal reactor, reacted at 160°C for 12h, and then cooled to room temperature, the product was centrifuged, and washed alternately with anhydrous methanol and deionized water. The centrifuged product was placed in an oven at 120°C and dried to constant weight to obtain an amino-terminated nitrogen-phosphorus POSS polymer;
[0048] S2. Add 0.6 g acrylic acid, 0.96 g EDC·HCl and 0.56 g NHS into 200 mL dimethyl sulfoxide, stir for 0.5 h, add 5.2 g amino-terminated nitrogen-phosphorus POSS polymer, stir and react for 24 h. After the reaction, pour the reaction product into acetone for precipitation, wash with acetone for 3 times, filter, and vacuum dry at 60°C to constant weight to obtain a POSS-based cross-linking agent.
[0049] Example 5
[0050] A method for preparing a flame retardant diaphragm material for a lithium battery comprises the following steps:
[0051] (1) In parts by weight, 18 parts of polyvinylidene fluoride-hexafluoropropylene copolymer (molecular weight 500,000, purchased from Shanghai MacLean Biochemical Technology Co., Ltd.), 20 parts of the zeolite-based reinforcing agent of Example 1, 3 parts of the POSS-based crosslinking agent of Example 3 and 55 parts of deionized water were added to a stirrer, stirred at a speed of 500 r / min for 1 h, 0.2 parts of initiator were added, stirred for 0.5 h, and then 0.5 parts of wetting agent were added, and stirring was continued for 0.5 h to obtain a flame retardant coating;
[0052] (2) The flame retardant coating is uniformly coated on both sides of the single-layer polypropylene porous membrane, with a single-side coating thickness of 1 μm. The membrane is placed in a 50° C. environment and dried for 8 h, and rolled up to obtain a lithium battery flame retardant diaphragm material.
[0053] Wherein, the initiator is dicumyl peroxide and the wetting agent is sodium dodecyl sulfate.
[0054] Example 6
[0055] A method for preparing a flame retardant diaphragm material for a lithium battery comprises the following steps:
[0056] (1) In parts by weight, 20 parts of polyvinylidene fluoride-hexafluoropropylene copolymer (molecular weight 500,000, purchased from Shanghai MacLean Biochemical Technology Co., Ltd.), 22 parts of the zeolite-based reinforcing agent of Example 2, 4 parts of the POSS-based crosslinking agent of Example 3 and 60 parts of deionized water were added to a stirrer, stirred at a speed of 800 r / min for 0.8 h, 0.4 parts of initiator were added, stirred for 0.5 h, and then 0.8 parts of wetting agent were added, and stirring was continued for 0.8 h to obtain a flame retardant coating;
[0057] (2) The flame retardant coating is uniformly coated on both sides of the single-layer polypropylene porous membrane, with a single-side coating thickness of 2 μm. The membrane is placed in a 55° C. environment and dried for 7 h, and then rolled up to obtain a lithium battery flame retardant diaphragm material.
[0058] Wherein, the initiator is benzoyl peroxide and the wetting agent is sodium dodecyl sulfate.
[0059] Example 7
[0060] A method for preparing a flame retardant diaphragm material for a lithium battery comprises the following steps:
[0061] (1) In parts by weight, 23 parts of polyvinylidene fluoride-hexafluoropropylene copolymer (molecular weight 500,000, purchased from Shanghai MacLean Biochemical Technology Co., Ltd.), 25 parts of the zeolite-based reinforcing agent of Example 2, 5 parts of the POSS-based crosslinking agent of Example 4 and 65 parts of deionized water were added to a stirrer, stirred at a speed of 1000 r / min for 1 hour, 0.6 parts of initiator were added, stirred for 0.5 hours, and then 1 part of wetting agent was added, and stirring was continued for 1 hour to obtain a flame retardant coating;
[0062] (2) The flame retardant coating was evenly coated on both sides of the single-layer polypropylene porous membrane with a single-side coating thickness of 3 μm. The membrane was placed in a 60° C. environment and dried for 6 h. The membrane was rolled up to obtain a flame retardant separator material for a lithium battery.
[0063] Wherein, the initiator is dicumyl peroxide and the wetting agent is sodium dodecyl sulfate.
[0064] Comparative Example 2
[0065] A method for preparing a flame-retardant diaphragm material for a lithium battery, based on Example 5, wherein the zeolite-based enhancer in Example 5 is replaced by the substance in Comparative Example 1, and the remaining raw materials and preparation process are the same as in Example 5.
[0066] Comparative Example 3
[0067] A method for preparing a flame retardant diaphragm material for a lithium battery, based on Example 5, wherein the POSS-based cross-linking agent in Example 5 is replaced with divinylbenzene, and the remaining raw materials and preparation process are the same as Example 5.
[0068] The flame retardant diaphragm materials for lithium batteries obtained from Examples 5 to 7 and Comparative Examples 2 to 3 were tested, and the test items were as follows:
[0069] (I) Heat resistance: longitudinal and transverse shrinkage test (heating at 180°C for 6 hours, testing the longitudinal and transverse dimensional changes before and after heating);
[0070] (ii) Liquid absorption rate: The liquid absorption rate of the coated diaphragm was tested by weighing method. First, the mass of the diaphragm was recorded after it was completely dried. Then, the completely dried diaphragm was immersed in electrolyte for 24 hours. After the surface electrolyte was wiped dry, the weight of the diaphragm was recorded again. The difference between the two records was the liquid absorption rate of the diaphragm. Five samples were tested and the average value was calculated. The electrolyte composition was: 1 mol / L LiPF6 ethylene carbonate and dimethyl carbonate solution, in which the volume ratio of solvent ethylene carbonate and dimethyl carbonate was 1:1.
[0071] (III) Limiting oxygen index: tested in accordance with standard JIS-K7201-3-2008;
[0072] The test results are shown in Table 1:
[0073] Table 1
[0074] project Example 5 Example 6 Example 7 Comparative Example 2 Comparative Example 3 Longitudinal shrinkage (180℃, 4h) 1.3 1.2 1.0 1.3 2.4 Transverse shrinkage (180℃, 4h) 1.1 0.9 0.8 1.1 1.5 Liquid absorption rate (%) 206 211 215 187 190 Limiting oxygen index (%) 40.2 40.8 41.2 40.0 38.6
[0075] It can be seen from Table 1 that, compared with Comparative Example 2 and Comparative Example 3, the flame retardant diaphragm materials for lithium batteries obtained in Examples 5, 6 and 7 have better heat resistance, flame retardancy and liquid absorption rate.
[0076] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0077] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing a flame retardant diaphragm material for a lithium battery, characterized in that: The following steps are involved: (1) Mixing polyvinylidene fluoride polymer, zeolite-based reinforcing agent, POSS-based crosslinking agent and deionized water, stirring for 0.5-1h, adding initiator, stirring for 0.5h, adding wetting agent, and continuing to stir for 0.5-1h to obtain flame retardant coating; (2) uniformly coating the flame retardant coating on one side or both sides of the base film, drying it in an environment of 50-60°C for 6-8 hours, and rolling it up to obtain a flame retardant separator material for a lithium battery; The zeolite-based enhancer is obtained by the following steps: Pentaerythritol triallyl ether and 3-aminopropyltriethoxysilane are added to anhydrous tetrahydrofuran, reacted at 50°C for 12 hours under closed conditions, and the anhydrous tetrahydrofuran is removed under reduced pressure to obtain an intermediate product. The intermediate product and nano zeolite are placed in a solution consisting of tetrahydrofuran and deionized water, subjected to ultrasound for 30 minutes, and reacted at 50°C for 12 hours to obtain a zeolite-based enhancer. The POSS-based crosslinker is obtained by the following steps: S1, hexachlorocyclotriphosphazene and octa-p-aminophenyl-POSS were mixed and ground, and then transferred to a hydrothermal reactor, reacted at 160° C. for 12 h, and then cooled to room temperature, centrifuged the product, and washed alternately with anhydrous methanol and deionized water. The centrifuged product was placed in an oven at 120° C. and dried to constant weight to obtain an amino-terminated nitrogen-phosphorus POSS polymer; S2. Add acrylic acid, EDC·HCl and NHS to dimethyl sulfoxide, stir for 0.5 h, add amino-terminated nitrogen and phosphorus POSS polymer, stir and react for 24 h. After the reaction is completed, pour the reaction product into acetone for precipitation, wash it with acetone for 3 times, filter it, and vacuum dry it at 60°C to constant weight to obtain a POSS-based cross-linking agent.
2. The method for preparing a flame retardant separator material for a lithium battery according to claim 1, characterized in that: The flame retardant coating comprises the following raw materials in parts by weight: 18-23 parts of polyvinylidene fluoride polymer, 20-25 parts of zeolite-based reinforcing agent, 3-5 parts of POSS-based crosslinking agent, 0.2-0.6 parts of initiator, 0.5-1 parts of wetting agent and 55-65 parts of deionized water.
3. The method for preparing a flame retardant separator material for a lithium battery according to claim 1, characterized in that: The mass ratio of pentaerythritol triallyl ether to 3-aminopropyltriethoxysilane is 7.7-8.0:6.6, and the dosage ratio of the intermediate product, nano zeolite, tetrahydrofuran and deionized water is 2g:1-2g:60-80mL:5-10mL.
4. The method for preparing a flame retardant separator material for a lithium battery according to claim 1, characterized in that: The mass ratio of hexachlorocyclotriphosphazene to octa-p-aminophenyl-POSS in S1 is 0.7:2.6-3.
0.
5. The method for preparing a flame retardant separator material for a lithium battery according to claim 1, characterized in that: The usage ratio of acrylic acid, EDC·HCl, NHS, dimethyl sulfoxide and amino-terminated nitrogen-phosphorus POSS polymer in S2 is 0.4-0.6 g: 0.96 g: 0.56 g: 200 mL: 4.4-5.2 g.
6. A flame retardant diaphragm material for a lithium battery, characterized in that: Prepared by the preparation method according to any one of claims 1 to 5.
Citation Information
Patent Citations
A flame-retardant lithium battery coated separator and its preparation method are related to lithium-ion batteries.
CN116231228B
Novel lithium ion battery diaphragm with inorganic coating and preparation method thereof
CN103107301A
Inorganic filler modified ultraviolet curing adhesive
CN105820794A
POSS (polyhedral oligomeric silsesquioxane) enhanced aramid fiber coated membrane for lithium battery, and preparation method of POSS enhanced aramid fiber coated membrane
CN107768581A
Preparation method of lithium battery composite diaphragm with multi-layer structure
CN114421091A