A preparation device and preparation method of high nitrogen steel
By setting up a mixing chamber and nozzle at the bottom of the ladle, using argon and nitrogen to convection to mix nitrogen and nitrogen-containing alloy powder, the problem of diffusion control of nitrogen elements is solved, and uniform nitrogen increase and deoxygenation of high-nitrogen rebar is achieved, and the thread is improved The strength and corrosion resistance of steel are suitable for special environmental engineering.
Patent Information
- Application Number
- CN202311232798.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-22
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2043-09-22
AI Technical Summary
In the production of high-nitrogen rebar, the diffusion of nitrogen elements is difficult to control, and excessive nitrogen content is prone to occur, resulting in a large amount of nitrogen pores in the casting billet. The yield and uniformity of the components fluctuate significantly after the addition of nitrogen-containing alloys, which is difficult to control. .
A high-nitrogen steel preparation device is designed, including a mixing chamber, argon pipeline, nitrogen pipeline and gas-carrying alloy powder pipeline. The nitrogen gas and nitrogen-containing alloy powder are mixed in the mixing chamber through the nozzle, and strong convection is used to ensure that After fully mixing with the alloy powder, nitrogen gas is sprayed from the bottom of the ladle into the liquid steel. Combined with the powder control system and the flowmeter of the regulating valve, the nitrogen content in the liquid steel is uniformly and stably increased.
The nitrogen content in the steel is uniformly and stably improved, the appearance of cast billet pores is avoided, the strength and corrosion resistance of rebar are improved, and it is suitable for areas with special performance requirements such as marine engineering and nuclear industry.
Smart Images

Figure CN117248153B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of steel smelting, and specifically relates to a preparation device and a preparation method for high nitrogen steel. Background Art
[0002] Rebar is one of the basic materials used in building and infrastructure construction, and is commonly used for the reinforcement of concrete.
[0003] The nitrogen content of rebar currently produced by conventional smelting processes is usually low, below 0.012%, while the nitrogen content of high-nitrogen rebar is required to reach above 0.020%. Although the increase in nitrogen content can effectively improve the performance of rebar, the solubility of nitrogen in the component system of rebar is low, which leads to certain difficulties in increasing nitrogen in rebar during the smelting process.
[0004] In the field of iron and steel metallurgy, there are generally two ways to increase the nitrogen content in steel. One is to increase the nitrogen content in molten steel by setting a nozzle at the bottom of the ladle to spray nitrogen into the molten steel during the refining process outside the furnace; the other is to increase the nitrogen content in the molten steel by adding nitrogen-containing alloys to the molten steel from the top of the ladle during the alloying process.
[0005] However, both methods of producing high-nitrogen rebar have certain limitations. For nitrogen injection, the diffusion of nitrogen in the molten steel is difficult to control, and the nitrogen content is easily too high, which in turn causes a large number of nitrogen pores to appear in the ingot. For the method of adding nitrogen-containing alloys to the top of the molten steel, the reaction after the alloy is added is close to the gas-molten pool interface, which leads to significant fluctuations in the yield and uniformity of the relevant components, which are difficult to control. Summary of the invention
[0006] The object of the present invention is to provide a high nitrogen steel preparation device to solve at least one aspect of the problems and defects raised in the above background technology.
[0007] The present invention also provides a method for preparing the high nitrogen steel.
[0008] Specifically, the first aspect of the present invention discloses a high nitrogen steel preparation device, which is arranged at the bottom of a ladle and includes:
[0009] Mixing chamber, argon gas pipeline, nitrogen gas pipeline and airborne alloy powder pipeline;
[0010] The two sides of the mixing chamber are connected to the output ports of the argon pipeline; the input port of the argon pipeline is connected to the argon gas supply equipment;
[0011] Both sides of the lower part of the mixing chamber are connected with output ports of a nitrogen pipeline, and the input port of the nitrogen pipeline is connected with a nitrogen supply device;
[0012] The middle of the lower part of the mixing chamber is connected with an output port of an airborne alloy powder pipeline, and the input port of the airborne alloy powder pipeline is connected with a nitrogen gas supply device and a powder supply device;
[0013] Nozzle; the nozzle is arranged at the top of the device, and the device is connected with the bottom of the ladle through the nozzle.
[0014] According to one technical solution of the technical solution of the high nitrogen steel preparation device of the present invention, at least the following technical effects are achieved:
[0015] The high nitrogen steel preparation device delivers nitrogen to a mixing chamber through a nitrogen pipeline outlet, and delivers nitrogen-containing alloy powder to the mixing chamber through an airborne alloy powder pipeline outlet, and the nitrogen and the nitrogen-containing alloy powder are preliminarily mixed in the mixing chamber; in order to ensure the mixing effect, argon is delivered to the mixing chamber through argon pipeline outlets on both sides of the mixing chamber, and the argon delivered in the horizontal direction on both sides of the mixing chamber collides with the nitrogen and the nitrogen-containing alloy powder delivered in the vertical direction at the bottom of the mixing chamber, generating strong convection, further mixing the nitrogen and the nitrogen-containing alloy powder, and the mixed composite gas is sprayed from the bottom of the ladle into the molten steel through a nozzle on the top of the device, so as to achieve the purpose of uniformly and stably increasing the nitrogen content in the molten steel.
[0016] As a further solution of the present invention: the airborne alloy powder pipeline is provided with a powder control system.
[0017] Since the airborne alloy powder pipeline is provided with a powder control system, it is used to control the spraying of powder, which is pre-mixed with the nitrogen in the airborne alloy powder pipeline to form nitrogen-containing alloy powder, and then transported to the mixing chamber from the output port of the airborne alloy powder pipeline.
[0018] As a further solution of the present invention: the argon pipeline, nitrogen pipeline, airborne alloy powder pipeline and nozzle are respectively provided with regulating valves and flow meters.
[0019] Since the argon pipeline, nitrogen pipeline, airborne alloy powder pipeline and nozzle are respectively provided with regulating valves and flow meters, when each pipeline transports gas to the mixing chamber, the gas flow rate can be controlled by the regulating valve, and the flow meter can be used to observe whether the gas flow rate is controlled in place.
[0020] The second aspect of the present invention also discloses a method for preparing high nitrogen steel, comprising the following steps:
[0021] S1. Add slag-making materials into the ladle. After slag-making is completed, turn on the nitrogen supply equipment, adjust the regulating valve, and deliver nitrogen into the mixing chamber. After the airflow reaches a stable state, keep it for 1 to 3 minutes;
[0022] S2, opening the nitrogen gas supply device of the airborne alloy powder pipeline, adjusting the regulating valve, and simultaneously opening the powder supply device to transport the nitrogen-containing alloy powder entrained by nitrogen into the mixing chamber;
[0023] S3, turning on the argon gas supply equipment, adjusting the regulating valve, and delivering argon gas into the mixing chamber;
[0024] S4, turning on the nozzle switch, adjusting the regulating valve, spraying the nitrogen and nitrogen-containing alloy powder composite gas from the bottom of the ladle into the molten steel, and fully mixing with the molten steel to obtain high nitrogen steel;
[0025] S5. The obtained high nitrogen steel is sent to a continuous casting workshop, and high nitrogen threaded steel is obtained after smelting.
[0026] As a further solution of the present invention: wherein the alloy powder includes magnesium powder, manganese powder, silicon powder and nitrogen-containing alloy.
[0027] As a further solution of the present invention: wherein the alloy powder comprises the following raw materials in mass fractions: magnesium powder 6%~10%, manganese powder 15%~30%, silicon powder 15%~30%, and nitrogen-containing alloy 30%~60%.
[0028] The introduction of silicon powder and manganese powder plays a role in deoxidation and alloying, which helps to optimize the performance of steel; the introduction of magnesium powder has a dual role: on the one hand, it further reduces the oxygen and sulfur content in the steel; on the other hand, since magnesium has a lower melting point, its vapor will rise from the bottom of the furnace and stir the molten steel, thereby increasing the contact frequency between magnesium and molten steel, making the composite gas of nitrogen and nitrogen-containing alloy powder mix more fully with the molten steel.
[0029] As a further solution of the present invention: wherein the nitrogen flow rate in the nitrogen pipeline is controlled to be 0.04m 3 / s to 0.05m 3 / s.
[0030] As a further solution of the present invention: wherein the nitrogen flow rate in the airborne alloy powder pipeline is controlled to be 0.02m 3 / s to 0.03m 3 / s.
[0031] As a further solution of the present invention: wherein the argon flow rate in the argon pipeline is controlled to be 0.05m 3 / s to 0.07m 3 / s.
[0032] The preparation method can integrate nitrogen addition and deoxidation of molten steel, which can not only increase the nitrogen content in the molten steel in a short time, but also improve the cleanliness of the molten steel, make the components more evenly mixed, avoid the situation where the nitrogen content in the local molten steel is too high and cause a large number of nitrogen pores in the ingot, and achieve the purpose of evenly and stably increasing the nitrogen content in the molten steel.
[0033] The high-nitrogen rebar produced by this method has a more uniform nitrogen content, which effectively improves the strength and corrosion resistance of the rebar. It can be used in fields with special performance requirements, such as marine engineering, chemical equipment, nuclear industry and other extreme service environment engineering projects. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] In order to facilitate understanding by those skilled in the art, the present invention is further described below with reference to the accompanying drawings.
[0035] Figure 1 This is a schematic diagram of the structure of a high nitrogen steel preparation device.
[0036] Reference numerals:
[0037] 101. Mixing chamber; 102. Argon gas pipeline; 103. Nitrogen gas pipeline; 104. Airborne alloy powder pipeline; 105. Nozzle; 106. Regulating valve. DETAILED DESCRIPTION
[0038] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the technical solution of the present invention is further specifically described below by way of examples and in conjunction with the accompanying drawings. In the specification, the same or similar reference numerals indicate the same or similar components. The following description of the embodiments of the present invention with reference to the accompanying drawings is intended to explain the overall inventive concept of the present invention and should not be construed as a limitation of the present invention.
[0039] In addition, in the detailed description below, for ease of explanation, many specific details are set forth to provide a comprehensive understanding of the disclosed embodiments. However, it is apparent that one or more embodiments may be implemented without these specific details. In other cases, known structures and devices are embodied in a schematic manner to simplify the accompanying drawings.
[0040] like Figure 1The embodiment of the present invention is shown, a preparation device of high nitrogen steel is arranged at the bottom of the ladle 100, including: a mixing chamber 101, an argon pipeline 102, a nitrogen pipeline 103 and an airborne alloy powder pipeline 104; the output ports of the argon pipeline 102 are connected on both sides of the mixing chamber 101; the input port of the argon pipeline 102 is connected to the argon gas supply equipment; the output ports of the nitrogen pipeline 103 are connected on both sides of the lower part of the mixing chamber 101, and the input port of the nitrogen pipeline 103 is connected to the nitrogen gas supply equipment; the output port of the airborne alloy powder pipeline 104 is connected in the middle of the lower part of the mixing chamber 101, and the input port of the airborne alloy powder pipeline 104 is connected to the nitrogen gas supply equipment and the powder supply equipment; the nozzle 105 is arranged at the top of the device, and the device is connected to the bottom of the ladle 100 through the nozzle 105.
[0041] Specifically, the high nitrogen steel preparation device delivers nitrogen to the mixing chamber 101 through the output port of the nitrogen pipeline 103, and at the same time delivers the nitrogen-containing alloy powder to the mixing chamber 101 through the output port of the airborne alloy powder pipeline 104, and the nitrogen and the nitrogen-containing alloy powder are preliminarily mixed in the mixing chamber 101; in order to ensure the mixing effect, argon is delivered to the mixing chamber 101 through the output ports of the argon pipeline 102 on both sides of the mixing chamber 101, and the argon delivered horizontally on both sides of the mixing chamber 101 collides with the nitrogen and the nitrogen-containing alloy powder delivered vertically at the bottom of the mixing chamber 101, generating strong convection, further mixing the nitrogen and the nitrogen-containing alloy powder, and the mixed composite gas is sprayed into the molten steel from the bottom of the ladle 100 through the nozzle 105 at the top of the device, so as to achieve the purpose of uniformly and stably increasing the nitrogen content in the molten steel.
[0042] The airborne alloy powder pipeline 104 is provided with a powder control system (not shown in the figure). Specifically, since the airborne alloy powder pipeline 104 is provided with a powder control system, the system is used to control the powder to be sprayed out, pre-mixed with the nitrogen in the airborne alloy powder pipeline 104, to form a nitrogen-containing alloy powder, and then transported to the mixing chamber from the output port of the airborne alloy powder pipeline 104.
[0043] like Figure 1 As shown, the argon gas pipeline 102, the nitrogen gas pipeline 103, the gas-borne alloy powder pipeline 104 and the nozzle 105 are respectively provided with a regulating valve 106 and a flow meter. Specifically, since the argon gas pipeline 102, the nitrogen gas pipeline 103, the gas-borne alloy powder pipeline 104 and the nozzle 105 are respectively provided with a regulating valve 106 and a flow meter, when each pipeline transports gas to the mixing chamber 101, the gas flow rate can be controlled by the regulating valve 106, and the flow meter can be used to observe whether the gas flow rate is controlled within the required range.
[0044] Another embodiment of the present invention also discloses a method for preparing high nitrogen steel, comprising the following steps:
[0045] S1. Add slag-making materials into the ladle 100. After slag-making is completed, turn on the nitrogen supply equipment, adjust the regulating valve 106, and deliver nitrogen into the mixing chamber 101. After the airflow reaches a stable state, keep it for 1 to 3 minutes;
[0046] S2, opening the nitrogen supply device of the airborne alloy powder pipeline 104, adjusting the regulating valve 106, and opening the powder supply device at the same time, to transport the nitrogen-containing alloy powder entrained by nitrogen into the mixing chamber 101;
[0047] S3, turn on the argon gas supply equipment, adjust the regulating valve 106, and deliver the argon gas into the mixing chamber 101;
[0048] S4, opening the nozzle 105 switch, adjusting the regulating valve 106, spraying the nitrogen and nitrogen-containing alloy powder composite gas from the bottom of the ladle 100 into the molten steel, and fully mixing with the molten steel to obtain high nitrogen steel;
[0049] S5. The obtained high nitrogen steel is sent to a continuous casting workshop, and high nitrogen threaded steel is obtained after smelting.
[0050] Specifically, using the preparation method, nitrogen is delivered to the mixing chamber 101 through the output port of the nitrogen pipeline 103, and the airflow is maintained for 1 to 3 minutes after reaching a stable state.
[0051] At the same time, the nitrogen-containing alloy powder is transported to the mixing chamber 101 through the outlet of the airborne alloy powder pipeline 104 , and the nitrogen gas and the nitrogen-containing alloy powder are preliminarily mixed in the mixing chamber 101 .
[0052] To ensure the mixing effect, argon is delivered to the mixing chamber 101 through the output ports of the argon pipes 102 on both sides of the mixing chamber 101. The argon delivered horizontally on both sides of the mixing chamber 101 collides with the nitrogen delivered vertically at the bottom of the mixing chamber 101 and the nitrogen-containing alloy powder, generating strong convection to further mix the nitrogen and the nitrogen-containing alloy powder.
[0053] The mixed composite gas is sprayed into the molten steel from the bottom of the ladle 100 through the nozzle 105 at the top of the device, so as to increase the nitrogen content in the molten steel uniformly and stably, thereby producing high nitrogen steel.
[0054] The high nitrogen steel is then sent to the continuous casting workshop and smelted to produce high nitrogen rebar.
[0055] In the above-mentioned method for preparing high nitrogen steel, the alloy powder includes magnesium powder, manganese powder, silicon powder and nitrogen-containing alloy. The alloy powder includes the following raw materials in mass fraction: magnesium powder 6% to 10%, manganese powder 15% to 30%, silicon powder 15% to 30%, and nitrogen-containing alloy 30% to 60%.
[0056] Specifically, the introduction of silicon powder and manganese powder plays a role in deoxidation and alloying, which helps to optimize the performance of steel; while the introduction of magnesium powder has a dual role: on the one hand, it further reduces the oxygen and sulfur content in the steel; on the other hand, since magnesium has a lower melting point, its vapor will rise from the bottom of the furnace and stir the molten steel, thereby increasing the contact frequency between magnesium and molten steel, making the composite gas of nitrogen and nitrogen-containing alloy powder more fully mixed with the molten steel.
[0057] In the above-mentioned method for preparing high nitrogen steel, the nitrogen flow rate in the nitrogen pipeline 103 is controlled to be 0.04m 3 / s to 0.05m 3 / s; the nitrogen flow rate in the airborne alloy powder pipeline 104 is controlled to be 0.02m 3 / s to 0.03m 3 / s; the argon gas flow rate in the argon gas pipeline 102 is controlled to be 0.05m 3 / s to 0.07m 3 / s.
[0058] In the first embodiment of the method for preparing high nitrogen steel of the present invention, the airborne alloy powder and nitrogen are transported to the mixing chamber 101, and the nitrogen and the airborne alloy powder are mixed under the stirring of argon in the mixing chamber 101, wherein the nitrogen flow rate is 0.04m 3 / s, the airborne alloy powder flow rate is 0.02m 3 / s, the alloy powder contains 4% magnesium powder, 15% manganese powder, 15% silicon powder, and 66% vanadium nitride. The argon flow rate is 0.05m 3 / s, blown into the interior of the ladle, the refined ladle is placed on the ladle seating station, samples are taken at appropriate locations for full analysis and temperature measurement, the heating cover is lowered, and according to the measured temperature and the requirements of the steel type being produced, the corresponding alloy is added to make up the composition to the standard composition range, the input voltage and current are adjusted, the power is turned on for heating, the power is turned off, the three-phase electrode is raised, the furnace cover is raised, the temperature is measured, the molten steel temperature is required to be controlled at 1550℃~1600℃, and materials are added to make reducing slag. After refining, it is sent to the continuous casting workshop, the tundish is protected and poured, and the pulling speed is 2.5~3.5 m / min.
[0059] The second embodiment of the method for preparing high nitrogen steel of the present invention is adopted, and the same method is not repeated here. The difference from the first embodiment is that the nitrogen flow rate is 0.04m 3 / s, the airborne alloy powder flow rate is 0.03m 3 / s, the alloy powder contains 6% magnesium powder, 12% manganese powder, 18% silicon powder, and 64% vanadium nitride. The argon flow rate is 0.06m 3 / s.
[0060] The third embodiment of the method for preparing high nitrogen steel of the present invention is adopted, and the same method is not repeated here. The difference from the first two embodiments is that the nitrogen flow rate is 0.04m 3 / s, the airborne alloy powder flow rate is 0.02m 3 / s, the alloy powder contains 8% magnesium powder, 20% manganese powder, 20% silicon powder, and 56% vanadium nitride. The argon flow rate is 0.07m 3 / s.
[0061] Comparative Example: During the refining process of rebar outside the furnace, after the refining ladle car runs to the slag adding station and stops steadily, slag-making materials are added into the ladle 100, and nitrogen is blown, with a nitrogen flow rate of 0.003m 3 / s, blown into the interior of the ladle, the refined ladle is placed on the ladle seating station, samples are taken at appropriate locations for full analysis and temperature measurement, the heating cover is lowered, and according to the measured temperature and the requirements of the steel type being produced, the corresponding alloy is added to make up the composition to the standard composition range, the input voltage and current are adjusted, the power is turned on for heating, the power is turned off, the three-phase electrode is raised, the furnace cover is raised, the temperature is measured, the molten steel temperature is required to be controlled at 1550℃~1600℃, and materials are added to make reducing slag. After refining, it is sent to the continuous casting workshop, the tundish is protected and poured, and the pulling speed is 2.5~3.5 m / min.
[0062] The high nitrogen steels prepared in Examples 1 to 3 and Comparative Example 1 were subjected to performance tests, and the results are shown in Table 1.
[0063] Table 1 Performance test results of high nitrogen steels prepared in Examples 1 to 3 and Comparative Example 1
[0064]
[0065] According to the test results, the high nitrogen threaded steel is smelted by the present invention, and better nitrogen increase control is achieved. The design of this process allows various raw materials to be fully utilized in the furnace, the nitrogen content is more uniform, and there are fewer visible pores in the cross section of the ingot, which effectively improves the strength of the threaded steel, thereby achieving steel refining and optimization treatment, and successfully realizing the integration of nitrogen increase and deoxidation. The high nitrogen threaded steel can be used in fields requiring special performance requirements, such as marine engineering, chemical equipment, nuclear industry and other extreme service environment engineering projects.
[0066] The high nitrogen steel preparation device of the present invention delivers nitrogen to a mixing chamber 101 through an outlet of a nitrogen pipeline 103, and at the same time delivers nitrogen-containing alloy powder to the mixing chamber 101 through an outlet of an airborne alloy powder pipeline 104, and the nitrogen and the nitrogen-containing alloy powder are preliminarily mixed in the mixing chamber 101; in order to ensure the mixing effect, argon is delivered to the mixing chamber 101 through outlets of argon pipelines 102 on both sides of the mixing chamber 101, and the argon delivered in the horizontal direction on both sides of the mixing chamber 101 collides with the nitrogen and the nitrogen-containing alloy powder delivered in the vertical direction at the bottom of the mixing chamber 101, generating strong convection, further mixing the nitrogen and the nitrogen-containing alloy powder, and the mixed composite gas is sprayed into the molten steel from the bottom of the ladle 100 through a nozzle 105 at the top of the device, so as to achieve the purpose of uniformly and stably increasing the nitrogen content in the molten steel.
[0067] The preparation method of high nitrogen steel of the present invention can integrate nitrogen addition and deoxidation of molten steel, not only can the nitrogen content in molten steel be increased in a short time, but also the cleanliness of molten steel is improved, the component mixing is more uniform, fewer pores are visible on the cross section of the ingot, and the situation that the nitrogen content of the local molten steel is too high and a large number of nitrogen pores appear in the ingot is avoided, so as to achieve the purpose of uniformly and stably increasing the nitrogen content in the molten steel.
[0068] The high-nitrogen rebar produced by this method has a more uniform nitrogen content, which effectively improves the strength of the rebar. It can be used in fields with special performance requirements, such as marine engineering, chemical equipment, nuclear industry and other engineering projects in extreme service environments.
[0069] The specific embodiments described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A high nitrogen steel preparation device, arranged at the bottom of a ladle (100), characterized in that: include: A mixing chamber (101), an argon gas pipeline (102), a nitrogen gas pipeline (103), and an airborne alloy powder pipeline (104); The two sides of the mixing chamber (101) are connected to the output ports of the argon gas pipeline (102); the input port of the argon gas pipeline (102) is connected to the argon gas supply equipment; Both sides of the lower part of the mixing chamber (101) are connected to the output ports of the nitrogen pipeline (103), and the input port of the nitrogen pipeline (103) is connected to the nitrogen supply equipment; The middle of the lower part of the mixing chamber (101) is connected to an output port of an airborne alloy powder pipeline (104), and the input port of the airborne alloy powder pipeline (104) is connected to a nitrogen gas supply device and a powder supply device; Nozzle (105); the nozzle (105) is arranged at the top of the device, and the device is connected to the bottom of the ladle (100) through the nozzle (105).
2. The high nitrogen steel preparation device according to claim 1, characterized in that: The airborne alloy powder pipeline (104) is provided with a powder control system.
3. The high nitrogen steel preparation device according to claim 2, characterized in that: The argon pipeline (102), the nitrogen pipeline (103), the airborne alloy powder pipeline (104) and the nozzle (105) are each provided with a regulating valve (106) and a flow meter.
4. A method for preparing high nitrogen steel, prepared by using the high nitrogen steel preparation device as claimed in claim 3, characterized in that: The steps include: S1. Slag-making materials are added into the ladle (100). After slag-making is completed, the nitrogen supply device is turned on, and the regulating valve (106) is adjusted to transport nitrogen into the mixing chamber (101). After the gas flow reaches a stable state, it is maintained for 1 to 3 minutes; S2, opening the nitrogen supply device of the airborne alloy powder pipeline (104), adjusting the regulating valve (106), and simultaneously opening the powder supply device to transport the nitrogen-containing alloy powder entrained in nitrogen into the mixing chamber (101); S3, turning on the argon gas supply device, adjusting the regulating valve (106), and delivering the argon gas into the mixing chamber (101); S4, turning on the nozzle (105), adjusting the regulating valve (106), and injecting the nitrogen and nitrogen-containing alloy powder composite gas from the bottom of the ladle (100) into the molten steel, and fully mixing with the molten steel to produce high nitrogen steel; S5. The obtained high nitrogen steel is sent to a continuous casting workshop, and high nitrogen threaded steel is obtained after smelting.
5. The method for preparing high nitrogen steel according to claim 4, characterized in that: The alloy powder includes magnesium powder, manganese powder, silicon powder and nitrogen-containing alloy.
6. The method for preparing high nitrogen steel according to claim 5, characterized in that: The alloy powder comprises the following raw materials in mass fractions: 6% to 10% magnesium powder, 15% to 30% manganese powder, 15% to 30% silicon powder, and 30% to 60% nitrogen-containing alloy.
7. The method for preparing high nitrogen steel according to claim 4, characterized in that: The nitrogen flow rate in the nitrogen pipeline (103) is controlled to be 0.04 m 3 / s to 0.05m 3 / s.
8. The method for preparing high nitrogen steel according to claim 7, characterized in that: The nitrogen flow rate in the air-carrying alloy powder pipeline (104) is controlled to be 0.02 m 3 / s to 0.03m 3 / s.
9. The method for preparing high nitrogen steel according to claim 8, characterized in that: The argon gas flow rate in the argon gas pipeline (102) is controlled to be 0.05 m 3 / s to 0.07m 3 / s.
Citation Information
Patent Citations
Method for preparing high-nitrogen steel through combination of pressurized induction and protective-atmosphere electro-slag remelting
CN106756485A
High-nitrogen alloy steel and preparation method thereof
CN108660378A
Device for preparing high-nitrogen steel
CN209654687U
Ultra-high nitrogen ferritic heat resistant steel and its production
JP1994322487A
Method for adding nitrogen into molten steel
JP2000256730A