A dialkylphosphinate ammonium salt and its preparation method and application
By performing an alkylation reaction on dihydrocarbyl phosphinic acid to generate an ammonium salt of dihydrocarbyl phosphinic acid with active nitrogen atoms and alkylation groups, the problems of poor compatibility and insufficient flame retardant properties in polymer materials are solved and achieved. Efficient flame retardant effect and maintenance of physical properties.
Patent Information
- Application Number
- CN202311206309.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-18
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-09-18
AI Technical Summary
The existing application of dihydrocarbylphosphinic acid and its salts in polymer materials has problems such as poor compatibility, reduced cross-linking degree, high cost and insufficient reactivity. Especially when used in epoxy resin and polyurethane, the impact Improved flame retardant and physical properties.
By alkylation reaction of dialkyl phosphinic acid with NH3 or organic nitrogen-containing compounds, ammonium dialkyl phosphinate with active nitrogen atoms and appropriate alkylation groups is generated and applied to polymer materials. , to improve its compatibility and flame retardant efficiency.
It achieves good compatibility and flame retardant properties of dihydrocarbyl phosphinate ammonium salt in polymer materials, maintains the physical properties of epoxy resin, and is simple to prepare, suitable for industrial production, and overcomes the cost and compatibility of traditional methods. Sexual issues.
Smart Images

Figure CN117263974B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of flame retardant polymer materials and relates to a dialkylphosphinate ammonium salt and a preparation method and application thereof. Background Art
[0002] Polymer materials are widely used in all walks of life in the national economy. However, since most polymer materials are flammable, in order to reduce the fire disasters caused by them, it is often necessary to meet their flame retardant requirements by using flame retardant modification methods. The simplest way of flame retardant modification is to use flame retardants.
[0003] In recent years, phosphorus-based flame retardants have developed rapidly due to their high flame retardant efficiency and low smoke and toxicity of combustion products, especially dialkylphosphinic acid and its salts.
[0004] CN110945047A discloses the product of diethylphosphinic acid and epoxy reaction and its flame retardant application in polyurethane foam, but it is a monohydroxyl functional flame retardant, which reduces the crosslinking degree of polyurethane and consumes expensive isocyanate. WO2021074684 discloses diethylphosphinic acid or its product with epoxy resin for flame retardant of epoxy resin, but diethylphosphinic acid and epoxy reaction reduce the crosslinking functional group of epoxy resin, so that it needs to use low exothermic epoxy resin with trifunctionality and above. CN113929967B discloses dialkylphosphinic acid and amine compound neutralization product and its application, and such product is solid, has poor compatibility with polymer materials, and has uniform dispersion problem. EP3470444 discloses dialkylphosphinic acid quaternary ammonium salt, which is used for flame retardant of polyurethane, but quaternary ammonium salt lacks reactive groups and is easily precipitated and lost.
[0005] In summary, dialkylphosphinic acid can only be used after neutralization due to its strong acidity, but after neutralization, the number of functional groups of the neutralizer is often reduced, which is not conducive to the physical properties of flame retardant materials. In addition, existing solid dialkylphosphinic acid ammonium salts have poor compatibility with polymer materials and dialkylphosphinic acid quaternary ammonium salts lack reactivity. Summary of the invention
[0006] In view of the deficiencies in the prior art, the present invention aims to provide a dialkylphosphinate ammonium salt and a preparation method and application thereof.
[0007] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:
[0008] On the one hand, the present invention provides a dialkyl phosphinate ammonium salt, which is obtained by an alkylation reaction between a dialkyl phosphinate alkyl ester having a structural formula shown in formula (I) and NH3 or a nitrogen on at least one non-tertiary amine structure in an organic nitrogen-containing compound, wherein the alkyl group participating in the alkylation reaction comes from R1 in the structural formula shown in formula (I), the organic nitrogen-containing compound is selected from a primary amine, a secondary amine or an imine compound, and at least one nitrogen atom among the nitrogens that undergo an alkylation reaction in the dialkyl phosphinate ammonium salt has both an H atom and an R1 group obtained by the alkylation reaction.
[0009]
[0010] R1 is selected from C1~C 18 Straight chain alkyl, C1~C 18 Branched alkyl, or C3~C 18 Cycloalkyl;
[0011] R2 and R3 are independently selected from C1 to C 18 Straight chain alkyl, C1~C 18 Branched alkyl, C3~C 18 Cycloalkyl or C6~C 24 Aromatic base.
[0012] Preferably, R1 is selected from any one of methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl or decyl. Preferably, R1 is selected from any one of methyl, ethyl, propyl or butyl. Preferably, R1 is selected from any one of methyl and ethyl.
[0013] Preferably, R2 and R3 are independently selected from any one of methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl or phenyl. Alternatively, R2 and R3 are independently selected from any one of ethyl, propyl or butyl. Preferably, R2 and R3 are ethyl.
[0014] The dihydrocarbyl phosphinate alkyl ester having the structural formula shown in formula (I) can be a pure dihydrocarbyl phosphinate alkyl ester or a mixed dihydrocarbyl phosphinate alkyl ester having different R1, R2, and R3 substituents. For example, the dihydrocarbyl phosphinate alkyl ester can be methyl diethyl phosphinate, ethyl diethyl phosphinate, or a mixture thereof.
[0015] Preferably, the dihydrocarbyl phosphinate alkyl ester comprises one or a combination of at least two of methyl dimethylphosphinate, methyl diethylphosphinate, methyl dipropylphosphinate, methyl ethylpropylphosphinate, methyl diphenylphosphinate, ethyl dimethylphosphinate, ethyl diethylphosphinate, ethyl dipropylphosphinate, ethyl ethylpropylphosphinate, propyl dimethylphosphinate, propyl diethylphosphinate, propyl dipropylphosphinate, propyl ethylpropylphosphinate, methylphenylphosphinate or methyl diphenylphosphinate.
[0016] The organic nitrogen-containing compound is selected from primary amines, secondary amines and imines. In the present invention, primary amines are derivatives in which one hydrogen atom in the NH3 molecule is replaced by a (substituted) hydrocarbon group, secondary amines are derivatives in which two hydrogen atoms in the NH3 molecule are replaced by (substituted) hydrocarbon groups, and imines are structurally equivalent to products obtained by condensation of ammonia or primary amines with aldehydes or ketones, and have an amine shown in the following formula (II).
[0017] R4
[0018]
[0019] Wherein, R4 and R5 are independently selected from hydrogen, substituted or unsubstituted alkyl, and substituted or unsubstituted aromatic.
[0020] In the structure of the primary amine, secondary amine, and imine, a plurality of amino groups and / or imino groups and / or -C=NH groups may be contained in the same molecule. For example, in the primary amine, two amino groups, or one amino group and one imino group, or one amino group and one -C=NH group may be contained at the same time. When there are a plurality of amino groups, imino groups, and / or -C=NH groups in the structure of the primary amine, secondary amine, and imine, the dialkylphosphinate ammonium salt formed by the alkylation reaction of at least one nitrogen atom therein with the dialkylphosphinate alkyl ester also falls within the scope of the present invention. In the present invention, typical organic nitrogen-containing compounds include methylamine, ethylamine, propylamine, butylamine, pentylamine, hexylamine, heptylamine, octylamine, nonylamine, quinoline, dodecylamine, octadecylamine, cyclohexylamine, diethylamine, methylpropylamine, ethylenediamine, propylenediamine, butylenediamine, pentylenediamine, hexylenediamine, heptylenediamine, octylenediamine, 1,4-cyclohexyldiamine, diethanolamine, m-phenylenediamine, p-phenylenediamine, piperazine, 2-methylpiperazine, 2-methylimidazole, tetraethylenepentamine, triethylenetetramine, aniline, N-methylaniline, 4-methylaniline, diaminodiphenylmethane, 2,2-bis(4-aminophenyl)propane, diaminodiphenyl sulfone, diaminobenzophenone, cyanamide, melamine or dicyandiamide, or a combination of at least two thereof.
[0021] Preferably, the organic nitrogen-containing compound is a primary amine compound.
[0022] At least one of the nitrogen atoms in the dialkylphosphinate ammonium salt that has undergone the alkylation reaction has an H atom. After the reaction of the dialkylphosphinate alkyl ester and the organic nitrogen-containing compound is completed, at least one of the nitrogen atoms in the organic nitrogen portion of the dialkylphosphinate ammonium salt that has participated in the alkylation reaction still has at least one H atom.
[0023] Preferably, the dialkyl ammonium hypophosphite salt has any one of the following structures:
[0024]
[0025]
[0026] In the above formulae (III) to (XVIII), R1, R2, and R3 have the same definitions as R1, R2, and R3 in formula (I).
[0027] Preferably, in the above formula (III) to formula (XVIII), R1 is selected from a C1-C6 alkyl group; R2 and R3 are independently selected from a C1-C 18 Straight or branched alkyl or C6~C 24 Aromatic base.
[0028] Preferably, R1 is independently selected from methyl, ethyl, propyl, isopropyl or butyl; R2 and R3 are independently selected from methyl, ethyl, propyl, isopropyl, butyl or phenyl.
[0029] Preferably, R1 is selected from methyl, ethyl or propyl; R2 and R3 are independently selected from ethyl, propyl, isopropyl or butyl.
[0030] Preferably, R1 is selected from methyl, ethyl or propyl; R2 and R3 are ethyl.
[0031] On the other hand, the present invention provides a method for preparing the dialkylphosphinate ammonium salt as described above, the preparation method comprising the following steps:
[0032] The dialkylphosphinate alkyl ester is subjected to an alkylation reaction with NH3 or the nitrogen on at least one non-tertiary amine structure in an organic nitrogen-containing compound to obtain the dialkylphosphinate ammonium salt.
[0033] When there are multiple nitrogens in the organic nitrogen-containing compound, one or more of them can participate in the alkylation reaction, but at least one of the nitrogens still has at least one hydrogen atom after participating in the alkylation reaction. For example, the organic nitrogen-containing compound used in the present invention may include primary amines, secondary amines and imines containing tertiary amine structures. In this case, the nitrogen of the tertiary amine structure can also be alkylated by the dialkylphosphinate alkyl ester, but at least one of all the nitrogens participating in the alkylation reaction in the primary amines, secondary amines and imines still has at least one hydrogen atom.
[0034] Typical dihydrocarbyl phosphinate alkyl esters include methyl dimethylphosphinate, methyl diethylphosphinate, methyl dipropylphosphinate, methyl ethylpropylphosphinate, methyl diphenylphosphinate, ethyl dimethylphosphinate, ethyl diethylphosphinate, ethyl dipropylphosphinate, ethyl ethylpropylphosphinate, propyl dimethylphosphinate, propyl diethylphosphinate, propyl dipropylphosphinate, propyl ethylpropylphosphinate, methyl phenylphosphinate or methyl diphenylphosphinate, or a combination of at least two thereof.
[0035] Optionally, the organic nitrogen-containing compound includes methylamine, ethylamine, propylamine, butylamine, pentylamine, hexylamine, heptylamine, octylamine, nonylamine, quinoline, dodecylamine, octadecylamine, cyclohexylamine, diethylamine, methylpropylamine, ethylenediamine, propylenediamine, butylenediamine, pentylenediamine, hexylenediamine, heptylenediamine, octanediamine, 1,4-cyclohexyldiamine, diethanolamine, m-phenylenediamine, p-phenylenediamine, piperazine, 2-methylpiperazine, 2-methylimidazole, tetraethylenepentamine, triethylenetetramine, aniline, N-methylaniline, 4-methylaniline, diaminodiphenylmethane, 2,2-bis(4-aminophenyl)propane, diaminodiphenyl sulfone, diaminobenzophenone, cyanamide, melamine or dicyandiamide, or a combination of at least two thereof.
[0036] In the present invention, the molar ratio of the reaction of the organic nitrogen-containing compound and the dialkyl phosphinate is determined by the total amount of nitrogen in the organic nitrogen-containing compound. Preferably, the molar ratio of the sum of the molar numbers of nitrogen in the organic nitrogen-containing compound to the dialkyl phosphinate is 10 / 1-1 / 10, such as 10 / 1, 9 / 1, 8 / 1, 7 / 1, 6 / 1, 5 / 1, 4 / 1, 3 / 1, 2 / 1, 1 / 1, 1 / 2, 1 / 3, 1 / 4, 1 / 5, 1 / 6, 1 / 7, 1 / 8, 1 / 9 or 1 / 10. If the ratio is too small, the flame retardancy of the obtained product is poor, and if the ratio is too high, the excess dialkyl phosphinate needs to be recovered, and the economic efficiency is reduced.
[0037] Preferably, the molar ratio of the sum of the molar numbers of nitrogen in the organic nitrogen-containing compound to the alkyl dihydrocarbyl phosphinate is 6 / 1-1 / 6; for example, it can be 5 / 1-1 / 6; 4 / 1-1 / 6; 3 / 1-1 / 6; 2 / 1-1 / 6; 1 / 1-1 / 6; 1 / 1-1 / 5; 1 / 1-1 / 4; 1 / 1-1 / 3, 1 / 1-1 / 2.5 or 1 / 1-1 / 2.
[0038] Preferably, the alkylation reaction temperature is 0-250°C, such as 0°C, 10°C, 50°C, 80°C, 100°C, 150°C, 180°C, 200°C, 220°C or 250°C.
[0039] Preferably, the alkylation reaction time is 0.1-30 hours, for example 0.1 hours, 3 hours, 5 hours, 8 hours, 10 hours, 13 hours, 15 hours, 18 hours, 20 hours, 23 hours, 25 hours, 28 hours or 30 hours.
[0040] In the present invention, the alkylation reaction can be carried out under normal pressure, negative pressure or positive pressure.
[0041] When the organic nitrogen-containing compound contains two or more reactive nitrogens, the product can be a product in which all or part of the nitrogen is alkylated or a mixture of these products. For example, after the reaction of diaminodiphenylmethane and methyl diethylphosphinate, the products obtained can be compounds having structural formulas (III) and (IV) or a mixture of the two.
[0042] On the other hand, the present invention provides a flame retardant polymer material, which comprises a flame retardant and a polymer material, wherein the flame retardant comprises the dialkylphosphinate ammonium salt as described above.
[0043] Preferably, the flame retardant polymer material comprises 0.1-50 wt % of a flame retardant and 50-99.9 wt % of a polymer material.
[0044] In the present invention, the mass content of the flame retardant in the flame retardant polymer material is independently selected from any value among 0.1%, 0.2%, 0.5%, 0.8%, 1%, 1.2%, 1.5%, 2%, 2..2%, 2.5%, 3%, 3.5%, 4%, 5%, 6%, 8%, 10%, 15%, 20%, 30%, 40% or 50%, or any range value between two of them.
[0045] Preferably, the flame retardant polymer material also includes functional additives.
[0046] Preferably, the functional additive is selected from at least one of a reinforcing agent, an anti-dripping agent, a stabilizer, a pigment, a dye, a carbon-forming catalyst, a dispersant, a nucleating agent, an inorganic filler, an organic filler or an antioxidant.
[0047] Preferably, the reinforcing agent is selected from glass fibers.
[0048] Preferably, the anti-drip agent is selected from Teflon.
[0049] Preferably, the inorganic filler is selected from at least one of silicon dioxide, mica, calcium carbonate, aluminum oxide, aluminum nitride, talc, calcium oxide, calcium silicate, glass fiber powder or silica.
[0050] Preferably, the organic filler is selected from at least one of polytetrafluoroethylene powder, polyphenylene sulfide powder or polyethersulfone powder.
[0051] Preferably, the mass content of the functional additive in the flame retardant polymer material is 5-40%, for example, 5%, 8%, 10%, 15%, 18%, 20%, 25%, 28%, 30%, 33%, 35%, 38% or 40%.
[0052] Preferably, the flame retardant polymer material also includes a flame retardant Q.
[0053] Preferably, the flame retardant Q is selected from at least one of a phosphorus-based flame retardant, a nitrogen-based flame retardant or a boron-based flame retardant.
[0054] Preferably, the phosphorus-based flame retardant is selected from at least one of bisphosphates, phosphazenes, dialkyl phosphinates, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide derivatives (such as 6H-dibenzo[c,e][1,2]oxyphosphoglycerate, 6,6'-(1,2-ethanediyl)bis-6,6'-dioxide and HTP-6123 of Guizhou Yuanyi Group), and phosphine oxide compounds.
[0055] Preferably, the bisphosphate is selected from at least one of bisphenol A bisdiphenyl phosphate, resorcinol bisdiphenyl phosphate or 1,3-phenylene (2,6-xylyl) tetraphosphate.
[0056] Preferably, the phosphazene flame retardant is selected from at least one of hexaphenoxy cyclotriphosphazene, cyanophenoxyphosphazene (such as FP-300 of Fushimi Pharmaceutical Co., Ltd. of Japan), allyl cyclophosphazene (such as SPV-100 of Otsuka of Japan) or cyclic biphenyloxyphosphazene (such as BP-PZ of Otsuka of Japan).
[0057] Preferably, the dihydrocarbyl phosphinate is at least one selected from aluminum diethylphosphinate, aluminum diisobutylphosphinate, aluminum dipropylphosphinate, and zinc diethylphosphinate.
[0058] Preferably, the 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide derivative is selected from at least one of 6H-dibenzo[c,e][1,2]oxaphosphatinane-6,6'-(1,4-ethanediyl)bis-,6,6'-dioxide and 6H-dibenzo[c,e][1,2]oxaphosphatinane-6,6'-(1,4-phenylethanediyl)bis-,6,6'-dioxide.
[0059] Preferably, the phosphine oxide compound is p-xylylbisdiphenylphosphine oxide (eg PQ-60 from Jinyi Chemical).
[0060] Preferably, the nitrogen-based flame retardant is selected from at least one of melamine cyanurate, melamine polyphosphate or ammonium polyphosphate.
[0061] Preferably, the boron-based flame retardant is selected from zinc borate.
[0062] Preferably, the mass content of the flame retardant Q in the flame retardant polymer material is 0.5-20%, for example, 0.5%, 0.8%, 1%, 3%, 5%, 8%, 10%, 13%, 15%, 18% or 20%.
[0063] Preferably, the polymer material is selected from thermoplastic polymer resin or thermosetting resin.
[0064] Preferably, the thermoplastic polymer resin is selected from at least one of polybutadiene, polyamide, polyester, polyphenylene ether, acrylonitrile-butadiene-styrene copolymer, polyethylene, polypropylene, polyvinyl chloride, polystyrene, polyimide, polyphenylene sulfide or polyetheretherketone.
[0065] Preferably, the thermosetting resin is selected from at least one of vinyl polyphenylene ether resin, epoxy resin, cyanate resin, BT resin, bismaleimide resin, phenolic resin, polyurethane resin, thermosetting polyimide, unsaturated polyester resin, vinyl resin, benzoxazine resin, aromatic acetylene resin or furan resin.
[0066] Preferably, the thermosetting resin is at least one of vinyl polyphenylene ether resin, epoxy resin, cyanate resin, BT resin, bismaleimide resin, and thermosetting polyimide. Particularly preferably, the thermosetting resin is epoxy resin.
[0067] Preferably, the epoxy resin is selected from at least one of bisphenol A epoxy resin, bisphenol F epoxy resin, dicyclopentadiene epoxy resin, biphenyl epoxy resin or naphthol epoxy resin.
[0068] The epoxy resin described in the present invention includes but is not limited to epoxy resins currently available on the market.
[0069] Preferably, the flame retardant polymer material of the present invention is a flame retardant epoxy resin material, the flame retardant epoxy resin material comprises a flame retardant and an epoxy resin, and the flame retardant comprises the dialkyl phosphinate ammonium salt as described above.
[0070] Preferably, the flame retardant epoxy resin material comprises 0.1-18 wt % of dialkylphosphinate ammonium salt and 82-99.9 wt % of epoxy resin.
[0071] Preferably, the content of the flame retardant having the structure of formula (I) in the flame retardant material is 0.1%, 0.2%, 0.5%, 0.8%, 1%, 1.2%, 1.5%, 2%, 2.2%, 2.5%, 3%, 3.5%, 4%, 5%, 6%, 8%, 10%, 15%, 18% by weight, any value thereof, or a range value between any two of them.
[0072] Preferably, the flame retardant epoxy resin material further includes a functional additive;
[0073] Preferably, the functional additive is selected from at least one of a reinforcing agent, an anti-dripping agent, a stabilizer, a pigment, a dye, a carbon-forming catalyst, a dispersant, a nucleating agent, an inorganic filler, an organic filler or an antioxidant.
[0074] Preferably, the reinforcing agent is selected from glass fibers.
[0075] Preferably, the anti-drip agent is selected from Teflon.
[0076] Preferably, the inorganic filler is selected from at least one of silicon dioxide, mica, calcium carbonate, aluminum oxide, aluminum nitride, talc, calcium oxide, calcium silicate, glass fiber powder or silica.
[0077] Preferably, the organic filler is selected from at least one of polytetrafluoroethylene powder, polyphenylene sulfide powder or polyethersulfone powder.
[0078] Preferably, the mass content of the functional additive in the flame retardant epoxy resin material is 5-40%, for example, 5%, 8%, 10%, 15%, 18%, 20%, 25%, 28%, 30%, 33%, 35%, 38% or 40%.
[0079] The dialkyl ammonium hypophosphite salt prepared by the invention is simple to prepare and is suitable for industrial large-scale production. When the dialkyl ammonium hypophosphite salt is applied to epoxy resin, the flame retardant efficiency is high and the physical properties of the epoxy resin can be effectively maintained.
[0080] Compared with the prior art, the present invention has the following advantages:
[0081] The dialkylphosphinic acid ammonium salt of the present invention has a lower melting point than the solid amine used to prepare it, is easy to liquefy, has good compatibility with the resin, has a fast compatibility speed, and is easy to operate. It not only overcomes the problems of solid amines having a high melting point, being difficult to liquefy, and being difficult to be compatible with the resin system, but also overcomes the problems of corrosiveness caused by the dialkylphosphinic acid or its residue.
[0082] The dialkylphosphinate ammonium salt of the present invention as a flame retardant not only has high flame retardant efficiency but also can effectively maintain the physical properties of polymer materials, especially the glass transition temperature.
[0083] The dialkylphosphinate ammonium salt of the invention is simple to prepare, does not require a solvent and a catalyst, is a 1+1=2 reaction, has high atom economy, and is suitable for large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0084] Figure 1 This is the H NMR spectrum of DDM-MDP-1-2.
[0085] Figure 2 This is the H NMR spectrum of melamine-MDP-1-3.
[0086] Figure 3 This is the H NMR spectrum of TEPA-MDP-1-5. DETAILED DESCRIPTION
[0087] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0088] The raw materials used in the examples are as follows:
[0089] Melamine: Sinopharm Chemical Reagent Co., Ltd.
[0090] Dicyandiamide (DICY): Shanghai Aladdin Biochemical Technology Co., Ltd.
[0091] Diaminodiphenylmethane (DDM): Shanghai Aladdin Biochemical Technology Co., Ltd.
[0092] Tetraethylenepentamine (TEPA): Shanghai MacLean Biochemical Technology Co., Ltd.
[0093] Methyl diethylphosphite (MDP): Jiangsu Liside New Materials Co., Ltd.
[0094] E44 Epoxy Resin (DGEBA): Baling Petrochemical Co., Ltd.
[0095] Phenolic epoxy resin SQPN-O48 (F48): Shandong Shengquan Chemical Co., Ltd.
[0096] 2-Methylimidazole: Sane Chemical Technology (Shanghai) Co., Ltd.
[0097] N,N-Dimethylformamide (DMF): Shanghai Aladdin Biochemical Technology Co., Ltd.
[0098] Combustion test standard: GB / T 2408 2008 standard
[0099] Example 1 Preparation of a product of melamine and methyl diethylphosphinate in a 1 / 4 molar ratio
[0100] Melamine and diethyl methyl hypophosphite react at a molar ratio of 1:4. The specific reaction operation is as follows:
[0101] 2g (0.016mol) of melamine (melting point 354°C) and 13.9g (0.102mol) of diethyl methyl phosphite were mixed, reacted at 200°C for 6h, and the excess diethyl methyl phosphite was removed by vacuum distillation, and dried at 160°C in vacuo to obtain 10.5g (98.9%) of yellow viscous liquid, which was recorded as melamine-MDP-1-4. 1 H NMR, DMSO-d6 as solvent: 2.6-3.6 ppm (N-CH3, 12H), 1.3-2.0 ppm (- CH2 CH3, 16H), 0.8-1.2ppm(-CH2 CH3 , 24H). It has the following structure:
[0102]
[0103] Example 2 Preparation of a product of melamine and methyl diethylphosphinate in a 1 / 3 molar ratio
[0104] Melamine and diethyl methyl hypophosphite react at a molar ratio of 1:3. The specific reaction operation is as follows:
[0105] 10g (0.08mol) of melamine (melting point 354℃) was mixed with 32.35g (0.24mol) of diethyl methyl hypophosphite and reacted at 200℃ for 6h to obtain 36g (85.0%, transfer loss) of light yellow liquid. It was recorded as melamine-MDP-1-3. Figure 2 As shown, 1 H NMR, DMSO-d6 as solvent: 2.6-3.6 ppm (N-CH3, 9H), 1.3-2.0 ppm (- CH2 CH3, 12H), 0.8-1.2ppm(-CH2 CH3 , 18H). It has the following structure:
[0106]
[0107] Example 3 Preparation of a product of dicyandiamide and methyl diethylphosphinate in a 1 / 2 molar ratio
[0108] Dicyandiamide and diethyl methyl hypophosphite react at a molar ratio of 1:2. The specific reaction operation is as follows:
[0109] 5 g (0.06 mol) of dicyandiamide (209.5°C) was mixed with 17.8 g (0.13 mol) of diethyl methyl hypophosphite, reacted at 180-190°C for 4 h, and vacuum dried at 160°C to obtain 18.3 g (86.4%, transfer loss) of yellow transparent liquid, which was recorded as DICY-MDP-1-2. 1H NMR, DMSO-d6 as solvent: 2.6-3.7 ppm (N-CH3, 6H), 1.3-1.5 ppm (- CH2 CH3, 8H), 0.8-1.1ppm(-CH2 CH3 , 12H). It has the following structure:
[0110] mixture.
[0111] Example 4 Preparation of a product of dicyandiamide and methyl diethylphosphinate in a 1 / 3 molar ratio
[0112] Dicyandiamide and diethyl methyl hypophosphite react at a molar ratio of 1:3. The specific reaction operation is as follows:
[0113] 5 g (0.06 mol) of dicyandiamide (209.5°C) was mixed with 26.7 g (0.2 mol) of diethyl methyl hypophosphite, reacted at 190°C for 6 h, and dried under vacuum at 160°C to obtain 27.1 g (92.6%, transfer loss) of a yellow transparent liquid, which was recorded as DICY-MDP-1-3. 1 H NMR, DMSO-d6 as solvent: 2.6-3.7 ppm (N-CH3, 9H), 1.3-1.5 ppm (- CH2 CH3, 12H), 0.8-1.1ppm(-CH2 CH3 , 18H). It has the following structure:
[0114]
[0115] Example 5 Preparation of a product of diaminodiphenylmethane and diethylphosphinate in a 1 / 2 molar ratio
[0116] 4,4-Diaminodiphenylmethane and diethyl methyl hypophosphite react at a molar ratio of 1:2. The specific reaction operation is as follows:
[0117] 10g (0.05mol) 4,4-diaminodiphenylmethane (melting point 89-91℃) was mixed with 13.31g (0.10mol) diethyl methyl hypophosphite, heated at 160℃, reacted for about 1.5h, and 22.84g (98.0%) of wine red liquid was obtained. It was recorded as DDM-MDP-1-2. Figure 1 As shown, 1 H NMR, DMSO-d6 as solvent: 6.3-7.2 ppm (Ph-H, NH, 12H), 3.6 ppm (Ph-CH2-Ph, 2H): 2.8-3.0 ppm (N-CH3, 6H), 1.7 ppm (- CH2 CH3, 8H), 1.2ppm(-CH2 CH3 , 12H). It has the following structure:
[0118]
[0119] Example 6 Preparation of a product of diaminodiphenylmethane and ethyl diethylphosphinate in a 1 / 2 molar ratio
[0120] Preparation of ethyl diethyl hypophosphite: 100 g (0.6 mol) of triethyl orthoacetate and 75.2 g (0.6 mol) of diethyl hypophosphite were mixed, reacted at 100-110° C. for 20 h, and by-products were removed by distillation at 100° C. to obtain 88 g (97.8%) of ethyl diethyl hypophosphite (EDP). 1 H NMR, CDCl3 as solvent: 3.9 ppm (PO- CH2 CH3, 2H), 1.6ppm(- CH2 CH3, 4H), 1.2ppm(PO-CH2 CH3 , 3H), 1.1ppm(-CH2 CH3 , 6H). It has the structure shown below:
[0121]
[0122] 4,4-Diaminodiphenylmethane and diethyl phosphite were reacted in a molar ratio of 1:2. The specific reaction operation was as follows: 10g (0.05mol) of 4,4-diaminodiphenylmethane (melting point 89-91°C) was mixed with 14.82g (0.10mol) of diethyl phosphite, and heated at 200°C; reacted for about 3h to obtain 23.98g (97.0%) of wine red liquid. It was recorded as DDM-EDP-1-2. 1 H NMR, DMSO-d6 as solvent: 6.3-7.2 ppm (Ph-H, 8H), 3.6 ppm (Ph-CH2-Ph, 2H): 2.8-3.4 ppm (N- CH2 CH3, 4H), 1.7ppm(- CH2 CH3, 8H), 1.2ppm(-CH2 CH3 、N-CH2 CH3 , 18H). It has the following structure:
[0123]
[0124] Example 7 Preparation of a product of tetraethylenepentamine and methyl diethylphosphinate in a 1 / 5 molar ratio
[0125] Tetraethylenepentamine and diethyl methyl hypophosphite react at a molar ratio of 1:5. The specific reaction operation is as follows:
[0126] 5g (0.026mol) tetraethylenepentamine (melting point -40℃) was mixed with 17.4g (0.128mol) diethyl methyl hypophosphite, reacted at 150℃ for 1h, and dried under vacuum at 160℃ to obtain 20.28g (91.9%, transfer loss) of yellow transparent liquid. It was recorded as TEPA-MDP-1-5. Figure 3 As shown, 1 H NMR, DMSO-d6 as solvent: 2.0-4.0 ppm (N-CH3, -CH2CH2-, 31H), 1.3-1.5 ppm (- CH2 CH3, 20H), 0.8-1.1ppm(-CH2 CH3 , 30H). It has the following structure:
[0127]
[0128] Example 8
[0129] Heat 79.6 parts of epoxy resin DGEBA at 80℃, add 17.4 parts of 4,4-diaminodiphenylmethane (DDM) after it is fully softened, and stir quickly to promote the dissolution of DDM; add 3 parts of melamine-MDP-1-4 (prepared in Example 1) after most of DDM is dissolved, continue stirring for 1 minute to form a uniform mixed solution; pour the mixed solution into a mold preheated at 80℃ while hot, let it stand for 10 minutes, then heat it to 120℃ for pre-curing for 2 hours, and then heat it to 170℃ for curing for 4 hours. Cool it naturally to room temperature to obtain an EP / melamine-MDP-1-4 composite material with an addition amount of 3wt%. The sample thickness is 3.2mm. It reaches UL94 V0 grade. Tg 151℃. The results are shown in Table 1.
[0130] Example 9
[0131] Heat 80.4 parts of epoxy resin DGEBA at 80°C, add 17.6 parts of 4,4-diaminodiphenylmethane (DDM) after it is fully softened, and stir quickly to promote the dissolution of DDM; after most of the DDM is dissolved, add 2 parts of melamine-MDP-1-4 (prepared in Example 1), continue stirring for 1 minute, and form a uniform mixed solution; pour the mixed solution into a mold preheated at 80°C while hot, let it stand for 10 minutes, then heat it to 120°C for pre-curing for 2 hours, and then heat it to 170°C for curing for 4 hours. Cool it naturally to room temperature to obtain an EP / melamine-MDP-1-4 composite material with an addition amount of 2wt%. The sample thickness is 3.2mm. It reaches UL94 V1 grade. The results are shown in Table 1.
[0132] Example 10
[0133] Heat 79.6 parts of epoxy resin DGEBA at 80°C, add 17.4 parts of 4,4-diaminodiphenylmethane (DDM) after it is fully softened, and stir quickly to promote the dissolution of DDM; add 3 parts of melamine-MDP-1-3 (prepared in Example 2) after most of the DDM is dissolved, continue stirring for 1 minute to form a uniform mixed solution; pour the mixed solution into a mold preheated at 80°C while hot, let it stand for 10 minutes, then heat it to 120°C for pre-curing for 2 hours, and then heat it to 170°C for curing for 4 hours. Cool it naturally to room temperature to obtain an EP / melamine-MDP-1-3 composite material with an addition amount of 3wt%. The sample thickness is 3.2mm. It reaches UL94 V0 grade. Tg 150°C. The results are shown in Table 1.
[0134] Embodiment 11
[0135] Heat 80.4 parts of epoxy resin DGEBA at 80°C, add 17.6 parts of 4,4-diaminodiphenylmethane (DDM) after it is fully softened, and stir quickly to promote the dissolution of DDM; after most of the DDM is dissolved, add 2 parts of melamine-MDP-1-3 (prepared in Example 2), continue stirring for 1 minute, and form a uniform mixed solution; pour the mixed solution into a mold preheated at 80°C while hot, let it stand for 10 minutes, then heat it to 120°C for pre-curing for 2 hours, and then heat it to 170°C for curing for 4 hours. Cool it naturally to room temperature to obtain an EP / melamine-MDP-1-3 composite material with an addition amount of 2wt%. The sample thickness is 3.2mm. It reaches UL94 V1 grade. The results are shown in Table 1.
[0136] Example 12
[0137] Heat 79.6 parts of epoxy resin DGEBA at 80℃, add 17.4 parts of 4,4-diaminodiphenylmethane (DDM) after it is fully softened, and stir quickly to promote the dissolution of DDM; add 3 parts of DICY-MDP-1-2 (prepared in Example 3) after most of DDM is dissolved, continue stirring for 1 minute to form a uniform mixed solution; pour the mixed solution into a mold preheated at 80℃ while hot, let it stand for 10 minutes, then heat it to 120℃ for pre-curing for 2 hours, and then heat it to 170℃ for curing for 4 hours. Cool it naturally to room temperature to obtain an EP / DICY-MDP-1-2 composite material with an addition amount of 3wt%. The sample thickness is 3.2mm. It reaches UL94 V0 grade. Tg147℃. The results are shown in Table 1.
[0138] Embodiment 13
[0139] Heat 80.4 parts of epoxy resin DGEBA at 80°C, add 17.6 parts of 4,4-diaminodiphenylmethane (DDM) after it is fully softened, and stir quickly to promote the dissolution of DDM; after most of the DDM is dissolved, add 2 parts of DICY-MDP-1-2 (prepared in Example 3), continue stirring for 1 minute, and form a uniform mixed solution; pour the mixed solution into a mold preheated at 80°C while hot, let it stand for 10 minutes, then heat it to 120°C for pre-curing for 2 hours, and then heat it to 170°C for curing for 4 hours. Cool it naturally to room temperature to obtain an EP / DICY-MDP-1-2 composite material with an addition amount of 2wt%. The sample thickness is 3.2mm. It reaches UL94 V1 grade. The results are shown in Table 1.
[0140] Embodiment 14
[0141] Heat 80.4 parts of epoxy resin DGEBA at 80℃, add 17.6 parts of 4,4-diaminodiphenylmethane (DDM) after it is fully softened, and stir quickly to promote the dissolution of DDM; after most of the DDM is dissolved, add 2 parts of DICY-MDP-1-3 (prepared in Example 4), continue stirring for 1 minute, and form a uniform mixed solution; pour the mixed solution into a mold preheated at 80℃ while hot, let it stand for 10 minutes, then heat it to 120℃ for pre-curing for 2 hours, and then heat it to 170℃ for curing for 4 hours. Cool it naturally to room temperature to obtain an EP / DICY-MDP-1-3 composite material with an addition amount of 2wt%. The sample thickness is 3.2mm. It reaches UL94 V0 grade. Tg153℃. The results are shown in Table 1.
[0142] Embodiment 15
[0143] Heat 81.3 parts of epoxy resin DGEBA at 80°C, add 17.7 parts of 4,4-diaminodiphenylmethane (DDM) after it is fully softened, and stir quickly to promote the dissolution of DDM; add 1 part of DICY-MDP-1-3 (prepared in Example 4) after most of the DDM is dissolved, and continue stirring for 1 minute to form a uniform mixed solution; pour the mixed solution into a mold preheated at 80°C while hot, let it stand for 10 minutes, then heat it to 120°C for pre-curing for 2 hours, and then heat it to 170°C for curing for 4 hours. Cool it naturally to room temperature to obtain an EP / DICY-MDP-1-3 composite material with an addition amount of 1wt%. The sample thickness is 3.2mm. It reaches UL94 V1 grade. The results are shown in Table 1.
[0144] Example 16
[0145] Heat 78.8 parts of epoxy resin DGEBA at 80℃, add 17.2 parts of 4,4-diaminodiphenylmethane (DDM) after it is fully softened, and stir quickly to promote the dissolution of DDM; add 4 parts of DDM-MDP-1-2 (prepared in Example 5) after most of DDM is dissolved, continue stirring for 1 minute to form a uniform mixed solution; pour the mixed solution into a mold preheated at 80℃ while hot, let it stand for 10 minutes, then heat it to 120℃ for pre-curing for 2 hours, and then heat it to 170℃ for curing for 4 hours. Cool it naturally to room temperature to obtain an EP / DDM-MDP-1-2 composite material with an addition amount of 4wt%. The sample thickness is 3.2mm. It reaches UL94 V0 grade. Tg145℃. The results are shown in Table 1.
[0146] Embodiment 17
[0147] Heat 79.6 parts of epoxy resin DGEBA at 80°C, add 17.4 parts of 4,4-diaminodiphenylmethane (DDM) after it is fully softened, and stir quickly to promote the dissolution of DDM; after most of the DDM is dissolved, add 3 parts of DDM-MDP-1-2 (prepared in Example 5), continue stirring for 1 minute, and form a uniform mixed solution; pour the mixed solution into a mold preheated at 80°C while hot, let it stand for 10 minutes, then heat it to 120°C for pre-curing for 2 hours, and then heat it to 170°C for curing for 4 hours. Cool it naturally to room temperature to obtain an EP / DDM-MDP-1-2 composite material with an addition amount of 3wt%. The sample thickness is 3.2mm. It reaches UL94 V1 grade. The results are shown in Table 1.
[0148] Embodiment 18
[0149] Heat 81.0 parts of epoxy resin DGEBA to 80°C, add 15.0 parts of 4,4-diaminodiphenylmethane (DDM) after it is fully softened, and stir quickly to promote the dissolution of DDM; after most of the DDM is dissolved, add 4 parts of DDM-MDP-1-2 (prepared in Example 5, replacing part of DDM according to the functionality of 4), continue stirring for 1 minute, and form a uniform mixed solution; pour the mixed solution into a mold preheated at 80°C while hot, let it stand for 10 minutes, then heat it to 120°C for pre-curing for 2 hours, and then heat it to 170°C for curing for 4 hours. Cool naturally to room temperature to obtain an EP / DDM-MDP-1-2-react-4 composite material with an addition amount of 4wt%. Reach UL94 V0 grade. Use dichloromethane for Soxhlet extraction. After 24 hours, the extract is 1 H and 31 P NMR examination showed that DDM-MDP-1-2 was not found, indicating that DDM-MDP-1-2 was involved in the curing.
[0150] Embodiment 19
[0151] Heat 80.1 parts of epoxy resin DGEBA at 80°C, add 16.9 parts of 4,4-diaminodiphenylmethane (DDM) after it is fully softened, and stir quickly to promote the dissolution of DDM; after most of the DDM is dissolved, add 3 parts of DDM-MDP-1-2 (prepared in Example 2, replacing part of DDM according to the functionality of 2), continue stirring for 1 minute, and form a uniform mixed solution; pour the mixed solution into a mold preheated at 80°C while hot, let it stand for 10 minutes, then heat it to 120°C for pre-curing for 2 hours, and then heat it to 180°C for curing for 4 hours. Cool it naturally to room temperature to obtain an EP / DDM-MDP-1-2-react-2 composite material with an addition amount of 3wt%. Reach UL94 V0 grade. Tg 150°C. The results are shown in Table 1.
[0152] Embodiment 20
[0153] Heat 78.8 parts of epoxy resin DGEBA at 80℃, add 17.2 parts of 4,4-diaminodiphenylmethane (DDM) after it is fully softened, and stir quickly to promote the dissolution of DDM; add 4 parts of DDM-EDP-1-2 (prepared in Example 6) after most of DDM is dissolved, continue stirring for 1 minute to form a uniform mixed solution; pour the mixed solution into a mold preheated at 80℃ while hot, let it stand for 10 minutes, then heat it to 120℃ for pre-curing for 2 hours, and then heat it to 170℃ for curing for 4 hours. Cool it naturally to room temperature to obtain an EP / DDM-EDP-1-2 composite material with an addition amount of 4wt%. The sample thickness is 3.2mm. It reaches UL94 V0 grade. Tg146℃. The results are shown in Table 1.
[0154] Embodiment 21
[0155] Heat 79.6 parts of epoxy resin DGEBA at 80℃, add 17.2 parts of 4,4-diaminodiphenylmethane (DDM) after it is fully softened, and stir quickly to promote the dissolution of DDM; add 3 parts of DDM-EDP-1-2 (prepared in Example 6) after most of DDM is dissolved, continue stirring for 1 minute to form a uniform mixed solution; pour the mixed solution into a mold preheated at 80℃ while hot, let it stand for 10 minutes, then heat it to 120℃ for pre-curing for 2 hours, and then heat it to 170℃ for curing for 4 hours. Cool it naturally to room temperature to obtain an EP / DDM-EDP-1-2 composite material with an addition amount of 3wt%. The sample thickness is 3.2mm. It reaches UL94 V1 grade. The results are shown in Table 1.
[0156] Embodiment 22
[0157] Heat 79.6 parts of epoxy resin DGEBA at 80°C, add 17.4 parts of 4,4-diaminodiphenylmethane (DDM) after it is fully softened, and stir quickly to promote the dissolution of DDM; add 3 parts of TEPA-MDP-1-5 (prepared in Example 7) after most of DDM is dissolved, continue stirring for 1 minute to form a uniform mixed solution; pour the mixed solution into a mold preheated at 80°C while hot, let it stand for 10 minutes, then heat it to 120°C for pre-curing for 2 hours, and then heat it to 170°C for curing for 4 hours. Cool it naturally to room temperature to obtain an EP / TEPA-MDP-1-5 composite material with an addition amount of 3wt%. The sample thickness is 3.2mm. It reaches UL94 V0 grade. Tg148°C. The results are shown in Table 1.
[0158] Embodiment 23
[0159] Heat 80.4 parts of epoxy resin DGEBA at 80°C, add 17.6 parts of 4,4-diaminodiphenylmethane (DDM) after it is fully softened, and stir quickly to promote the dissolution of DDM; after most of the DDM is dissolved, add 2 parts of TEPA-MDP-1-5 (prepared in Example 7), continue stirring for 1 minute, and form a uniform mixed solution; pour the mixed solution into a mold preheated at 80°C while hot, let it stand for 10 minutes, then heat it to 120°C for pre-curing for 2 hours, and then heat it to 170°C for curing for 4 hours. Cool it naturally to room temperature to obtain an EP / TEPA-MDP-1-5 composite material with an addition amount of 2wt%. The sample thickness is 3.2mm. It reaches UL94 V1 grade. The results are shown in Table 1.
[0160] Embodiment 24
[0161] 83.2 parts of F48 epoxy resin, 8.7 parts of dicyandiamide, 0.1 parts of 2-methylimidazole, and 8 parts of DICY-MDP-1-3 (prepared in Example 4) were mixed, and N, N-dimethylformamide (DMF) of the same mass as dicyandiamide was added to promote dissolution, and heated and stirred at 100°C. After forming a uniform solution, DMF was removed in a vacuum oven at 100°C. Finally, the mixed solution was poured into a mold preheated at 100°C, pre-cured at 130°C for 1h, and cured at 170°C for 4h to obtain an EP-F48 / DICY-MDP-1-3 composite material with an addition amount of 8%. The sample thickness was 3.2mm. It reached UL94 V0 grade. The results are shown in Table 1.
[0162] Embodiment 25
[0163] 83.2 parts of F48 epoxy resin, 8.7 parts of dicyandiamide, 0.1 parts of 2-methylimidazole, and 8 parts of TEPA-MDP-1-5 (prepared in Example 7) were mixed, and N, N-dimethylformamide (DMF) of the same mass as dicyandiamide was added to promote dissolution, and heated and stirred at 100°C. After forming a uniform solution, DMF was removed in a vacuum oven at 100°C. Finally, the mixed solution was poured into a mold preheated at 100°C, pre-cured at 130°C for 1h, and cured at 170°C for 4h to obtain an EP-F48 / TEPA-MDP-1-5 composite material with an addition amount of 8%. The sample thickness was 3.2mm. It reached the UL94 V0 grade. The results are shown in Table 1.
[0164] Embodiment 26
[0165] After polypropylene (PP) was dried in a blast oven at 80°C for 4 hours, 80 parts of PP and 20 parts of DICY-MDP-1-3 (prepared in Example 4) were melted in an internal mixer at a speed of 50 r / min, and the temperature was set to 200°C. After 6 minutes, the mixture was taken out for cooling and drying. The mixture was then filled into a mold, preheated for 10 minutes in a flat vulcanizer at 200°C, maintained at 10 MPa for 5 minutes, and then cold pressed. After cooling, the sample was cut and tested, and the sample thickness was 3.2 mm. UL94 V0 grade.
[0166] Comparative Example 1
[0167] 4,4-Diaminodiphenylmethane, diethyl hypophosphorous acid 1:2 reaction: Add 5g (0.025mol) of 4,4-diaminodiphenylmethane in batches to 5.97g (0.049mol) of diethyl hypophosphorous acid, and react at 80-100℃. The reaction is complete when 4,4-diaminodiphenylmethane is completely dissolved. 10.4g (94.8%, transfer loss) of yellow liquid product DDM-DEP-1-2 is obtained, which slowly crystallizes at room temperature to form a yellow-green solid. It is very easy to absorb moisture in the air and is inconvenient to use. 1 H NMR: 7.0ppm (Ph-H, 4H), 6.8ppm (NH, 6H), 6.7ppm (Ph-H, 4H), 3.8ppm (Ph-CH2-Ph, 2H), 1.7ppm (- CH2 CH3, 8H), 1.2ppm(-CH2 CH3 , 12H). It has the following structure:
[0168]
[0169] Comparative Example 2
[0170] Melamine, diethylphosphite 1:3 reaction: 5g (0.04mol) melamine was mixed with 14.51g (0.12mol) diethylphosphite, and reacted at 190-200℃ for 2h to obtain 17.55g (89.9%, transfer loss) of light yellow paste solid melamine-DEP-1-3. It has very poor compatibility with DGEBA, and most of melamine-DEP-1-3 exists in EP in solid form after curing. 1 H NMR: 6.0-11.0ppm (NH, 9H), 1.3-1.5ppm (- CH2 CH3, 12H), 0.8-1.1ppm(-CH2 CH3 , 18H). It has the following structure:
[0171]
[0172] Comparative Example 3
[0173] Dicyandiamide, diethyl hypophosphorous acid 1:2 reaction: 5g (0.07mol) dicyandiamide was mixed with 14.51g (0.12mol) diethyl hypophosphorous acid, and reacted at 100℃. Alkaline gas was detected in the tail gas with pH test paper. The nuclear magnetic resonance results showed that the mixture after the reaction was a mixture of dicyandiamide, diethyl hypophosphorous acid, and the product DICY-DEP-1-2, with a large amount of by-products. It was impossible to obtain a pure DICY-DEP-1-2 product.
[0174] Comparative Example 4
[0175] Dicyandiamide and diethylphosphorous acid react in a ratio of 1:2: 5 g (0.07 mol) of dicyandiamide and 14.51 g (0.12 mol) of diethylphosphorous acid are mixed and dissolved in 30 g of water. After reacting at 70°C for 30 min, a DICY-DEP-1-2 aqueous solution is obtained. The water is evaporated at 70°C to decompose the product. 31 The peak of diethyl hypophosphorous acid reappeared in the P NMR results, indicating that diethyl hypophosphorous acid was regenerated.
[0176] Comparative Example 5
[0177] Tetraethylenepentamine and diethylphosphorous acid in a ratio of 1:5: 5 g (0.03 mol) of tetraethylenepentamine was mixed with 15.31 g (0.12) of diethylphosphorous acid and heated to 100°C. A large amount of alkaline gas was detected in the tail gas using pH test paper, and the pure TEPA-DEP-1-5 product could not be obtained.
[0178] Comparative Example 6
[0179] Heat 82.1 parts of epoxy resin DGEBA at 80℃, add 17.9 parts of 4,4-diaminodiphenylmethane (DDM) after it is fully softened, and stir quickly to promote the dissolution of DDM; after DDM is completely dissolved, pour the mixture into the mold preheated at 80℃ while it is hot, let it stand for 10 minutes, then heat it to 120℃ for pre-curing for 2 hours, and then heat it to 170℃ for curing for 4 hours. Cool it naturally to room temperature to obtain pure EP material. The sample thickness is 3.2mm. UL94 NR grade. Tg 149℃. The results are shown in Table 1.
[0180] Comparative Example 7
[0181] Heat 79.6 parts of epoxy resin DGEBA at 80°C, add 17.4 parts of 4,4-diaminodiphenylmethane (DDM) after it is fully softened, and stir quickly to promote the dissolution of DDM; after most of the DDM is dissolved, add 3 parts of melamine-DEP-1-3 (prepared in Comparative Example 2), continue stirring for 1 minute, and form a uniform mixed solution; pour the mixed solution into a mold preheated at 80°C while hot, let it stand for 10 minutes, then heat it to 120°C for pre-curing for 2 hours, and then heat it to 170°C for curing for 4 hours. Cool it naturally to room temperature to obtain an EP / melamine-DEP-1-3 composite material with an addition amount of 3wt%. The sample thickness is 3.2mm. It reaches UL94 V1 grade. The results are shown in Table 1.
[0182] Comparative Example 8
[0183] Heat 79.6 parts of epoxy resin DGEBA at 80°C, add 17.4 parts of 4,4-diaminodiphenylmethane (DDM) after it is fully softened, and stir quickly to promote the dissolution of DDM; add 3 parts of DDM-DEP-1-2 (prepared in Comparative Example 1) after most of the DDM is dissolved, continue stirring for 1 minute to form a uniform mixed solution; pour the mixed solution into a mold preheated at 80°C while hot, let it stand for 10 minutes, then heat it to 120°C for pre-curing for 2 hours, and then heat it to 170°C for curing for 4 hours. Cool it naturally to room temperature to obtain an EP / DDM-DEP-1-2 composite material with an addition amount of 3wt%. The sample thickness is 3.2mm. It reaches UL94 V0 grade. Tg153°C. The results are shown in Table 1.
[0184] Comparative Example 9
[0185] 90.4 parts of F48 epoxy resin, 9.5 parts of dicyandiamide, and 0.1 parts of 2-methylimidazole were mixed, and N,N-dimethylformamide (DMF) of the same mass as dicyandiamide was added to promote dissolution, and heated and stirred at 100°C. After forming a uniform solution, DMF was removed in a vacuum oven at 100°C. Finally, the mixed solution was poured into a mold preheated at 100°C, pre-cured at 130°C for 1h, and cured at 170°C for 4h to obtain pure EP-F48. The sample thickness was 3.2mm. UL94 NR grade. The results are shown in Table 1.
[0186] Comparative Example 10
[0187] After 100 parts of polypropylene (PP) were dried in a blast oven at 80℃ for 4 hours, the PP was melted in an internal mixer with a speed of 50r / min, and the temperature was set to 200℃. After 6 minutes, it was taken out for cooling and drying. Then the PP was filled into the mold, preheated in a flat vulcanizer at 200℃ for 10 minutes, maintained at 10MPa for 5 minutes, and then cold pressed. After cooling, the sample was cut and tested. The sample thickness was 3.2mm. UL94NR grade.
[0188] Example 18 uses a flame retardant prepared with DDM as a raw material, and uses it as a reactive additive to replace part of the curing agent DDM. After Soxhlet extraction of the cured sample, no flame retardant DDM-MDP-1-2 was detected in the extract, indicating that DDM-MDP-1-2 can participate in the curing of epoxy resin and can be used as a reactive flame retardant.
[0189] Comparative Example 7 and Examples 8 to 11 all use flame retardants prepared using melamine as a raw material, but the flame retardant efficiency of the reaction product of methyl diethylphosphinate and melamine is obviously higher than the flame retardant efficiency of the neutralization product of diethylphosphinic acid and melamine prepared in Comparative Example 2, although the former has a lower phosphorus content, which is very unexpected.
[0190] Comparative Example 8 and Examples 16, 17, and 19 all use flame retardants prepared using DDM as raw material. The flame retardant efficiency of the flame retardant of the present invention is comparable to the product of diethylphosphinic acid and DDM neutralized by Comparative Example 1, but the latter easily absorbs moisture and is inconvenient to store and use.
[0191] Examples 12-15, 22, and 23 show that the product of the reaction of diethylphosphinate with DICY and TEPA also has a very high flame retardant efficiency. Example 14 only uses 2 parts of the flame retardant of the present invention, which reaches V0, and even using 1 part (Example 15) can significantly make the epoxy resin reach V1 level. However, the neutralization product corresponding to diethylphosphinate cannot be obtained due to the acid hydrolysis reaction of DICY and TEPA during the synthesis process (Comparative Examples 3, 4, and 5), which shows the superiority of diethylphosphinate instead of diethylphosphinate.
[0192] The comparison between Comparative Example 9 and Examples 24 and 25 shows that the flame retardant of the present invention has good flame retardant properties in phenolic epoxy resin, and the flame retardant requirements can be met when the addition amount is less than 10%. Example 26 is the application of the flame retardant of the present invention in polypropylene (PP). The flame retardant prepared using DICY as the raw material can make PP pass the UL94 test at an addition amount of 20%. It shows the wide application of the flame retardant of the present invention in polymer materials such as epoxy resin and polyolefin.
[0193] Table 1 Application of dialkyl ammonium hypophosphite in epoxy resin
[0194]
[0195]
[0196]
[0197]
[0198] The applicant declares that the present invention uses the above-mentioned embodiments to illustrate the dialkylphosphinate ammonium salt and its preparation method and application, but the present invention is not limited to the above-mentioned embodiments, that is, it does not mean that the present invention must rely on the above-mentioned embodiments to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the raw materials selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A dialkylphosphinate ammonium salt, It is characterized in that The dialkylphosphinate ammonium salt is obtained by alkylating a dialkylphosphinate alkyl ester having a structural formula shown in formula (I) with nitrogen on at least two non-tertiary amine structures in an organic nitrogen-containing compound, wherein the alkyl group involved in the alkylation reaction comes from R in the structural formula shown in formula (I). 1 The organic nitrogen-containing compound comprises one or a combination of at least two of ethylenediamine, propylenediamine, butylenediamine, pentanediamine, hexanediamine, heptanediamine, octanediamine, 1,4-cyclohexanediamine, m-phenylenediamine, p-phenylenediamine, piperazine, 2-methylpiperazine, 2-methylimidazole, tetraethylenepentamine, triethylenetetramine, diaminodiphenylmethane, 2,2-bis(4-aminophenyl)propane, diaminodiphenylsulfone, diaminobenzophenone, melamine or dicyandiamide; at least one nitrogen atom in the dialkylphosphinate ammonium salt that has undergone an alkylation reaction has an H atom and an R atom obtained by the alkylation reaction. 1 Group; R 1 Any one selected from methyl, ethyl, propyl or butyl; R 2 , R 3 Independently selected from any one of ethyl, propyl or butyl.
2. The dialkylphosphinate ammonium salt according to claim 1, It is characterized in that R 1 Any one selected from methyl and ethyl.
3. The dialkylphosphinate ammonium salt according to claim 1, It is characterized in that R 2 , R 3 It is ethyl.
4. The dialkylphosphinate ammonium salt according to claim 1, It is characterized in that The dihydrocarbyl phosphinate alkyl ester includes one or a combination of at least two of diethyl phosphinate methyl, dipropyl phosphinate methyl, ethyl propyl phosphinate, diethyl phosphinate ethyl, dipropyl phosphinate ethyl, ethyl propyl phosphinate ethyl, diethyl phosphinate propyl, dipropyl phosphinate propyl or ethyl propyl phosphinate propyl.
5. The dialkylphosphinate ammonium salt according to claim 1, It is characterized in that The dialkylphosphinate ammonium salt has any one of the following structures: Among them, R 1 , R 2 , R 3 Same as defined in claim 1.
6. A method for preparing a dialkylphosphinate ammonium salt according to any one of claims 1 to 5, It is characterized in that The preparation method comprises the following steps: The dialkylphosphinate alkyl ester and the nitrogen on at least two non-tertiary amine structures in the organic nitrogen-containing compound undergo alkylation reaction to obtain the dialkylphosphinate ammonium salt.
7. The preparation method according to claim 6, It is characterized in that The dihydrocarbyl phosphinate alkyl ester includes any one or a combination of two of diethyl phosphinate methyl, dipropyl phosphinate methyl, ethyl propyl phosphinate, diethyl phosphinate ethyl, dipropyl phosphinate ethyl, ethyl propyl phosphinate ethyl, diethyl phosphinate propyl, dipropyl phosphinate propyl or ethyl propyl phosphinate propyl.
8. The preparation method according to claim 6, It is characterized in that The molar ratio of the sum of the moles of nitrogen in the organic nitrogen-containing compound to the alkyl dihydrocarbyl phosphinate is 10 / 1-1 / 10.
9. The preparation method according to claim 6, It is characterized in that The alkylation reaction temperature is 0-250°C.
10. The preparation method according to claim 6, It is characterized in that The alkylation reaction time is 0.1-30 hours.
11. A flame retardant polymer material, It is characterized in that The flame retardant polymer material comprises a flame retardant and a polymer material, and the flame retardant comprises the dialkylphosphinate ammonium salt according to any one of claims 1 to 5.
12. The flame retardant polymer material according to claim 11, It is characterized in that The flame retardant polymer material comprises 0.1-50 wt % of a flame retardant and 50-99.9 wt % of a polymer material.
13. The flame retardant polymer material according to claim 11, It is characterized in that The flame retardant polymer material also includes functional additives.
14. The flame retardant polymer material according to claim 13, It is characterized in that The functional additive is selected from at least one of a reinforcing agent, an anti-dripping agent, a stabilizer, a pigment, a dye, a carbon-forming catalyst, a dispersant, a nucleating agent, an inorganic filler, an organic filler or an antioxidant.
15. The flame retardant polymer material according to claim 14, It is characterized in that The reinforcing agent is selected from glass fibers.
16. The flame retardant polymer material according to claim 14, It is characterized in that The anti-drip agent is selected from Teflon.
17. The flame retardant polymer material according to claim 14, It is characterized in that The inorganic filler is selected from at least one of silicon dioxide, mica, calcium carbonate, aluminum oxide, aluminum nitride, talc, calcium oxide, calcium silicate, glass fiber powder or silica.
18. The flame retardant polymer material according to claim 14, It is characterized in that The organic filler is selected from at least one of polytetrafluoroethylene powder, polyphenylene sulfide powder or polyethersulfone powder.
19. The flame retardant polymer material according to claim 13, It is characterized in that The mass content of the functional additive in the flame retardant polymer material is 5-40%.
20. The flame retardant polymer material according to claim 11, It is characterized in that The flame retardant polymer material further includes a flame retardant Q, and the flame retardant Q is selected from at least one of a phosphorus flame retardant, a nitrogen flame retardant or a boron flame retardant.
21. The flame retardant polymer material according to claim 20, It is characterized in that The phosphorus-based flame retardant is selected from at least one of bisphosphates, phosphazenes, dialkyl phosphinates, 6H-dibenzo[c,e][1,2]oxyphosphoglycerate, 6H-dibenzo[c,e][1,2]oxaphosphatin-6,6'-(1,4-ethanediyl)bis-,6,6'-dioxide, 6H-dibenzo[c,e][1,2]oxaphosphatin-6,6'-(1,4-phenylethanediyl)bis-,6,6'-dioxide, HTP-6123, and phosphine oxide compounds.
22. The flame retardant polymer material according to claim 21, It is characterized in that The bisphosphate is selected from at least one of bisphenol A bisdiphenyl phosphate, resorcinol bisdiphenyl phosphate or 1,3-phenylene (2,6-xylyl) tetraphosphate.
23. The flame retardant polymer material according to claim 21, It is characterized in that The phosphazene flame retardant is selected from at least one of hexaphenoxy cyclotriphosphazene, cyanophenoxyphosphazene, allyl cyclophosphazene or cyclic biphenyloxyphosphazene.
24. The flame retardant polymer material according to claim 21, It is characterized in that The dihydrocarbyl phosphinate is at least one selected from the group consisting of aluminum diethylphosphinate, aluminum diisobutylphosphinate, aluminum dipropylphosphinate, and zinc diethylphosphinate.
25. The flame retardant polymer material according to claim 21, It is characterized in that The phosphine oxide compound is p-xylylbisdiphenylphosphine oxide.
26. The flame retardant polymer material according to claim 20, It is characterized in that The nitrogen-based flame retardant is selected from at least one of melamine cyanurate, melamine polyphosphate or ammonium polyphosphate.
27. The flame retardant polymer material according to claim 20, It is characterized in that The boron flame retardant is selected from zinc borate.
28. The flame retardant polymer material according to claim 20, It is characterized in that The mass content of the flame retardant Q in the flame retardant polymer material is 0.5-20%.
29. The flame retardant polymer material according to claim 12, It is characterized in that The polymer material is selected from thermoplastic polymer resin or thermosetting resin.
30. The flame retardant polymer material according to claim 29, It is characterized in that The thermoplastic polymer resin is selected from at least one of polybutadiene, polyamide, polyester, polyphenylene ether, acrylonitrile-butadiene-styrene copolymer, polyethylene, polypropylene, polyvinyl chloride, polystyrene, polyimide, polyphenylene sulfide or polyetheretherketone.
31. The flame retardant polymer material according to claim 29, It is characterized in that The thermosetting resin is selected from at least one of vinyl polyphenylene ether resin, epoxy resin, cyanate resin, BT resin, bismaleimide resin, phenolic resin, polyurethane resin, thermosetting polyimide, unsaturated polyester resin, vinyl resin, benzoxazine resin, aromatic acetylene resin or furan resin.
32. The flame retardant polymer material according to claim 29, It is characterized in that The thermosetting resin is at least one of vinyl polyphenylene ether resin, epoxy resin, cyanate resin, BT resin, bismaleimide resin, and thermosetting polyimide.
33. The flame retardant polymer material according to claim 32, It is characterized in that The thermosetting resin is epoxy resin.
34. The flame retardant polymer material according to claim 33, It is characterized in that The epoxy resin is selected from at least one of bisphenol A epoxy resin, bisphenol F epoxy resin, dicyclopentadiene epoxy resin, biphenyl epoxy resin or naphthol epoxy resin.
35. The flame retardant polymer material according to any one of claims 11 to 34, It is characterized in that The flame retardant polymer material is a flame retardant epoxy resin material, the flame retardant epoxy resin material comprises a flame retardant and an epoxy resin, and the flame retardant comprises the dialkyl phosphinate ammonium salt according to any one of claims 1 to 5.
36. The flame retardant polymer material according to claim 35, It is characterized in that The flame retardant epoxy resin material comprises 0.1-18 wt % of dialkylphosphinate ammonium salt and 82-99.9 wt % of epoxy resin.
Citation Information
Patent Citations
Reactive flame retardants for flexible polyurethane foams
CN110945047A
Phosphorus-nitrogen complex salts, their preparation methods, flame retardants, and their applications
CN113929967B
Method for the production of polyisocyanates comprising isocyanurate groups and their use
EP3470444A1
Flame retardant epoxy resin composition
WO2021074684A1
Process for producing phosphinic acid esters
CN104159906A