Aluminum ion-based all-solid-state electrochromic device and preparation method thereof

The all-solid-state electrochromic device is formed in the aluminum ion-based electrochromic device through magnetron sputtering technology, which solves the leakage problem of liquid or semi-liquid devices in the existing technology and achieves improvement in stability and industrial application.

CN117270273BActive Publication Date: 2024-10-01深圳豪威显示科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310703825.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-14
Publication Date
2024-10-01
Estimated Expiration
2043-06-14

AI Technical Summary

Technical Problem

Existing aluminum ion-based electrochromic devices are mainly liquid or semi-liquid, making it difficult to prepare a fully solid form. The packaging process is complex and there are leakage problems, which limits their industrial application.

Method used

Magnetron sputtering technology is used to deposit a NiO derivative film on a transparent conductive layer as an ion storage layer. An aluminum salt ceramic target is used to deposit a solid electrolyte film containing aluminum ions. It is formed by combining a tungsten target to deposit an electrochromic layer and a transparent conductive electrode target. The top transparent conductive layer is used to prepare an aluminum ion-based all-solid-state electrochromic device.

Benefits of technology

The preparation of aluminum ion-based all-solid-state electrochromic devices is achieved, which reduces the packaging process requirements, avoids leakage, improves the stability and industrialization potential of the device, and the process conditions are mild and the process is simple.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117270273B_ABST
    Figure CN117270273B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of electrochromic materials, and specifically discloses an aluminum ion-based all-solid-state electrochromic device and a preparation method thereof. The present invention first uses an alloy nickel target to deposit an ion storage layer on a bottom transparent conductive layer; then deposits a solid electrolyte film containing aluminum ions on the ion storage layer through an aluminum salt ceramic target to obtain an ion conduction layer; then uses a tungsten target to deposit an electrochromic layer on the ion conduction layer; finally, uses a transparent conductive electrode target to deposit a transparent conductive film to form a top transparent conductive layer to obtain an aluminum ion-based all-solid-state electrochromic device. The aluminum ion-based all-solid-state electrochromic device prepared by the present invention uses aluminum ions as transmission ions to replace lithium ions used in traditional electrochromic devices, and completes the charge transfer and balance between the anode and cathode in the electrochromic device. Selecting WO3 and NiO composite thin film materials helps to improve the cycle stability of all-solid-state electrochromism.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of electrochromic materials, and in particular to an aluminum ion-based all-solid-state electrochromic device and a preparation method thereof. Background Art

[0002] Electrochromism refers to the phenomenon that the optical properties of a material (reflectivity, transmittance, absorptivity, etc.) undergo stable and reversible color changes under the action of an external electric field, which is manifested in the appearance of reversible changes in color and transparency. Electrochromic devices made of electrochromic materials are widely used in various fields, such as: electrochromic smart glass has the adjustability of light absorption and transmission under the action of an electric field, can selectively absorb or reflect external thermal radiation and reduce internal heat diffusion, and reduce the large amount of energy that must be consumed to keep office buildings and residential buildings cool in summer and warm in winter. At the same time, it improves the degree of natural light and prevents peeping, solving the problem of modern urban light pollution that is worsening. Electrochromic glass usually consists of 5 layers, namely transparent conductive layer, ion storage layer, ion conduction layer (electrolyte), electrochromic layer, transparent conductive layer, etc.

[0003] The transport ions that are currently widely studied are lithium ions (Li + ), which has the advantages of small ion radius (0.059 nm), fast migration rate, and low driving voltage. However, the content of lithium salt in the earth's crust is relatively low, resulting in high price and complicated subsequent recycling and treatment procedures, which greatly limits the development of lithium-ion-based electrochromic devices. People have turned their attention to multivalent ions - aluminum ions (Al 3+ ), first, the radius of aluminum ions is equivalent to that of lithium ions, which is 0.054nm. Secondly, when the same amount of lithium ions and aluminum ions are injected into the electrochromic layer, the amount of electrons introduced by aluminum ions is three times that of lithium ions. Therefore, it is reasonable to speculate that aluminum ion electrochromic devices have faster response speed, higher contrast and stability. In addition, aluminum salts are abundant in the earth and are environmentally friendly. Introducing aluminum ions into electrochromic devices has great development prospects.

[0004] At present, there are patents related to electrochromic devices using aluminum ions as transmission ions, such as Chinese patent application CN110376816A discloses a self-powered tungsten oxide-based electrochromic device based on aluminum ion hydrogel and its preparation method, which uses polyacrylamide hydrogel to infiltrate aluminum chloride solution to prepare aluminum chloride hydrogel, and on this basis, prepares an electrochromic device; Chinese patent application CN109634019A discloses an electrochromic device and its manufacturing method, which uses a gel electrolyte layer, or an organic solvent layer containing lithium ions, or an aqueous solution layer containing hydrogen ions, or sodium ions, or potassium ions, or aluminum ions, on this basis, prepares an electrochromic device. The aluminum ion-based electrochromic device prepared by the above method is liquid or semi-liquid (i.e., gel state), and all of them fail to prepare a fully solid-state electrochromic device, and the packaging process has high requirements and there is a possibility of leakage, which is not conducive to the actual industrial application of electrochromic devices.

[0005] Therefore, how to disclose an aluminum ion-based all-solid-state electrochromic device and a preparation method thereof, transform the aluminum ion-based electrochromic device from a liquid or semi-liquid state (i.e., a gel state) into a solid state, prepare an all-solid-state electrolyte film that can freely migrate aluminum ions, reduce the requirements for the packaging process, and avoid leakage are difficult problems that need to be solved urgently in this field. Summary of the invention

[0006] In view of this, the present invention provides an aluminum ion-based all-solid-state electrochromic device and a preparation method thereof, so as to solve the problem that there are currently no reports on aluminum ion-based all-solid-state electrochromic devices.

[0007] In order to achieve the above object, the present invention adopts the following technical solution:

[0008] A method for preparing an aluminum ion-based all-solid-state electrochromic device comprises the following steps:

[0009] 1) Using a nickel alloy target to deposit a NiO derivative film on the underlying transparent conductive layer to form an ion storage layer;

[0010] 2) Using the aluminum salt ceramic target material to deposit a solid electrolyte film containing aluminum ions on the ion storage layer through magnetron sputtering coating technology to obtain an ion conduction layer;

[0011] 3) Depositing an electrochromic layer on the ion conducting layer using a tungsten target;

[0012] 4) A transparent conductive film is deposited using a transparent conductive electrode target to form a top transparent conductive layer, thereby obtaining an aluminum ion-based all-solid-state electrochromic device.

[0013] Preferably, the thickness of the bottom transparent conductive layer is 50-200 nm; the thickness of the ion storage layer is 50-350 nm; the thickness of the ion conduction layer is 20-300 nm; the thickness of the electrochromic layer is 50-500 nm; and the thickness of the top transparent conductive layer is 100-400 nm.

[0014] Preferably, the material of the bottom transparent conductive layer includes one or more of FTO, ITO, AZO and ATO.

[0015] Preferably, the nickel alloy target is NiA x B y , A and B independently include one or more of Mg, Al, K, Ca, Ti, V, Cr, Mn, Fe, Co, Cu, Zn, Ga, Ge, Rb, Sr, Y, Zr, Nb, Mo, Ru, Rh, Pd, Ag, Cd, In, Sn, Sb, Cs, Ba, Hf, Ta and W, x is 0~1, y is 0~1.

[0016] Preferably, the working pressure of the deposition in step 1) is 0.5-5 Pa, the power of the deposition is 20-500 W, and the deposition atmosphere is a mixed atmosphere of oxygen and argon;

[0017] Among them, the volume ratio of oxygen and argon is 0% ~ 80%.

[0018] Preferably, the aluminum salt ceramic target in step 2) includes one or more of aluminum phosphate, aluminum silicate, aluminum phosphosilicate, lithium aluminum silicate, aluminum vanadate, aluminum titanate, aluminum borate, aluminum manganate, aluminum ferrite, aluminum tungstate and aluminum niobate;

[0019] The working pressure of the deposition in step 2) is 0.5-3 Pa, the power of the deposition is 20-500 W, and the deposition atmosphere is a mixed atmosphere of oxygen and krypton;

[0020] Among them, the volume ratio of oxygen and krypton ranges from 0% to 80%.

[0021] Preferably, in step 2), water vapor needs to be introduced into the vacuum environment before the mixed atmosphere of oxygen and krypton is introduced, and the local vacuum degree is 10 -5 Pa, the pressure range of water vapor is 10 -4 ~10 -1 Pa.

[0022] Preferably, the deposition in step 3) includes a first deposition and a second deposition;

[0023] The working pressure of the first deposition and the second deposition is independently 0.5~3 Pa, the deposition power is independently 20~500 W, and the deposition atmosphere is independently a mixed atmosphere of oxygen and argon;

[0024] The volume ratio of oxygen and argon in the first deposition is 0~100%; the volume ratio of oxygen and argon in the second deposition is 0~20%.

[0025] Preferably, the transparent conductive electrode target material in step 4) includes one or more of a FTO target material, an ITO target material, an AZO target material and an ATO target material;

[0026] The working pressure of the deposition in step 3) is 0.3-0.5 Pa, the power of the deposition is 90-110 W, and the deposition atmosphere is an argon atmosphere.

[0027] Another object of the present invention is to provide an aluminum ion-based all-solid-state electrochromic device prepared by a method for preparing an aluminum ion-based all-solid-state electrochromic device.

[0028] It can be seen from the above technical solution that compared with the prior art, the present invention has the following beneficial effects:

[0029] 1. The present invention adopts magnetron sputtering technology, which has mild process conditions, simple process, can be prepared continuously, and is not limited by substrate texture, morphology, etc.;

[0030] 2. The preparation method of the aluminum ion-based all-solid-state electrochromic device of the present invention uses aluminum ions to replace the lithium ions used in the traditional electrochromic device, and selects the electrochromic layer and ion storage layer suitable for aluminum ions, namely, WO3 film and NiO film doped with other elements. The amorphous WO3 film structure contains relatively large ion channels, and the hexavalent W 6+ This results in a relatively weak attraction between aluminum ions and the surrounding oxygen anions, allowing aluminum ions to pass through, thereby improving the coloring efficiency of the electrochromic device and having extremely high electrochemical stability; at the same time, the selected doped NiO thin film material can be used for aluminum ion transmission and storage, thereby stabilizing the electrochemical cycle;

[0031] 3. The present invention can further adjust the response time of the electrochromic device by changing the density, thickness and aluminum ion concentration of the film of the ion conduction layer;

[0032] 4. The preparation of aluminum ion conductive layer film can be controlled by temperature control during the temperature gradient change process. It can prepare an ion conductive layer with a certain stress, fine and porous microstructure, and further adjust the response time of the electrochromic device;

[0033] 5. The preparation of the aluminum ion conductive layer film of the present invention has unique technical advantages. In order to increase the concentration of free aluminum ions in the film, the magnetron sputtering coating process is carried out in a water vapor saturated environment. Moreover, the use of krypton as the working gas has advantages such as high energy, which improves the deposition rate and makes the industrialization of electrochromic devices possible.

[0034] 6. The ion storage layer material of the present invention is a nickel alloy (NiA x B y ) Target reactive sputtering, the atomic ratio of other metal elements doped in the target x is 0~1, y The optical contrast and electrochromic performance of the device can be adjusted by changing the ratio of element doping and the oxygen-argon ratio in the sputtering atmosphere. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 Schematic diagram of the structure of the aluminum ion-based electrochromic device of the present invention, wherein 100 is a bottom glass substrate; 110 is a bottom transparent conductive layer; 120 is an ion storage layer; 130 is an ion conduction layer; 140 is an electrochromic layer; 150 is a top transparent conductive layer;

[0036] FIG2 is a performance characterization diagram of the aluminum ion-based all-solid-state electrochromic device prepared in Example 1 of the present invention; A: Relationship between transmittance and response time at a wavelength of 630 nm; B: Current change potential of the device; C: Example of calculation of the color change efficiency of the device;

[0037] FIG3 is a physical property characterization diagram of the aluminum ion-based all-solid-state electrochromic device prepared in Example 1 of the present invention;

[0038] Figure 4 is a performance characterization diagram of the aluminum ion-based all-solid-state electrochromic device prepared in Example 2 of the present invention. A: Relationship between transmittance and response time at a wavelength of 630nm; B: Current change potential; D: Spectral data at different voltages; E: Cross-sectional electron microscope (SEM) image of the device

[0039] Figure 5 Characterization of the AC impedance spectrum of the aluminum ion-based all-solid-state electrochromic device prepared in Example 2 of the present invention, AC impedance spectra under different bias voltages ((0V, 0.2V, 0.4V, 0.6V, 0.8V, 1.0V, 1.2V)). DETAILED DESCRIPTION

[0040] A method for preparing an aluminum ion-based all-solid-state electrochromic device comprises the following steps:

[0041] 1) Using a nickel alloy target to deposit a NiO derivative film on the underlying transparent conductive layer to form an ion storage layer;

[0042] 2) Using the aluminum salt ceramic target material to deposit a solid electrolyte film containing aluminum ions on the ion storage layer through magnetron sputtering coating technology to obtain an ion conduction layer;

[0043] 3) Depositing an electrochromic layer on the ion conducting layer using a tungsten target;

[0044] 4) A transparent conductive film is deposited using a transparent conductive electrode target to form a top transparent conductive layer, thereby obtaining an aluminum ion-based all-solid-state electrochromic device.

[0045] In the present invention, the thickness of the bottom transparent conductive layer is 50~200nm; the thickness of the ion storage layer is 50~350nm; the thickness of the ion conduction layer is 20~300nm; the thickness of the electrochromic layer is 50~500nm; the thickness of the top transparent conductive layer is 100~400nm.

[0046] In the present invention, the material of the bottom transparent conductive layer includes one or more of FTO, ITO, AZO and ATO.

[0047] In the present invention, the nickel alloy (NiA x B y ) Other elements in the target include one or more of Mg, Al, K, Ca, Ti, V, Cr, Mn, Fe, Co, Cu, Zn, Ga, Ge, Rb, Sr, Y, Zr, Nb, Mo, Ru, Rh, Pd, Ag, Cd, In, Sn, Sb, Cs, Ba, Hf, Ta and W. The atomic ratio of the doping elements of other elements is x is 0~1, y is 0~1, x or y Specifically, it can be 0.2, 0.4, 0.5, 0.6, or 0.8.

[0048] In the present invention, when the atomic ratio of the doping element x or y When both are 0, it means that the alloy nickel target does not contain other metal elements.

[0049] In the present invention, the working pressure of the deposition in step 1) is 0.5-5 Pa, specifically 0.8 Pa, 1 Pa, 2 Pa, 3 Pa, 4 Pa; the deposition power is 20-500 W, specifically 40 W, 50 W, 60 W, 80 W, 100 W, 150 W, 200 W, 250 W, 300 W, 350 W, 400 W, 450 W; the deposition atmosphere is a mixed atmosphere of oxygen and argon;

[0050] The volume ratio of oxygen to argon is 0-80%, specifically 10%, 20%, 40%, and 60%.

[0051] In the present invention, the aluminum salt ceramic target in step 2) includes one or more of aluminum phosphate, aluminum silicate, aluminum phosphosilicate, lithium aluminum silicate, aluminum vanadate, aluminum titanate, aluminum borate, aluminum manganate, aluminum ferrite, aluminum tungstate and aluminum niobate;

[0052] The working pressure of the deposition in the step 2) is 0.5-3 Pa, specifically 0.8 Pa, 1 Pa, 1.5 Pa, 2Pa, 2.5 Pa; the power of the deposition is 20-500 W, specifically 40 W, 50 W, 60 W, 80 W, 100 W, 150 W, 200 W, 250 W, 300 W, 350 W, 400 W, 450 W; the deposition atmosphere is a mixed atmosphere of oxygen and krypton;

[0053] The volume ratio of oxygen to krypton is 0-80%, specifically 10%, 20%, 40%, and 60%.

[0054] In the present invention, before the mixed atmosphere of oxygen and krypton is introduced in step 2), water vapor is introduced into the vacuum environment to reduce the pressure in the vacuum chamber to 10 -5 Pa was adjusted to 10 -4 Pa~10 -2 Pa range.

[0055] In the present invention, the deposition in step 3) includes a first deposition and a second deposition;

[0056] The working pressure of the first deposition and the second deposition is independently 0.5~3 Pa, specifically 0.8 Pa, 1Pa, 1.5 Pa, 2 Pa, 2.5 Pa; the deposition power is independently 20~500 W, specifically 40 W, 50 W, 60 W, 80 W, 100 W, 150 W, 200 W, 250 W, 300 W, 350 W, 400 W, 450 W; the deposition atmosphere is independently a mixed atmosphere of oxygen and krypton;

[0057] The volume ratio of oxygen and argon in the first deposition is 0-100%; the volume ratio of oxygen and argon in the second deposition is 0-20%.

[0058] In the present invention, the transparent conductive electrode target material in step 4) includes one or more of a FTO target material, an ITO target material, an AZO target material and an ATO target material;

[0059] The working pressure of the deposition in the step 3) is 0.3-0.5 Pa, specifically 0.32 Pa, 0.35 Pa, 0.38 Pa, 0.4 Pa, 0.42 Pa, 0.45 Pa, 0.48 Pa; the deposition power is 90-110 W, specifically 92 W, 95 W, 98 W, 100 W, 102 W, 105 W, 108 W; the deposition atmosphere is argon atmosphere.

[0060] The present invention also provides an aluminum ion-based all-solid-state electrochromic device prepared by a method for preparing an aluminum ion-based all-solid-state electrochromic device.

[0061] The schematic diagram of the structure of the aluminum ion-based electrochromic device prepared by the present invention is as follows Figure 1 shown.

[0062] Example 1

[0063] 1) The transparent conductive layer material is selected from an ITO glass substrate;

[0064] 2) Preparation of ion storage layer: Using clean ITO glass as substrate, oxygen and argon as working gas, and using a chromium-doped nickel alloy target with an atomic ratio of 0.2, a layer of NiCr with a thickness of 150 nm is deposited on the transparent conductive substrate by reactive sputtering. 0.2 O x Thin film; basic parameters are: cavity background vacuum is less than 10 -4 Pa, the flow ratio of argon and oxygen was 40:10, the working gas pressure was 1 Pa, the sputtering power was 100 W of DC power supply, and the substrate temperature was room temperature to form an ion storage layer;

[0065] 3) Preparation of ion conduction layer: In a water vapor saturated vacuum environment, krypton and oxygen are used as working gases, and aluminum silicate ceramic targets are reactively sputtered on the ion storage layer NiCr 0.2 O x A 100nm thick aluminum ion solid electrolyte film is further deposited on the thin film material; the basic parameters are: the cavity background vacuum is less than 10 -4 Pa, water is introduced through the micro-leak valve to make the vacuum degree of the vacuum chamber to be 10 -3 Pa, the flow ratio of krypton and oxygen is 50:0, the working gas pressure is 1Pa, the sputtering power is 70 W of RF power supply, and the substrate temperature is room temperature to form an ion conductive layer film;

[0066] 4) Preparation of electrochromic layer: Using argon and oxygen as working gases, the electrochromic layer is further deposited on the ion conductive layer by reactive sputtering of a metal tungsten target. The basic parameters are: the background vacuum of the cavity is less than 10 -4Pa, working gas pressure 2 Pa, sputtering power of DC power supply 70 W, substrate temperature at room temperature, when the flow ratio of argon and oxygen is 25:25, deposition is performed once to obtain the first WO3 thin film color-changing layer, when the flow ratio of argon and oxygen is 47:3, deposition is performed for the second time to obtain the second WO3 thin film color-changing layer, and then a WO3 electrochromic layer with a thickness of 350 nm is obtained;

[0067] 5) Preparation of the top transparent conductor ITO: Using argon as the working gas, a layer of ITO transparent conductive film with a thickness of 400 nm is deposited on the electrochromic layer using an ITO target by radio frequency sputtering; the basic parameters are: the cavity background vacuum is less than 10 -4 Pa, argon flow rate was 50, working gas pressure was 0.3 Pa, sputtering power was 100 W RF, substrate temperature was room temperature, and the top layer of ITO was formed.

[0068] Example 2

[0069] 1) The transparent conductive layer material is selected as an ITO glass substrate;

[0070] 2) Preparation of ion storage layer: Using clean ITO glass as substrate, oxygen and argon as working gas, and using a nickel alloy target doped with niobium, the atomic ratio of the doped element is 0.5, a layer of NiNb with a thickness of 100 nm is deposited on the transparent conductive substrate by reactive sputtering. 0.5 O x Thin film; basic parameters are: cavity background vacuum degree is less than 10 -4 Pa, the flow ratio of argon and oxygen was 40:10, the working gas pressure was 1 Pa, the sputtering power was 200 W of DC power supply, and the substrate temperature was room temperature to form an ion storage layer;

[0071] 3) Preparation of ion conduction layer: In a water vapor saturated vacuum environment, krypton and oxygen were used as working gases, and aluminum phosphate ceramic targets were reactively sputtered on the ion storage layer NiNb 0.5 O x A layer of aluminum ion solid electrolyte film with a thickness of 100 nm is further deposited on the derivative film material; the basic parameters are: the background vacuum of the cavity is less than 10 -4 Pa, water is introduced through the micro-leak valve to make the vacuum degree of the vacuum chamber to be 10 -3 Pa, the flow ratio of krypton and oxygen is 50:0, the working gas pressure is 2 Pa, the sputtering power is 100 W of RF power supply, and the substrate temperature is room temperature to form an ion conductive layer film;

[0072] 4) Preparation of electrochromic layer: Using argon and oxygen as working gases, the electrochromic layer is further deposited on the ion conductive layer by reactive sputtering of a metal tungsten target. The basic parameters are: the background vacuum of the cavity is less than 10-4 Pa, working gas pressure 2.5Pa, sputtering power is 70 W of DC power supply, substrate temperature is room temperature, when the flow ratio of argon and oxygen is 25:25, deposition is performed once to obtain the first WO3 thin film color-changing layer, when the flow ratio of argon and oxygen is 47:3, deposition is performed for the second time to obtain the second WO3 thin film color-changing layer, and then a WO3 electrochromic layer with a thickness of 400 nm is obtained;

[0073] 5) Preparation of the top transparent conductor, such as ITO: Using argon as the working gas, a layer of ITO transparent conductive film with a thickness of 350 nm is deposited on the electrochromic layer by radio frequency sputtering using an ITO target; the basic parameters are: the cavity background vacuum is less than 10 -4 Pa, argon flow rate was 50, working gas pressure was 0.3 Pa, sputtering power was RF 90 W, substrate temperature was room temperature, and the top layer of ITO was formed.

[0074] Example 3

[0075] 1) The transparent conductive layer material is selected from an ITO glass substrate;

[0076] 2) Preparation of ion storage layer: Using clean ITO glass as substrate, oxygen and argon as working gas, and using a chromium-doped nickel alloy target with an atomic ratio of 0.3, a layer of NiCr with a thickness of 100 nm is deposited on the transparent conductive substrate by reactive sputtering. 0.3 O x Thin film; basic parameters are: cavity background vacuum is less than 10 -4 Pa, the flow ratio of argon and oxygen was 45:5, the working gas pressure was 1 Pa, the sputtering power was 100 W of DC power supply, and the substrate temperature was room temperature to form an ion storage layer;

[0077] 3) Preparation of ion conduction layer: In a water vapor saturated vacuum environment, krypton and oxygen are used as working gases, and aluminum phosphate ceramic targets are reactively sputtered on the ion storage layer NiCr 0.3 O x A 50 nm thick aluminum ion solid electrolyte film is further deposited on the thin film material; the basic parameters are: the cavity background vacuum is less than 10 -4 Pa, water is introduced through the micro-leak valve to make the vacuum degree of the vacuum chamber to be 10 -3 Pa, the flow ratio of krypton and oxygen is 50:0, the working gas pressure is 1 Pa, the sputtering power is 100 W of RF power supply, and the substrate temperature is room temperature to form an ion conductive layer film;

[0078] 4) Preparation of electrochromic layer: Using argon and oxygen as working gases, the electrochromic layer is further deposited on the ion conductive layer by reactive sputtering of a metal tungsten target. The basic parameters are: the background vacuum of the cavity is less than 10 -4 Pa, working gas pressure 2 Pa, sputtering power of DC power supply 70 W, substrate temperature at room temperature, when the flow ratio of argon and oxygen is 25:25, deposition is performed once to obtain the first WO3 thin film color-changing layer, when the flow ratio of argon and oxygen is 47:3, deposition is performed for the second time to obtain the second WO3 thin film color-changing layer, and then a WO3 electrochromic layer with a thickness of 350 nm is obtained;

[0079] 5) Preparation of the top transparent conductor ITO: Using argon as the working gas, a layer of ITO transparent conductive film with a thickness of 400 nm is deposited on the electrochromic layer using an ITO target by radio frequency sputtering; the basic parameters are: the cavity background vacuum is less than 10 -4 Pa, argon flow rate was 50, working gas pressure was 0.3 Pa, sputtering power was RF 90 W, substrate temperature was room temperature, and the top layer of ITO was formed.

[0080] Example 4

[0081] 1) The transparent conductive layer material is selected from a FTO glass substrate;

[0082] 2) Preparation of ion storage layer: Using clean FTO glass as substrate, oxygen and argon as working gas, and using a chromium-doped nickel alloy target with an atomic ratio of 0.4, a layer of NiCr with a thickness of 100 nm is deposited on the transparent conductive substrate by reactive sputtering. 0.4 O x Thin film; basic parameters are: cavity background vacuum is less than 10 -4 Pa, the flow ratio of argon and oxygen was 40:10, the working gas pressure was 1 Pa, the sputtering power was 100 W of DC power supply, and the substrate temperature was room temperature to form an ion storage layer;

[0083] 3) Preparation of ion conduction layer: In a water vapor saturated vacuum environment, krypton and oxygen are used as working gases, and aluminum phosphate ceramic targets are reactively sputtered on the ion storage layer NiCr 0.4 O x A 50 nm thick aluminum ion solid electrolyte film is further deposited on the thin film material; the basic parameters are: the cavity background vacuum is less than 10 -4 Pa, water is introduced through the micro-leak valve to make the vacuum degree of the vacuum chamber to be 10 -3 Pa, the flow ratio of krypton and oxygen is 50:0, the working gas pressure is 1 Pa, the sputtering power is 100 W of RF power supply, and the substrate temperature is room temperature to form an ion conductive layer film;

[0084] 4) Preparation of electrochromic layer: Using argon and oxygen as working gases, the electrochromic layer is further deposited on the ion conductive layer by reactive sputtering of a metal tungsten target. The basic parameters are: the background vacuum of the cavity is less than 10 -4 Pa, working gas pressure 2 Pa, sputtering power of DC power supply 70 W, substrate temperature at room temperature, when the flow ratio of argon and oxygen is 25:25, deposition is performed once to obtain the first WO3 thin film color-changing layer, when the flow ratio of argon and oxygen is 47:3, deposition is performed for the second time to obtain the second WO3 thin film color-changing layer, and then a WO3 electrochromic layer with a thickness of 350 nm is obtained;

[0085] 5) Preparation of the top transparent conductor ITO: Using argon as the working gas, a layer of ITO transparent conductive film with a thickness of 400 nm is deposited on the electrochromic layer using an ITO target by radio frequency sputtering; the basic parameters are: the cavity background vacuum is less than 10 -4 Pa, argon flow rate was 50, working gas pressure was 0.3 Pa, sputtering power was RF 90 W, substrate temperature was room temperature, and the top layer of ITO was formed.

[0086] Example 5

[0087] 1) The transparent conductive layer material is selected from an ITO glass substrate;

[0088] 2) Preparation of ion storage layer: Using clean ITO glass as substrate, oxygen and argon as working gas, and using a chromium-doped nickel alloy target with an atomic ratio of 0.5, a layer of NiCr with a thickness of 150 nm is deposited on the transparent conductive substrate by reactive sputtering. 0.5 O x Thin film; basic parameters are: cavity background vacuum degree is less than 10 -4 Pa, the flow ratio of argon and oxygen was 40:10, the working gas pressure was 1 Pa, the sputtering power was 100 W of DC power supply, and the substrate temperature was room temperature to form an ion storage layer;

[0089] 3) Preparation of ion conduction layer: In a water vapor saturated vacuum environment, argon and oxygen are used as working gases, and aluminum phosphate ceramic targets are reactively sputtered on the ion storage layer NiCr 0.5 O x A 50 nm thick aluminum ion solid electrolyte film is further deposited on the thin film material; the basic parameters are: the cavity background vacuum is less than 10 -4 Pa, water is introduced through the micro-leak valve to make the vacuum degree of the vacuum chamber to be 10 -3 Pa, the flow ratio of krypton and oxygen is 50:0, the working gas pressure is 1 Pa, the sputtering power is 100 W of RF power supply, and the substrate temperature is room temperature to form an ion conductive layer film;

[0090] 4) Preparation of electrochromic layer: Using argon and oxygen as working gases, the electrochromic layer is further deposited on the ion conductive layer by reactive sputtering of a metal tungsten target. The basic parameters are: the background vacuum of the cavity is less than 10 -4 Pa, working gas pressure 2 Pa, sputtering power of DC power supply 70 W, substrate temperature at room temperature, when the flow ratio of argon and oxygen is 25:25, deposition is performed once to obtain the first WO3 thin film color-changing layer, when the flow ratio of argon and oxygen is 47:3, deposition is performed for the second time to obtain the second WO3 thin film color-changing layer, and then a WO3 electrochromic layer with a thickness of 350 nm is obtained;

[0091] 5) Preparation of the top transparent conductor ITO: Using argon as the working gas, a layer of ITO transparent conductive film with a thickness of 400 nm is deposited on the electrochromic layer using an ITO target by radio frequency sputtering; the basic parameters are: the cavity background vacuum is less than 10 -4 Pa, argon flow rate was 50, working gas pressure was 0.3 Pa, sputtering power was 100 W RF, substrate temperature was room temperature, and the top layer of ITO was formed.

[0092] Example 6

[0093] 1) The transparent conductive layer material is selected from an ITO glass substrate;

[0094] 2) Preparation of ion storage layer: Using clean ITO glass as substrate, oxygen and argon as working gas, and using a chromium-doped nickel alloy target with an atomic ratio of 0.6, a layer of NiCr with a thickness of 100 nm is deposited on the transparent conductive substrate by reactive sputtering. 0.6 O x Thin film; basic parameters are: cavity background vacuum is less than 10 -4 Pa, the flow ratio of argon and oxygen was 40:10, the working gas pressure was 1 Pa, the sputtering power was 100 W of DC power supply, and the substrate temperature was room temperature to form an ion storage layer;

[0095] 3) Preparation of ion conduction layer: In a water vapor saturated vacuum environment, krypton and oxygen are used as working gases, and aluminum phosphate ceramic targets are reactively sputtered on the ion storage layer NiCr 0.6 O x A 50 nm thick aluminum ion solid electrolyte film is further deposited on the thin film material; the basic parameters are: the cavity background vacuum is less than 10 -4 Pa, water is introduced through the micro-leak valve to make the vacuum degree of the vacuum chamber to be 10 -3 Pa, the flow ratio of krypton and oxygen is 50:0, the working gas pressure is 1 Pa, the sputtering power is 100 W of RF power supply, and the substrate temperature is room temperature to form an ion conductive layer film;

[0096] 4) Preparation of electrochromic layer: Using argon and oxygen as working gases, the electrochromic layer is further deposited on the ion conductive layer by reactive sputtering of a metal tungsten target. The basic parameters are: the background vacuum of the cavity is less than 10 -4 Pa, working gas pressure 2 Pa, sputtering power of DC power supply 70 W, substrate temperature at room temperature, when the flow ratio of argon and oxygen is 25:25, deposition is performed once to obtain the first WO3 thin film color-changing layer, when the flow ratio of argon and oxygen is 47:3, deposition is performed for the second time to obtain the second WO3 thin film color-changing layer, and then a WO3 electrochromic layer with a thickness of 350 nm is obtained;

[0097] 5) Preparation of the top transparent conductor ITO: Using argon as the working gas, a layer of ITO transparent conductive film with a thickness of 400 nm is deposited on the electrochromic layer using an ITO target by radio frequency sputtering; the basic parameters are: the cavity background vacuum is less than 10 -4 Pa, argon flow rate was 50, working gas pressure was 0.3 Pa, sputtering power was 100 W RF, substrate temperature was room temperature, and the top layer of ITO was formed.

[0098] Experimental Example 1

[0099] The performance parameters of the aluminum ion-based all-solid-state electrochromic devices prepared in Examples 1 to 6 were tested, and the test results are shown in Table 1 (transmittance difference: 39 to 49; coloring time: 15 to 20 seconds; fading time: 6 to 8 seconds; number of cycles: 50,000 to 100,000.

[0100] Table 1 Performance parameters of aluminum ion-based all-solid-state electrochromic devices

[0101] Transmittance difference / % Coloring time / s Fading time / s Cycle times Example 1 79-30 20.55 7.55 100,000 times Example 2 70-29 16.45 5.57 50,000 times Example 3 78-29 19.52 6.07 100,000 times Example 4 75-32 16.23 6.82 80,000 times Example 5 70-31 17.14 7.54 80,000 times Example 6 74-28 15.25 7.31 90,000 times

[0102] Table 1 Performance parameters of aluminum ion-based all-solid-state electrochromic devices From Table 1, it can be seen that all the examples have good durability and optical properties, especially the durability and optical properties of Example 1 and Example 3 are better than those of other examples.

[0103] The performance of the aluminum ion-based all-solid-state electrochromic device prepared in Example 1 was characterized, and the results are shown in FIG2 . Figure 2A It can be seen that the device has an optical contrast of 49% at a voltage of 3V, a coloring time of 20.55s, and a fading time of 7.55s. Figure 2B is a real-time current graph, Figure 2C The calculated coloring efficiency diagram shows that the coloring efficiency of the device is 53.9 cm 2 / C.

[0104] The physical properties of the aluminum ion-based all-solid-state electrochromic device prepared in Example 1 were characterized, and the results are shown in FIG3 . Figure 3A The SEM surface image shows that the surface morphology of the film is uniform. Figure 3B AFM 3D images of thin films. Figure 3C For substrate ITO and ITO / AlSiO x The XRD pattern shows that the aluminum silicate film is amorphous and non-crystalline. Figure 3D -G is the XPS spectrum of the film. It can be seen from the figure that the components inside the film are aluminum silicate and silicon dioxide.

[0105] The performance of the aluminum ion-based all-solid-state electrochromic device prepared in Example 2 was characterized, and the results are shown in FIG4 . Figure 4A It can be seen that the device has an optical contrast of 41% at a voltage of 3V, a coloring time of 16.45s, and a fading time of 5.57s. Figure 4B This is a real-time current graph. The coloring efficiency of the device is 21.32 cm 2 / C, Figure 4C is the spectrum of the device under different voltages. Figure 4D The SEM cross-sectional view of the device shows that the WO3 film contains Al elements. 3+ The movement of WO3 and its redox reaction with WO3 cause the film to be colored.

[0106] The AC impedance of the aluminum ion-based all-solid-state electrochromic device prepared in Example 2 was characterized. Figure 5 As shown in the figure, from the changes in the AC impedance spectrum under different bias voltages (0V, 0.2V, 0.4V, 0.6V, 0.8V, 1.0V, 1.2V), it can be seen that the device impedance gradually decreases with the increase of bias voltage, indicating that ions have begun to migrate inside the device when the bias is applied, causing the device impedance to gradually decrease.

[0107] The various embodiments in this specification are described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the various embodiments can be referenced to each other.

[0108] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A method for preparing an aluminum ion-based all-solid-state electrochromic device, It is characterized in that The steps include: 1) Depositing a NiO derivative thin film on the bottom transparent conductive layer using an alloy nickel target to form an ion storage layer, wherein the alloy nickel target is NiAxBy, A and B independently include one or more of Mg, Al, K, Ca, Ti, V, Cr, Mn, Fe, Co, Cu, Zn, Ga, Ge, Rb, Sr, Y, Zr, Nb, Mo, Ru, Rh, Pd, Ag, Cd, In, Sn, Sb, Cs, Ba, Hf, Ta and W, x is 0 to 1, and y is 0 to 1; 2) Depositing a solid electrolyte film containing aluminum ions on the ion storage layer by magnetron sputtering coating technology using an aluminum salt ceramic target to obtain an ion conduction layer, wherein the aluminum salt ceramic target is an aluminum phosphate ceramic target, and the aluminum salt ceramic target includes one or more of aluminum phosphate, aluminum phosphosilicate, lithium aluminum silicate, aluminum vanadate, aluminum titanate, aluminum borate, aluminum manganate, aluminum ferrite, aluminum tungstate and aluminum niobate; 3) Depositing an electrochromic layer on the ion conducting layer using a tungsten target; 4) Depositing a transparent conductive film using a transparent conductive electrode target to form a top transparent conductive layer to obtain an aluminum ion-based all-solid-state electrochromic device; Wherein, the working pressure of the deposition in step 2) is 0.5-3 Pa, the power of the deposition is 20-500 W, and the deposition atmosphere is a mixed atmosphere of oxygen and krypton; Among them, the volume ratio of oxygen and krypton is 0% to 80%; In step 2), water vapor needs to be introduced into the vacuum environment before the mixed atmosphere of oxygen and krypton is introduced. The local vacuum degree is 10 -5 Pa, the pressure of water vapor is 10 -4 Pa~10 -1 Pa.

2. A method for preparing an aluminum ion-based all-solid-state electrochromic device according to claim 1, It is characterized in that The thickness of the bottom transparent conductive layer is 50-200nm; the thickness of the ion storage layer is 50-350nm; the thickness of the ion conduction layer is 20-300nm; the thickness of the electrochromic layer is 50-500nm; and the thickness of the top transparent conductive layer is 100-400nm.

3. A method for preparing an aluminum ion-based all-solid-state electrochromic device according to claim 1 or 2, It is characterized in that The materials of the bottom transparent conductive layer and the top transparent conductive layer independently include one or more of FTO, ITO, AZO and ATO.

4. A method for preparing an aluminum ion-based all-solid-state electrochromic device according to claim 1 or 2, It is characterized in that The working pressure of the deposition in step 1) is 0.5-5 Pa, the power of the deposition is 20-500 W, and the deposition atmosphere is a mixed atmosphere of oxygen and argon; The volume ratio of oxygen to argon is 0% to 80%.

5. The method for preparing an aluminum ion-based all-solid-state electrochromic device according to claim 1, It is characterized in that The deposition in step 3) includes a first deposition and a second deposition; The working pressure of the first deposition and the second deposition is independently 0.5-3 Pa, the deposition power is independently 20-500 W, and the deposition atmosphere is independently a mixed atmosphere of oxygen and argon; The volume ratio of oxygen and argon in the first deposition is 0% to 100%; the volume ratio of oxygen and argon in the second deposition is 0% to 20%.

6. The method for preparing an aluminum ion-based all-solid-state electrochromic device according to claim 5, It is characterized in that The transparent conductive electrode target material in step 4) includes one or more of a FTO target material, an ITO target material, an AZO target material and an ATO target material; The working pressure of the deposition in step 4) is 0.3-0.5 Pa, the power of the deposition is 90-110 W, and the deposition atmosphere is an argon atmosphere, or a mixed atmosphere of argon and oxygen with a trace amount of oxygen added; The volume ratio of oxygen to argon is 0 to 10%.