A method for preparing water-based glue specially used for intelligent shoe machine
By using nano-silica modified fillers and raw materials such as polyols and isocyanates in the water-based glue for smart shoe machines, the problem of poor quality of adhesives being easily discovered and insufficient durability is achieved, and durability is improved and environmentally friendly Adhesive preparation.
Patent Information
- Application Number
- CN202311563859.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-22
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2043-11-22
AI Technical Summary
Quality problems for water-based adhesives for smart shoe machines are not easily discovered during use, resulting in frequent inspections, affecting efficiency and environment, and the durability of existing adhesives is insufficient, affecting the quality of the shoe.
Nanosilicon dioxide is used as raw materials to prepare modified fillers, and combined with raw materials such as polyols, isocyanates, ethylene-ethylene acetate copolymer emulsions, etc., the durability of aqueous glue is significantly improved through specific preparation steps and formulations.
It significantly improves the durability of water-based glue for smart shoe machines, reduces the detection cycle, and improves the quality and environmental friendliness of the adhesive.
Smart Images

Figure BDA0004563276730000121
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of adhesives, and in particular relates to a method for preparing a special water-based adhesive for an intelligent shoe machine. Background Art
[0002] Water-based adhesives are environmentally friendly adhesives made from natural or synthetic polymers and water as a solvent or dispersant, replacing toxic organic solvents that pollute the environment.
[0003] Adhesives are widely used in the shoemaking industry. Environmentally unfriendly adhesives will affect the environment and thus the health of the industry. Poor quality adhesives will also affect the quality of shoes. Because the water-based adhesive for smart shoe machines is machine-operated, the quality problems of water-based adhesives are not as easy to find during use as they are in manual operation. Therefore, frequent inspections are required, which costs manpower and material resources. It is necessary to develop a water-based adhesive for smart shoe machines that has good durability and reduces the inspection cycle. Summary of the invention
[0004] In response to the above problems, the researchers of the present invention conducted a series of studies on fillers for water-based adhesives for smart shoe machines and found that adding modified fillers can significantly improve durability. This patent is based on this discovery.
[0005] The present invention discloses a method for preparing a special water-based glue for an intelligent shoe machine, comprising the following steps:
[0006] S01, preparing modified filler using nano-silicon dioxide as raw material;
[0007] S02, synthesizing water-based adhesive stock solution with polyol and isocyanate as main raw materials;
[0008] S03, using the synthetic water-based adhesive stock solution and defoaming agent, substrate wetting agent, cross-linking agent, coupling agent, humectant, rheological additive, ethylene-vinyl acetate copolymer emulsion, and the modified filler as main raw materials to prepare a water-based adhesive specifically for smart shoe machines.
[0009] In some embodiments of the present invention, in S01, in addition to nano-silicon dioxide, the prepared raw materials also include polyethylene glycol, methacrylate oxypropylmethyldimethoxysilane, tin dichloride and glycidyl methacrylate.
[0010] In some embodiments of the present invention, S01 includes the following steps:
[0011] S11, taking nano-silicon dioxide, adding it to an ethanol aqueous solution, adding polyethylene glycol, and mixing and stirring;
[0012] S12, under mechanical stirring, add methacrylic acid oxypropylmethyldimethoxysilane dropwise, and continue stirring;
[0013] S13, adding tin dichloride and stirring;
[0014] S14, adding glycidyl methacrylate and stirring to react;
[0015] S15, centrifuging, washing with deionized water, and drying to obtain the modified filler.
[0016] In some embodiments of the present invention, in S14, the reaction is carried out at room temperature for 20-40 minutes.
[0017] In some embodiments of the present invention, in S01, the prepared raw materials include the following components in parts by weight:
[0018] 10-15 parts of nano-silicon dioxide, 150-250 parts of ethanol aqueous solution with a volume fraction of 20-40%, 20-25 parts of polyethylene glycol, 0.1-10 parts of methacrylic acid oxypropylmethyldimethoxysilane, 4-5 parts of tin dichloride, and 10-15 parts of glycidyl methacrylate;
[0019] Preferably, 10 parts of nano-silicon dioxide, 200 parts of 30% by volume ethanol aqueous solution, 20 parts of polyethylene glycol, 0.5-5 parts of methacrylic acid oxypropylmethyldimethoxysilane, 4 parts of tin dichloride, and 10 parts of glycidyl methacrylate;
[0020] Further preferably, 10 parts of nano-silicon dioxide, 200 parts of 30% by volume ethanol aqueous solution, 20 parts of polyethylene glycol, 1-3 parts of methacrylic acid oxypropylmethyldimethoxysilane, 4 parts of tin dichloride, and 10 parts of glycidyl methacrylate.
[0021] In some embodiments of the present invention, in S02, the isocyanate is hexamethylene diisocyanate, the polyol is polycarbonate diol, and the catalyst is stannous octoate.
[0022] In some embodiments of the present invention, S02 includes the following steps:
[0023] S21, taking polycarbonate diol, hexamethylene diisocyanate, modified filler and stannous octoate, mixing, stirring and reacting;
[0024] S22, add 2,2-dihydroxymethylbutyric acid, pentaerythritol and polyethylene glycol (MPEG1000), mix, and continue stirring to react;
[0025] S23, cooling, adding sulfonate, mixing, and stirring;
[0026] S24, adding deionized water and ethylene-vinyl acetate copolymer emulsion, mixing, stirring, and obtaining a synthetic water-based adhesive stock solution.
[0027] In some embodiments of the present invention, in S02, the prepared raw materials include the following components in parts by weight:
[0028] 100 parts of hexamethylene diisocyanate, 20-30 parts of polycarbonate diol, 0.5-5 parts of modified filler, 0.1-0.5 parts of stannous octoate, 5-10 parts of 2,2-dimethylolbutyric acid, 0.5-2 parts of pentaerythritol, 1-5 parts of polyethylene glycol (MPEG1000), 1-3 parts of sulfonate, and 100-140 parts of deionized water;
[0029] Preferably, 100 parts of hexamethylene diisocyanate, 25 parts of polycarbonate diol, 0.6-3 parts of modified filler, 0.2 parts of stannous octoate, 7 parts of 2,2-dihydroxymethylbutyric acid, 1 part of pentaerythritol, 3 parts of polyethylene glycol (MPEG1000), 2.5 parts of sulfonate, and 135 parts of deionized water.
[0030] In some embodiments of the present invention, in S21, the reaction is carried out at 90-95° C. for 2.5 h.
[0031] In some embodiments of the present invention, in S23, the temperature is lowered to 45°C and sulfonate is added.
[0032] In some embodiments of the present invention, in S03, the prepared raw materials include the following components in parts by weight:
[0033] 70-90 parts of water-based adhesive stock solution, 0.1-0.3 parts of defoaming agent TEGO Foamex8030, 0.2-0.5 parts of substrate wetting agent TEGO Wet KL245, TEGO Flow450, 0.1-0.5 parts of crosslinking agent HYMAX CA01, 0.3-0.5 parts of coupling agent H560, 1-3 parts of humectant G-400, 0.1-0.5 parts of rheological additive Rheo WT299, 10-40 parts of ethylene-vinyl acetate copolymer emulsion and 0.6-3 parts of modified filler;
[0034] Preferably, 80 parts of aqueous adhesive stock solution, 0.2 parts of defoaming agent TEGO Foamex8030, 0.3 parts of substrate wetting agent TEGO Wet KL245, 0.3 parts of crosslinking agent HYMAX CA01, 0.4 parts of coupling agent H560, 2 parts of humectant G-400, 0.2 parts of rheological additive Rheo WT299, 15 parts of ethylene-vinyl acetate copolymer emulsion and 0.6-3 parts of modified filler.
[0035] In some embodiments of the present invention, in S03, stirring is performed at 500-700 r / min for 20-30 min.
[0036] Beneficial effects:
[0037] The preparation method of the special water-based glue for intelligent shoe machines of the present invention uses polyol, isocyanate and ethylene-vinyl acetate copolymer emulsion as main raw materials, and can significantly improve the durability by adding modified fillers.
[0038] The modified filler of the invention is modified by using nano silicon dioxide as a raw material. Compared with the unmodified filler, the durability of the obtained special water-based glue for intelligent shoe machines is significantly improved. DETAILED DESCRIPTION
[0039] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.
[0040] Unless otherwise specified, the examples and comparative examples are parallel tests with the same components, component contents, preparation steps and preparation parameters. The stirring speed is 500 rpm. The polyethylene glycol is PEG1000. The brand of the ethylene-vinyl acetate copolymer emulsion is CP149, and the effective substance content is greater than 55.5%. The defoamer is TEGO Foamex8030, the substrate wetting agent is TEGOWet KL245, the crosslinking agent is HYMAX CA01, the coupling agent is H560, the humectant is G-400, and the rheological additive is Rheo WT299.
[0041] Example 1
[0042] A method for preparing water-based glue specially used for intelligent shoe machine
[0043] (1) Preparation of modified fillers
[0044] Take commercially available nano-silica, add it to a 50% (v / v) ethanol aqueous solution, add polyethylene glycol, and mix and stir for 10 minutes;
[0045] Under mechanical stirring, add methacrylic acid oxypropylmethyldimethoxysilane dropwise and continue stirring for 10 min;
[0046] Add tin dichloride and stir for 10 minutes;
[0047] Add glycidyl methacrylate and stir to react for 30 minutes;
[0048] Centrifuge, wash with deionized water three times, and dry to obtain the modified filler;
[0049] For every 10 parts by weight of nano-silica, 200 parts by weight of ethanol aqueous solution, 20 parts by weight of polyethylene glycol, 2 parts by weight of methacrylate oxypropylmethyldimethoxysilane, 4 parts by weight of tin dichloride, and 10 parts by weight of glycidyl methacrylate are added.
[0050] (2) Preparation of water-based adhesive stock solution
[0051] Take polycarbonate diol with a number average relative molecular mass of 1000-3000, hexamethylene diisocyanate, and stannous octoate, mix, stir, and react at 90°C for 1.5h;
[0052] Add 2,2-dihydroxymethylbutyric acid, pentaerythritol and polyethylene glycol (MPEG1000), mix, and continue stirring to react for 1.5 hours;
[0053] Cool down to 45°C, add sulfonate, mix, and stir for 30 min;
[0054] Deionized water was added, mixed, and stirred for 60 minutes to obtain a water-based adhesive stock solution.
[0055] Among them, hexamethylene diisocyanate 100 parts by weight, polycarbonate diol 25 parts by weight, stannous octoate 0.2 parts by weight, 2,2-dihydroxymethylbutyric acid 7 parts by weight, pentaerythritol 1 part by weight, polyethylene glycol (MPEG1000) 3 parts by weight, sulfonate 2.5 parts by weight, deionized water 135 parts by weight.
[0056] (3) mixing the synthesized aqueous adhesive stock solution, defoamer, substrate wetting agent, crosslinking agent, coupling agent, humectant, rheological additive, ethylene-vinyl acetate copolymer emulsion and the modified filler, and stirring evenly for 15-25 minutes;
[0057] Among them, 80 parts by weight of water-based adhesive stock solution, 0.2 parts by weight of defoamer, 0.3 parts by weight of substrate wetting agent, 0.3 parts by weight of crosslinking agent, 0.4 parts by weight of coupling agent H560, 2 parts by weight of humectant, 0.2 parts by weight of rheological additive, 15 parts by weight of ethylene-vinyl acetate copolymer emulsion and 1 part by weight of modified filler.
[0058] Example 2
[0059] A method for preparing water-based glue specially used for intelligent shoe machine
[0060] (1) Preparation of modified fillers
[0061] Take commercially available nano-silica, add it to a 50% (v / v) ethanol aqueous solution, add polyethylene glycol, and mix and stir for 10 minutes;
[0062] Under mechanical stirring, add methacrylic acid oxypropylmethyldimethoxysilane dropwise and continue stirring for 10 min;
[0063] Add tin dichloride and stir for 10 minutes;
[0064] Add glycidyl methacrylate and stir to react for 30 minutes;
[0065] Centrifuge, wash with deionized water three times, and dry to obtain the modified filler;
[0066] For every 10 parts by weight of nano-silica, 200 parts by weight of ethanol aqueous solution, 20 parts by weight of polyethylene glycol, 2 parts by weight of methacrylate oxypropylmethyldimethoxysilane, 4 parts by weight of tin dichloride, and 10 parts by weight of glycidyl methacrylate are added.
[0067] (2) Preparation of water-based adhesive stock solution
[0068] Take polycarbonate diol with a number average relative molecular mass of 1000-3000, hexamethylene diisocyanate, and stannous octoate, mix, stir, and react at 90°C for 1.5h;
[0069] Add 2,2-dihydroxymethylbutyric acid, pentaerythritol and polyethylene glycol (MPEG1000), mix, and continue stirring to react for 1.5 hours;
[0070] Cool down to 45°C, add sulfonate, mix, and stir for 30 min;
[0071] Deionized water was added, mixed, and stirred for 60 minutes to obtain a water-based adhesive stock solution.
[0072] Among them, hexamethylene diisocyanate 100 parts by weight, polycarbonate diol 25 parts by weight, stannous octoate 0.2 parts by weight, 2,2-dihydroxymethylbutyric acid 7 parts by weight, pentaerythritol 1 part by weight, polyethylene glycol (MPEG1000) 3 parts by weight, sulfonate 2.5 parts by weight, deionized water 135 parts by weight.
[0073] (3) mixing the synthesized aqueous adhesive stock solution, defoamer, substrate wetting agent, crosslinking agent, coupling agent, humectant, rheological additive, ethylene-vinyl acetate copolymer emulsion and the modified filler, and stirring evenly for 15-25 minutes;
[0074] Among them, 80 parts by weight of water-based adhesive stock solution, 0.2 parts by weight of defoamer, 0.3 parts by weight of substrate wetting agent, 0.3 parts by weight of crosslinking agent, 0.4 parts by weight of coupling agent H560, 2 parts by weight of humectant, 0.2 parts by weight of rheological additive, 15 parts by weight of ethylene-vinyl acetate copolymer emulsion and 2 parts by weight of modified filler.
[0075] Example 3
[0076] A method for preparing water-based glue specially used for intelligent shoe machine
[0077] (1) Preparation of modified fillers
[0078] Take commercially available nano-silica, add it to a 50% (v / v) ethanol aqueous solution, add polyethylene glycol, and mix and stir for 10 minutes;
[0079] Under mechanical stirring, add methacrylic acid oxypropylmethyldimethoxysilane dropwise and continue stirring for 10 min;
[0080] Add tin dichloride and stir for 10 minutes;
[0081] Add glycidyl methacrylate and stir to react for 30 minutes;
[0082] Centrifuge, wash with deionized water three times, and dry to obtain the modified filler;
[0083] For every 10 parts by weight of nano-silica, 200 parts by weight of ethanol aqueous solution, 20 parts by weight of polyethylene glycol, 2 parts by weight of methacrylate oxypropylmethyldimethoxysilane, 4 parts by weight of tin dichloride, and 10 parts by weight of glycidyl methacrylate are added.
[0084] (2) Preparation of water-based adhesive stock solution
[0085] Take polycarbonate diol with a number average relative molecular mass of 1000-3000, hexamethylene diisocyanate, and stannous octoate, mix, stir, and react at 90°C for 1.5h;
[0086] Add 2,2-dihydroxymethylbutyric acid, pentaerythritol and polyethylene glycol (MPEG1000), mix, and continue stirring to react for 1.5 hours;
[0087] Cool down to 45°C, add sulfonate, mix, and stir for 30 min;
[0088] Deionized water was added, mixed, and stirred for 60 minutes to obtain a water-based adhesive stock solution.
[0089] Among them, hexamethylene diisocyanate 100 parts by weight, polycarbonate diol 25 parts by weight, stannous octoate 0.2 parts by weight, 2,2-dihydroxymethylbutyric acid 7 parts by weight, pentaerythritol 1 part by weight, polyethylene glycol (MPEG1000) 3 parts by weight, sulfonate 2.5 parts by weight, deionized water 135 parts by weight.
[0090] (3) mixing the synthesized aqueous adhesive stock solution, defoamer, substrate wetting agent, crosslinking agent, coupling agent, humectant, rheological additive, ethylene-vinyl acetate copolymer emulsion and the modified filler, and stirring evenly for 15-25 minutes;
[0091] Among them, 80 parts by weight of water-based adhesive stock solution, 0.2 parts by weight of defoamer, 0.3 parts by weight of substrate wetting agent, 0.3 parts by weight of crosslinking agent, 0.4 parts by weight of coupling agent H560, 2 parts by weight of humectant, 0.2 parts by weight of rheological additive, 15 parts by weight of ethylene-vinyl acetate copolymer emulsion and 0.6 parts by weight of modified filler.
[0092] Example 4
[0093] A method for preparing water-based glue specially used for intelligent shoe machine
[0094] (1) Preparation of modified fillers
[0095] Take commercially available nano-silica, add it to a 50% (v / v) ethanol aqueous solution, add polyethylene glycol, and mix and stir for 10 minutes;
[0096] Under mechanical stirring, add methacrylic acid oxypropylmethyldimethoxysilane dropwise and continue stirring for 10 min;
[0097] Add tin dichloride and stir for 10 minutes;
[0098] Add glycidyl methacrylate and stir to react for 30 minutes;
[0099] Centrifuge, wash with deionized water three times, and dry to obtain the modified filler;
[0100] For every 10 parts by weight of nano-silica, there are mixed 200 parts by weight of ethanol aqueous solution, 20 parts by weight of polyethylene glycol, 1 part by weight of methacrylate oxypropylmethyldimethoxysilane, 4 parts by weight of tin dichloride, and 10 parts by weight of glycidyl methacrylate.
[0101] (2) Preparation of water-based adhesive stock solution
[0102] Take polycarbonate diol with a number average relative molecular mass of 1000-3000, hexamethylene diisocyanate, and stannous octoate, mix, stir, and react at 90°C for 1.5h;
[0103] Add 2,2-dihydroxymethylbutyric acid, pentaerythritol and polyethylene glycol (MPEG1000), mix, and continue stirring to react for 1.5 hours;
[0104] Cool down to 45°C, add sulfonate, mix, and stir for 30 min;
[0105] Deionized water was added, mixed, and stirred for 60 minutes to obtain a water-based adhesive stock solution.
[0106] Among them, hexamethylene diisocyanate 100 parts by weight, polycarbonate diol 25 parts by weight, stannous octoate 0.2 parts by weight, 2,2-dihydroxymethylbutyric acid 7 parts by weight, pentaerythritol 1 part by weight, polyethylene glycol (MPEG1000) 3 parts by weight, sulfonate 2.5 parts by weight, deionized water 135 parts by weight.
[0107] (3) mixing the synthesized aqueous adhesive stock solution, defoamer, substrate wetting agent, crosslinking agent, coupling agent, humectant, rheological additive, ethylene-vinyl acetate copolymer emulsion and the modified filler, and stirring evenly for 15-25 minutes;
[0108] Among them, 80 parts by weight of water-based adhesive stock solution, 0.2 parts by weight of defoamer, 0.3 parts by weight of substrate wetting agent, 0.3 parts by weight of crosslinking agent, 0.4 parts by weight of coupling agent H560, 2 parts by weight of humectant, 0.2 parts by weight of rheological additive, 15 parts by weight of ethylene-vinyl acetate copolymer emulsion and 1 part by weight of modified filler.
[0109] Example 5
[0110] A method for preparing water-based glue specially used for intelligent shoe machine
[0111] (1) Preparation of modified fillers
[0112] Take commercially available nano-silica, add it to a 50% (v / v) ethanol aqueous solution, add polyethylene glycol, and mix and stir for 10 minutes;
[0113] Under mechanical stirring, add methacrylic acid oxypropylmethyldimethoxysilane dropwise and continue stirring for 10 min;
[0114] Add tin dichloride and stir for 10 minutes;
[0115] Add glycidyl methacrylate and stir to react for 30 minutes;
[0116] Centrifuge, wash with deionized water three times, and dry to obtain the modified filler;
[0117] For every 10 parts by weight of nano-silica, there are mixed 200 parts by weight of ethanol aqueous solution, 20 parts by weight of polyethylene glycol, 3 parts by weight of methacrylate oxypropylmethyldimethoxysilane, 4 parts by weight of tin dichloride, and 10 parts by weight of glycidyl methacrylate.
[0118] (2) Preparation of water-based adhesive stock solution
[0119] Take polycarbonate diol with a number average relative molecular mass of 1000-3000, hexamethylene diisocyanate, and stannous octoate, mix, stir, and react at 90°C for 1.5h;
[0120] Add 2,2-dihydroxymethylbutyric acid, pentaerythritol and polyethylene glycol (MPEG1000), mix, and continue stirring to react for 1.5 hours;
[0121] Cool down to 45°C, add sulfonate, mix, and stir for 30 min;
[0122] Deionized water was added, mixed, and stirred for 60 minutes to obtain a water-based adhesive stock solution.
[0123] Among them, hexamethylene diisocyanate 100 parts by weight, polycarbonate diol 25 parts by weight, stannous octoate 0.2 parts by weight, 2,2-dihydroxymethylbutyric acid 7 parts by weight, pentaerythritol 1 part by weight, polyethylene glycol (MPEG1000) 3 parts by weight, sulfonate 2.5 parts by weight, deionized water 135 parts by weight.
[0124] (3) mixing the synthesized aqueous adhesive stock solution, defoamer, substrate wetting agent, crosslinking agent, coupling agent, humectant, rheological additive, ethylene-vinyl acetate copolymer emulsion and the modified filler, and stirring evenly for 15-25 minutes;
[0125] Among them, 80 parts by weight of water-based adhesive stock solution, 0.2 parts by weight of defoamer, 0.3 parts by weight of substrate wetting agent, 0.3 parts by weight of crosslinking agent, 0.4 parts by weight of coupling agent H560, 2 parts by weight of humectant, 0.2 parts by weight of rheological additive, 15 parts by weight of ethylene-vinyl acetate copolymer emulsion and 1 part by weight of modified filler.
[0126] Comparative Example 1
[0127] A method for preparing water-based glue specially used for intelligent shoe machine
[0128] (1) Preparation of modified fillers
[0129] Take commercially available nano-silica, add it to a 50% (v / v) ethanol aqueous solution, add polyethylene glycol, and mix and stir for 10 minutes;
[0130] Under mechanical stirring, add methacrylic acid oxypropylmethyldimethoxysilane dropwise and continue stirring for 10 min;
[0131] Add tin dichloride and stir for 10 minutes;
[0132] Add glycidyl methacrylate and stir to react for 30 minutes;
[0133] Centrifuge, wash with deionized water three times, and dry to obtain the modified filler;
[0134] For every 10 parts by weight of nano-silica, 200 parts by weight of ethanol aqueous solution, 20 parts by weight of polyethylene glycol, 2 parts by weight of methacrylate oxypropylmethyldimethoxysilane, 4 parts by weight of tin dichloride, and 10 parts by weight of glycidyl methacrylate are added.
[0135] (2) Preparation of water-based adhesive stock solution
[0136] Take polycarbonate diol with a number average relative molecular mass of 1000-3000, hexamethylene diisocyanate, and stannous octoate, mix, stir, and react at 90°C for 1.5h;
[0137] Add 2,2-dihydroxymethylbutyric acid, pentaerythritol and polyethylene glycol (MPEG1000), mix, and continue stirring to react for 1.5 hours;
[0138] Cool down to 45°C, add sulfonate, mix, and stir for 30 min;
[0139] Deionized water was added, mixed, and stirred for 60 minutes to obtain a water-based adhesive stock solution.
[0140] Among them, hexamethylene diisocyanate 100 parts by weight, polycarbonate diol 25 parts by weight, stannous octoate 0.2 parts by weight, 2,2-dihydroxymethylbutyric acid 7 parts by weight, pentaerythritol 1 part by weight, polyethylene glycol (MPEG1000) 3 parts by weight, sulfonate 2.5 parts by weight, deionized water 135 parts by weight.
[0141] (3) mixing the synthesized aqueous adhesive stock solution, defoamer, substrate wetting agent, crosslinking agent, coupling agent, humectant, rheological additive, ethylene-vinyl acetate copolymer emulsion and the modified filler, and stirring evenly for 15-25 minutes;
[0142] Among them, 80 parts by weight of water-based adhesive stock solution, 0.2 parts by weight of defoamer, 0.3 parts by weight of substrate wetting agent, 0.3 parts by weight of crosslinking agent, 0.4 parts by weight of coupling agent H560, 2 parts by weight of humectant, 0.2 parts by weight of rheological additive, 15 parts by weight of ethylene-vinyl acetate copolymer emulsion and 0.1 parts by weight of modified filler.
[0143] Comparative Example 2
[0144] A method for preparing a water-based adhesive specifically for an intelligent shoe machine, which differs from Example 1 in that unmodified nano-silicon dioxide is used.
[0145] Experimental example Durability
[0146] The water-based adhesive for smart shoe machines of the embodiment and comparative example were stored in a sealed environment at 45°C for 3 months. The peel strength of the application was measured. The water-based adhesive for smart shoe machines was stirred at 500 rpm for 30 minutes before application. The untreated comparative example 2 was used as the benchmark (100%), and the results are shown in Table 1.
[0147] Table 1 Product performance
[0148]
[0149] The results show that the durability of the water-based adhesives of Examples 1-5 after high-temperature storage is significantly better than that of Comparative Examples 1 and 2, among which Examples 1-3 are significantly better than Examples 4 and 5, and among Examples 1-3, Example 2 is better.
[0150] The preferred specific implementation modes and embodiments of the present invention are described in detail above, but the present invention is not limited to the above implementation modes and embodiments, and various changes can be made within the knowledge scope of those skilled in the art without departing from the concept of the present invention.
Claims
1. A method for preparing a water-based adhesive specifically for an intelligent shoe machine, characterized in that: The following steps are involved: S01, preparing modified filler using nano-silicon dioxide as raw material; S02, synthesizing water-based adhesive stock solution with polyol and isocyanate as main raw materials; S03, using the synthetic water-based adhesive stock solution and defoamer, substrate wetting agent, crosslinking agent, coupling agent, humectant, rheological additive, ethylene-vinyl acetate copolymer emulsion, and the modified filler as main raw materials to prepare a water-based adhesive for smart shoe machines; In S01, in addition to nano-silica, the raw materials prepared also include polyethylene glycol, methacrylate oxypropylmethyldimethoxysilane, tin dichloride and glycidyl methacrylate; In S01, The following steps are involved: S11, taking nano-silicon dioxide, adding it to an ethanol aqueous solution, adding polyethylene glycol, and mixing and stirring; S12, under mechanical stirring, add methacrylic acid oxypropylmethyldimethoxysilane dropwise, and continue stirring; S13, adding tin dichloride and stirring; S14, adding glycidyl methacrylate and stirring to react; S15, centrifuging, washing with deionized water, and drying to obtain the modified filler; In S03, the prepared raw materials include the following components in parts by weight: 70-90 parts of water-based adhesive stock solution, 0.1-0.3 parts of defoaming agent TEGO Foamex8030, 0.2-0.5 parts of substrate wetting agent TEGO Wet KL245, TEGO Flow450, 0.1-0.5 parts of crosslinking agent HYMAX CA01, 0.3-0.5 parts of coupling agent KH560, 1-3 parts of humectant G-400, 0.1-0.5 parts of rheological additive Rheo WT299, 10-40 parts of ethylene-vinyl acetate copolymer emulsion and 0.6-3 parts of modified filler; In S01, the prepared raw materials include the following components in parts by weight: 10-15 parts of nano-silicon dioxide, 150-250 parts of ethanol aqueous solution with a volume fraction of 20-40%, 20-25 parts of polyethylene glycol, 0.1-10 parts of methacrylic acid oxypropylmethyldimethoxysilane, 4-5 parts of tin dichloride, and 10-15 parts of glycidyl methacrylate; In S02, the prepared raw materials include the following components in parts by weight: 100 parts of hexamethylene diisocyanate, 20-30 parts of polycarbonate diol, 0.5-5 parts of modified filler, 0.1-0.5 parts of stannous octoate, 5-10 parts of 2,2-dihydroxymethylbutyric acid, 0.5-2 parts of pentaerythritol, 1-5 parts of polyethylene glycol MPEG1000, 1-3 parts of sulfonate, and 100-140 parts of deionized water.
2. The method for preparing the water-based glue for intelligent shoe machines according to claim 1, characterized in that: In S14, the reaction is carried out at room temperature for 20-40 minutes.
3. The method for preparing the special water-based glue for intelligent shoe machines according to claim 1 or 2, characterized in that: In S01, the prepared raw materials include the following components in parts by weight: 10 parts of nano silicon dioxide, 200 parts of 30% by volume ethanol aqueous solution, 20 parts of polyethylene glycol, 0.5-5 parts of methacrylic acid oxypropylmethyldimethoxysilane, 4 parts of tin dichloride, and 10 parts of glycidyl methacrylate.
4. The method for preparing the special water-based glue for intelligent shoe machines according to claim 1 or 2, characterized in that: In S01, the prepared raw materials include the following components in parts by weight: 10 parts of nano silicon dioxide, 200 parts of 30% by volume ethanol aqueous solution, 20 parts of polyethylene glycol, 1-3 parts of methacrylic acid oxypropylmethyldimethoxysilane, 4 parts of tin dichloride, and 10 parts of glycidyl methacrylate.
5. The method for preparing the special water-based glue for intelligent shoe machines according to claim 1 or 2, characterized in that: S02 includes the following steps: S21, taking polycarbonate diol, hexamethylene diisocyanate, modified filler and stannous octoate, mixing, stirring and reacting; S22, add 2,2-dihydroxymethylbutyric acid, pentaerythritol and polyethylene glycol MPEG1000, mix, and continue stirring to react; S23, cooling, adding sulfonate, mixing, and stirring; S24, adding deionized water and ethylene-vinyl acetate copolymer emulsion, mixing, stirring, and obtaining a synthetic water-based adhesive stock solution.
6. The method for preparing the special water-based glue for intelligent shoe machines according to claim 1 or 2, characterized in that: In S02, the prepared raw materials include the following components in parts by weight: 100 parts of hexamethylene diisocyanate, 25 parts of polycarbonate diol, 0.6-3 parts of modified filler, 0.2 parts of stannous octoate, 7 parts of 2,2-dihydroxymethylbutyric acid, 1 part of pentaerythritol, 3 parts of polyethylene glycol MPEG1000, 2.5 parts of sulfonate, and 135 parts of deionized water.
7. The method for preparing the special water-based glue for intelligent shoe machines according to claim 1 or 2, characterized in that: In S21, the reaction is carried out at 90-95°C for 1.5-4h; In S23, the temperature is lowered to 45°C and sulfonate is added.
8. The method for preparing the special water-based glue for intelligent shoe machines according to claim 1 or 2, characterized in that: In S03, stir at 500-700r / min for 20-30 min.