Adhesive composition, adhesive sheet and laminate

By using polycarbodiimide and (meth)acrylic polymers with low glass transition temperature, the problem of insufficient transparency and adhesion of the adhesive sheet in a humid and hot environment is solved, and high transparency is achieved. Whitening-resistant adhesive sheet, suitable for bonding of optical components.

CN117413036BActive Publication Date: 2024-12-06OJI HLDG CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202380012041.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2022-02-18
Filing Date
2023-02-16
Publication Date
2024-12-06
Estimated Expiration
2043-02-16

AI Technical Summary

Technical Problem

The existing adhesive sheets are insufficient in humid and hot environments, and are prone to whitening, and cannot maintain excellent performance under high temperature and high humidity conditions.

Method used

采用包含聚碳二亚胺和玻璃化转变温度为0℃以下的(甲基)丙烯酸类聚合物的粘合剂组合物,结合玻璃化转变温度为20℃以上的树脂、多官能单体和交联剂,形成高透明、耐白化的粘合片,用于光学构件的贴合。

Benefits of technology

In humid and hot environment, the adhesion and transparency of the adhesive sheet are significantly improved, the whitening phenomenon is suppressed, and the stable performance is ensured for long-term use.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004578859280000251
    Figure BDA0004578859280000251
  • Figure HDA0004578859290000011
    Figure HDA0004578859290000011
Patent Text Reader

Abstract

The present invention aims to provide an adhesive sheet which shows excellent adhesion to an adherend even in a hot and humid environment and whose whitening is suppressed. The present invention relates to an adhesive composition, comprising: polycarbodiimide and a (meth)acrylic polymer having a glass transition temperature of 0°C or less, the (meth)acrylic polymer having a (meth)acrylic monomer unit having a hydroxyl group, the content of the (meth)acrylic monomer unit having a hydroxyl group in the (meth)acrylic polymer being 20% ​​by mass or more relative to the total mass of the (meth)acrylic polymer, and the content of the (meth)acrylic monomer unit having a carboxylic acid group in the (meth)acrylic polymer being 0.1% by mass or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an adhesive composition, an adhesive sheet and a laminate. Background Art

[0002] In the past, input devices used in combination with display devices such as liquid crystal displays (LCDs) and touch panels have been widely used. In these display devices and input devices, transparent adhesive sheets are used for bonding optical components, and transparent adhesive sheets are also used for bonding the display device and the input device.

[0003] In order to improve the durability of the adhesive sheet, it is effective to improve the cohesive force of the adhesive contained in the adhesive sheet. Therefore, a scheme for improving the cohesive force of the adhesive by adding various crosslinking agents to the adhesive to crosslink the acrylic polymer has been studied. For example, Patent Document 1 discloses an adhesive composition containing an acrylic resin (A) and a carbodiimide compound (B). Here, the acrylic resin (A) contains more than 0% by weight and less than 0.2% by weight of a carboxyl-containing monomer in all polymerized components, and the amount of carboxyl groups (Xmmol) in the acrylic resin (A) and the amount of carbodiimide groups (Ymmol) in the carbodiimide compound (B) satisfy the relationship of Y / X≥1. Patent Document 1 studies the improvement of the durability of the adhesive sheet by crosslinking between the carboxyl groups possessed by the acrylic resin (A) and the carbodiimide compound (B).

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2020-143211 Summary of the invention

[0007] Problem that the invention aims to solve

[0008] The adhesive sheet bonded to the optical component is required to have high transparency and adhesion. In recent years, the optical component bonded with the adhesive sheet is sometimes used in harsh environments such as high temperature and high humidity environments, and is required to exhibit high transparency and adhesion under such conditions. However, the adhesive sheet obtained in Patent Document 1 sometimes whitens in a hot and humid environment, and there is also room for improvement in the adhesion to the adherend.

[0009] Therefore, in order to solve the problems of the prior art, the present inventors have conducted studies for the purpose of providing a PSA sheet that exhibits excellent adhesion to an adherend even in a hot and humid environment and in which whitening is suppressed.

[0010] Solutions for solving problems

[0011] Specifically, the present invention has the following configurations.

[0012] [1] An adhesive composition comprising: a polycarbodiimide and a (meth)acrylic polymer having a glass transition temperature of 0° C. or less;

[0013] The (meth)acrylic polymer comprises a (meth)acrylic monomer unit having a hydroxyl group.

[0014] The content of the (meth)acrylic monomer unit having a hydroxyl group in the (meth)acrylic polymer is 20% by mass or more relative to the total mass of the (meth)acrylic polymer.

[0015] The content of the (meth)acrylic acid monomer unit having a carboxylic acid group in the (meth)acrylic acid polymer is 0.1% by mass or less.

[0016] [2] The adhesive composition according to [1], wherein the weight average molecular weight of the polycarbodiimide is 1,000 or more.

[0017] [3] The adhesive composition according to [1] or [2], further comprising a resin having a glass transition temperature of 20° C. or higher.

[0018] [4] The adhesive composition according to any one of [1] to [3], further comprising a polyfunctional monomer.

[0019] [5] The adhesive composition according to any one of [1] to [4], further comprising a cross-linking agent.

[0020] [6] The adhesive composition according to any one of [1] to [5], further comprising a photopolymerization initiator.

[0021] [7] A pressure-sensitive adhesive sheet comprising the pressure-sensitive adhesive composition according to any one of [1] to [6].

[0022] [8] The pressure-sensitive adhesive sheet according to [7], which is used for bonding an adherend,

[0023] Here, the adherend contains a resin having a carbonyl group.

[0024] [9] The pressure-sensitive adhesive sheet according to [8], wherein the adherend comprises at least one selected from the group consisting of polycarbonate and polymethyl methacrylate.

[0025]

[10] A laminate comprising an adherend and the pressure-sensitive adhesive sheet according to any one of [7] to [9],

[0026] The adherend contains at least one selected from the group consisting of polycarbonate and polymethyl methacrylate.

[0027] Effects of the Invention

[0028] According to the present invention, a PSA sheet can be obtained which exhibits excellent adhesion to an adherend even in a hot and humid environment and in which whitening is suppressed. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 This is a schematic diagram showing a cross section of a pressure-sensitive adhesive sheet having a release sheet. DETAILED DESCRIPTION

[0030] The present invention is described in detail below. The description of the technical features described below is sometimes based on representative embodiments and specific examples, but the present invention is not limited to such embodiments. It should be noted that the numerical range represented by "to" in this specification refers to a range including the numerical values ​​recorded before and after "to" as the lower limit and upper limit.

[0031] In addition, in this specification, "(meth)acrylic acid" means both or any one of acrylic acid and methacrylic acid. In addition, in this specification, "monomer" and "monomer" have the same meaning, and "polymer" and "polymer" have the same meaning.

[0032] (Adhesive composition)

[0033] The present invention relates to an adhesive composition, comprising: polycarbodiimide and a (meth)acrylic polymer having a glass transition temperature of 0°C or less. Here, the (meth)acrylic polymer comprises a (meth)acrylic monomer unit having a hydroxyl group, and the content of the (meth)acrylic monomer unit having a hydroxyl group in the (meth)acrylic polymer is 20% by mass or more relative to the total mass of the (meth)acrylic polymer. In addition, the content of the (meth)acrylic monomer unit having a carboxylic acid group in the (meth)acrylic polymer is 0.1% by mass or less.

[0034] By the above-mentioned constitution, the adhesive sheet formed by the adhesive composition of the present invention also has excellent adhesion to the adherend under a hot and humid environment. In addition, the adhesive sheet formed by the adhesive composition of the present invention also exerts excellent whitening resistance under a hot and humid environment. Thus, the adhesive sheet formed by the adhesive composition of the present invention is highly transparent and has excellent light transmittance, and therefore, is particularly preferably used for optical purposes. In addition, the adhesive sheet formed by the adhesive composition of the present invention also exerts excellent adhesion to the adherend. Even if it is placed under a hot and humid environment for a long time, this characteristic can also be exerted.

[0035] In this specification, when evaluating the adhesion of the adhesive sheet, a wet heat constant load test is performed, and if the time until the weight falls is above the specified value, it is judged to be excellent in adhesion. Specifically, after a laminate with a polyester film on one side of the adhesive sheet and an adherend on the other side is placed in a constant temperature and humidity machine at a temperature of 85°C and a relative humidity of 85% for 30 minutes, a 100g weight is hung on the end of the polyester film, and the time until the weight falls from the adhesive layer is measured. For example, the time until the weight falls is preferably more than 15 minutes, more preferably more than 30 minutes.

[0036] In this specification, when evaluating the whitening resistance of the adhesive sheet, first, the adhesive sheet is bonded to the glass plate and the adherend, and then treated in an autoclave at a temperature of 30°C and a pressure of 0.5 MPa for 30 minutes, and then left to stand for 1 day at atmospheric pressure and room temperature. Next, the laminate is placed in a constant temperature and humidity machine adjusted to a temperature of 85°C and a relative humidity of 85%. After 7 days, the haze value of the laminate is measured using HM-150 of Murakami Color Technology Research Institute. For example, the haze value is preferably less than 3, and more preferably less than 1.5.

[0037] <(Meth)acrylic polymer>

[0038] The adhesive composition contains a (meth)acrylic acid polymer having a (meth)acrylic acid monomer unit having a hydroxyl group and having a glass transition temperature of 0° C. or less. The content of the (meth)acrylic acid monomer unit having a hydroxyl group in the (meth)acrylic acid polymer is 20% by mass or more relative to the total mass of the (meth)acrylic acid polymer, and the content of the (meth)acrylic acid monomer unit having a carboxylic acid group in the (meth)acrylic acid polymer is 0.1% by mass or less.

[0039] Examples of the (meth)acrylic monomer having a hydroxyl group include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 3-chloro-2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, and polyalkylene glycol mono(meth)acrylate. Among them, it is preferred to use at least one selected from 2-hydroxyethyl (meth)acrylate and 4-hydroxybutyl (meth)acrylate.

[0040] The content of the (meth) acrylic monomer units having a hydroxyl group in the (meth) acrylic polymer is 20% or more by mass relative to the total mass of the (meth) acrylic polymer, preferably 25% or more by mass. In addition, the content of the (meth) acrylic monomer units having a hydroxyl group in the (meth) acrylic polymer is preferably 50% or less by mass relative to the total mass of the (meth) acrylic polymer. By making the content of the (meth) acrylic monomer units having a hydroxyl group within the above range, the whitening resistance and adhesion of the adhesive sheet under high temperature and high humidity environments can be more effectively improved.

[0041] The content of the (meth)acrylic acid monomer unit having a carboxylic acid group in the (meth)acrylic acid polymer is 0.1% by mass or less, preferably 0.01% by mass or less. This means that the (meth)acrylic acid polymer does not substantially have a (meth)acrylic acid monomer unit having a carboxylic acid group. That is, the (meth)acrylic acid polymer contained in the adhesive composition of the present invention does not have a (meth)acrylic acid monomer unit having a carboxylic acid group, and the obtained adhesive composition is an acid-free adhesive composition.

[0042] The glass transition temperature of the (meth)acrylic polymer may be 0° C. or lower, preferably -10° C. or lower, more preferably -20° C. or lower, and further preferably -30° C. or lower. The lower limit of the glass transition temperature of the (meth)acrylic polymer is not particularly limited, but is preferably -80° C. or higher, for example.

[0043] In addition, the glass transition temperature of a (meth)acrylic-based polymer can be calculated from the following FOX formula.

[0044] 1 / Tgp=W1 / Tg1+W2 / Tg2+···+Wn / Tgn

[0045] Tgp is the glass transition temperature of the acrylic polymer, Wn is the weight fraction of each monomer, and Tgn is the glass transition temperature when each monomer forms a homopolymer.

[0046] The weight average molecular weight of the (meth)acrylic polymer is preferably greater than 10,000, more preferably 100,000 or more, and further preferably 200,000 or more. In addition, the weight average molecular weight of the (meth)acrylic polymer is preferably 2 million or less, more preferably 1.5 million or less, and further preferably 1 million or less. It should be noted that the weight average molecular weight of the (meth)acrylic polymer is measured by gel permeation chromatography (GPC), and is a value calculated and obtained by converting a standard curve made using standard polystyrene with known molecular weight. As the (meth)acrylic polymer, a commercially available product can be used, and a product synthesized according to a known method can also be used.

[0047] The (meth) acrylic polymer may also have a (meth) acrylic monomer unit having a ring structure. The (meth) acrylic monomer having a ring structure is preferably a (meth) acrylic monomer having an alicyclic ring or an aromatic ring. As an alicyclic ring, for example, cyclopropane, cyclobutane, cyclopentane, cyclohexane, cycloheptane, cyclooctane, cyclononane, cyclodecane, cycloundecane, cyclododecane, norbornene, norbornadiene, dicyclopentane, tetrahydrofuran, tetrahydropyran, etc. can be cited. It should be noted that the alicyclic ring may also have a spirocyclic structure. As an aromatic ring, for example, benzene, naphthalene, anthracene, pyridine, furan, benzofuran, pyrrole, thiophene, imidazole, oxazole can be cited. Among them, the ring structure is preferably an alicyclic ring, particularly preferably at least one selected from cyclohexane, dicyclopentane, isobornyl and benzene. It should be noted that the above-mentioned ring structure may also have a substituent. Examples of the substituent include a substituent selected from a halogen atom, a haloalkyl group, an alkyl group, an alkenyl group, an acyl group, a hydroxyl group, a hydroxyalkyl group, an alkoxy group, an aryl group, a heteroaryl group, an alicyclic group, a cyano group, an epoxy group, an oxetanyl group, a mercapto group, an amino group, a (meth)acryloyl group, and the like.

[0048] As the (meth) acrylic monomer with a ring structure, for example, cyclohexyl (meth) acrylate, dicyclopentyl (meth) acrylate, dicyclopentenyl (meth) acrylate, isobornyl (meth) acrylate, phenoxyethyl (meth) acrylate, 3-phenoxybenzyl (meth) acrylate, ortho-phenylphenoxyethyl (meth) acrylate, etc. can be cited. The content of the (meth) acrylic monomer unit with a ring structure in the (meth) acrylic polymer is preferably more than 1% by mass, more preferably more than 3% by mass, and further preferably more than 5% by mass relative to the total mass of the (meth) acrylic polymer. In addition, the content of the (meth) acrylic monomer unit with a ring structure in the (meth) acrylic polymer is preferably less than 30% by mass. By making the content of the (meth) acrylic monomer unit with a ring structure within the above range, the whitening resistance and adhesion of the adhesive sheet can be more effectively improved.

[0049] (Meth) acrylic polymers can also contain (meth) acrylic acid alkyl ester units in addition to (meth) acrylic acid monomer units having hydroxyl groups. As examples of (meth) acrylic acid alkyl esters, methyl (meth) acrylate, ethyl (meth) acrylate, butyl (meth) acrylate, isobutyl (meth) acrylate, 2-ethylhexyl (meth) acrylate, nonyl (meth) acrylate, decyl (meth) acrylate, lauryl (meth) acrylate, hexadecyl (meth) acrylate, stearyl (meth) acrylate, behenyl (meth) acrylate and other (meth) acrylic acid alkyl esters, etc. can be cited. The content of the (meth) acrylic acid alkyl ester unit is preferably 30% by mass or more, more preferably 40% by mass or more, and further preferably 50% by mass or more relative to the total mass of the (meth) acrylic acid polymer. In addition, the content of the (meth) acrylic acid alkyl ester unit is preferably 95% by mass or less, preferably 80% by mass or less relative to the total mass of the (meth) acrylic acid polymer. By making the content of the (meth) acrylic acid alkyl ester unit within the above range, the whitening resistance and adhesion of the adhesive sheet can be more effectively improved.

[0050] (Meth) acrylic polymer can also be equipped with (meth) acrylic monomer unit with crosslinking functional group except (meth) acrylic monomer unit with hydroxyl group.As the crosslinking functional group possessed by (meth) acrylic monomer with crosslinking functional group, amide group, amino group, mercapto group, isocyanate group, epoxy group, silanol group can be cited.The content of (meth) acrylic monomer unit with crosslinking functional group in (meth) acrylic polymer is preferably below 10 mass %, more preferably below 5 mass %, further preferably below 3 mass %.By making the content of (meth) acrylic monomer unit with crosslinking functional group in (meth) acrylic polymer be above-mentioned scope, thus can more effectively improve the adhesion of adhesive sheet and adherend.

[0051] The (meth)acrylic polymer may have other monomer units as required. Other monomers may be copolymerizable with the above-mentioned monomer components, and examples thereof include (meth)acrylonitrile, vinyl acetate, vinyl chloride, ethyl vinyl ether, etc. The content of other monomer units in the (meth)acrylic polymer is preferably 10% by mass or less, more preferably 5% by mass or less.

[0052] The adhesive composition may also contain an acrylic syrup A containing a (meth)acrylic polymer. Here, the acrylic syrup A contains at least a (meth)acrylic polymer and a monomer constituting the (meth)acrylic polymer. Therefore, the adhesive composition may contain a monomer constituting the (meth)acrylic polymer in addition to the (meth)acrylic polymer. It should be noted that when the acrylic syrup A contains a monomer constituting the (meth)acrylic polymer, these monomers are polymerized in the process of manufacturing the adhesive sheet to form the (meth)acrylic polymer.

[0053] <Polycarbodiimide>

[0054] The adhesive composition contains polycarbodiimide. Polycarbodiimide is a compound having two or more carbodiimide groups (-N=C=N-) in one molecule. The number of carbodiimide groups contained in one molecule of polycarbodiimide is preferably two or more, more preferably three or more.

[0055] In the present invention, the (meth) acrylic polymer does not substantially contain a (meth) acrylic monomer unit having a carboxylic acid group, and therefore, the polycarbodiimide does not function as a crosslinking agent. That is, in the adhesive sheet formed by the adhesive composition of the present invention, the polycarbodiimide exists without forming a crosslinked structure. Thus, the adhesive sheet can exhibit more excellent adhesion.

[0056] The weight average molecular weight of the polycarbodiimide is preferably 1000 or more, more preferably 1500 or more, and further preferably 2000 or more. In addition, the carbodiimide equivalent is preferably 100 or more, and further preferably 200 or more. The carbodiimide equivalent is preferably 2000 or less, and further preferably 1000 or less. The carbodiimide equivalent refers to the chemical formula weight per 1 mol of the carbodiimide group.

[0057] Examples of the polycarbodiimide include poly(4,4'-dicyclohexylmethanecarbodiimide), poly(4,4'-diphenylmethanecarbodiimide), poly(3,5'-dimethyl-4,4'-biphenylmethanecarbodiimide), poly(p-phenylenecarbodiimide), poly(m-phenylenecarbodiimide), poly(3,5'-dimethyl-4,4'-diphenylmethanecarbodiimide), poly(naphthylenecarbodiimide), poly(1,3-diisopropylphenylenecarbodiimide), poly(1-methyl-3,5-diisopropylphenylenecarbodiimide), poly(1,3,5-triethylphenylenecarbodiimide), poly(triisopropylphenylenecarbodiimide), and p-phenylene-bis(2,6-xylylcarbodiimide). The polycarbodiimide may be used alone or in combination of two or more.

[0058] Polycarbodiimide can be obtained by, for example, subjecting an isocyanate compound such as monoisocyanate or diisocyanate to a carbodiimidization reaction in the presence of a carbodiimidization catalyst (phosphene or the like).

[0059] In addition, polycarbodiimide can also be obtained as a commercial product. Examples of the commercial products include Carbodilite V-02 (manufactured by Nisshinbo Chemical Inc.), Carbodilite V-02B (manufactured by Nisshinbo Chemical Inc.), Carbodilite V-02-L2 (manufactured by Nisshinbo Chemical Inc.), Carbodilite V-03 (manufactured by Nisshinbo Chemical Inc.), Carbodilite V-04 (manufactured by Nisshinbo Chemical Inc.), Carbodilite V-05 (manufactured by Nisshinbo Chemical Inc.), Stabaxol P (manufactured by LANXESS), and Elastostab H01 (manufactured by BASF).

[0060] The content of polycarbodiimide in the adhesive composition is preferably 0.01 mass parts or more, more preferably 0.05 mass parts or more, and further preferably 0.1 mass parts or more, relative to the total mass 100 mass parts of the (meth) acrylic polymer and the monomer constituting the (meth) acrylic polymer. In addition, the content of polycarbodiimide in the adhesive composition is preferably 20 mass parts or less, more preferably 10 mass parts or less, and further preferably 5 mass parts or less, relative to the total mass 100 mass parts of the (meth) acrylic polymer and the monomer constituting the (meth) acrylic polymer. It should be noted that in the adhesive sheet consisting of the adhesive composition, the monomer constituting the (meth) acrylic polymer constitutes the (meth) acrylic polymer, and therefore, the content of polycarbodiimide is preferably the above-mentioned range relative to 100 mass parts of the (meth) acrylic polymer. By making the content of polycarbodiimide be within the above-mentioned range, the adhesive sheet formed by the adhesive composition can exert more excellent adhesion.

[0061] <Tackifying resin>

[0062] The adhesive composition may further include a resin having a glass transition temperature of 20°C or more (excluding the above-mentioned polycarbodiimide). In the present invention, the resin having a glass transition temperature of 20°C or more functions as a tackifying resin (tackifier). The adhesive composition contains a tackifying resin in addition to the (meth)acrylic polymer, thereby improving the compatibility of the components in the adhesive composition, and the adhesive sheet formed by the adhesive composition exhibits better whitening resistance and adhesion.

[0063] The glass transition temperature of the resin (tackifier resin) having a glass transition temperature of 20° C. or higher is preferably 30° C. or higher, more preferably 40° C. or higher, and further preferably 50° C. or higher. In addition, the glass transition temperature of the tackifier resin is preferably 200° C. or lower, more preferably 180° C. or lower, and further preferably 150° C. or lower. By setting the glass transition temperature of the tackifier resin within the above range, the adhesion of the pressure-sensitive adhesive sheet to the adherend can be improved.

[0064] The weight average molecular weight of tackifying resin is preferably more than 3000, more preferably more than 3200, further preferably more than 3500. In addition, the weight average molecular weight of tackifying resin is as long as less than 10000, more preferably less than 9000, further preferably less than 8000. The weight average molecular weight of tackifying resin is measured according to gel permeation chromatography (GPC), and is the value calculated and obtained by using the standard curve made of known standard polystyrene using molecular weight. As this resin, commercially available products can be used, and synthesizers according to known methods can also be used.

[0065] The tackifier resin preferably has substantially no functional group. In this case, the tackifier resin does not form a crosslinked structure with the (meth)acrylic polymer.

[0066] The tackifying resin may also contain a monomer unit having an alicyclic ring. When the tackifying resin contains a monomer unit having an alicyclic ring, the carbon number constituting the alicyclic ring is preferably 6 or more. As the alicyclic ring having a carbon number of 6 or more, for example, cyclohexane, cycloheptane, cyclooctane, cyclononane, cyclodecane, cycloundecane, cyclododecane, norbornene, norbornadiene, dicyclopentane, etc. can be cited.

[0067] As the monomer having an alicyclic ring, for example, isobornyl (meth)acrylate, dicyclopentyl (meth)acrylate, dicyclopentenyl (meth)acrylate, etc. can be preferably used.

[0068] When the tackifying resin includes a monomer unit having an alicyclic ring, the content of the monomer unit having an alicyclic ring is preferably more than 5% by mass, more preferably more than 10% by mass, relative to the total mass of the tackifying resin. In addition, the content of the monomer unit having an alicyclic ring is preferably less than 90% by mass, preferably less than 80% by mass, relative to the total mass of the tackifying resin. By making the content of the monomer unit having an alicyclic ring within the above range, the compatibility of the (meth) acrylic polymer and the tackifying resin can be improved, and the adhesion of the adhesive sheet to the adherend can be more effectively improved.

[0069] The tackifier resin may also contain an alkyl (meth)acrylate unit. As an example of an alkyl (meth)acrylate, methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, lauryl (meth)acrylate, hexadecyl (meth)acrylate, stearyl (meth)acrylate, behenyl (meth)acrylate and the like alkyl (meth)acrylates, etc., may be cited. Wherein, the tackifier resin preferably includes methyl (meth)acrylate. The content of the alkyl (meth)acrylate unit is preferably 10% by mass or more, more preferably 15% by mass or more, relative to the total mass of the tackifier resin. In addition, the content of the alkyl (meth)acrylate unit is preferably 95% by mass or less, preferably 90% by mass or less, relative to the total mass of the tackifier resin. By making the content of the alkyl (meth)acrylate unit be within the above range, the compatibility of the (meth)acrylic polymer and the tackifier resin can be improved, and the adhesion of the adhesive sheet to the adherend can be more effectively improved.

[0070] The tackifying resin may also have other monomer units as required. Other monomers may be copolymerized with the above-mentioned monomer components, for example, (meth) acrylonitrile, vinyl acetate, vinyl chloride, ethyl vinyl ether, etc. The content of other monomer units in the tackifying resin is preferably 10% by mass or less, more preferably 5% by mass or less.

[0071] The content of the tackifying resin in the adhesive composition is preferably 1 mass part or more, more preferably 1.2 mass parts or more, and more preferably 1.5 mass parts or more relative to the total mass 100 mass parts of the monomers constituting the (meth) acrylic polymer and the (meth) acrylic polymer. In addition, the content of the tackifying resin in the adhesive composition is preferably 50 mass parts or less, more preferably 30 mass parts or less, and more preferably 25 mass parts or less relative to the total mass 100 mass parts of the monomers constituting the (meth) acrylic polymer. It should be noted that in the adhesive sheet consisting of the adhesive composition, the monomer constituting the (meth) acrylic polymer constitutes the (meth) acrylic polymer, and therefore, the content of the tackifying resin is preferably the above-mentioned range relative to 100 mass parts of the (meth) acrylic polymer. By making the content of the tackifying resin within the above-mentioned range, the adhesion of the adhesive sheet to the adherend can be improved, and then, the whitening resistance of the adhesive sheet can be more effectively improved.

[0072] <Multifunctional monomer>

[0073] The adhesive composition may further contain a polyfunctional monomer having two or more reactive double bonds in the molecule. The polyfunctional monomer has two or more reactive double bonds, wherein the polyfunctional monomer preferably has two or more and less than five reactive double bonds, and more preferably has two or more and less than four reactive double bonds.

[0074] As for the multifunctional monomer, for example, as a bifunctional monomer, polyethylene glycol diacrylate, alkyl diacrylate, polytetramethylene glycol diacrylate, polypropylene glycol diacrylate, dioxane diacrylate, tricyclodecanol diacrylate, fluorene diacrylate can be cited. In addition, as a monomer having three or more functions, alkoxylated trimethylolpropane triacrylate, alkoxylated glycerol triacrylate, caprolactone-modified isocyanurate triacrylate, pentaerythritol acrylate, alkoxylated pentaerythritol acrylate, (alkoxylated) pentaerythritol acrylate, (alkoxylated) di(trimethylol)propane acrylate, (alkoxylated) dipentaerythritol acrylate, (ethoxylated) polyglycerol acrylate, etc. can be cited.

[0075] As the multifunctional monomer, commercially available products can be used. Examples of commercially available products include difunctional monomer A-200 (polyethylene glycol #200 diacrylate) manufactured by Shin-Nakamura Chemical Industry Co., Ltd., trifunctional monomer A-TMPT ((alkoxylated) trimethylolpropane acrylate), difunctional monomer M240 (polyethylene glycol diacrylate) manufactured by Toagosei Co., Ltd., and tetrafunctional monomer M-408 (di(trimethylol)propane tetraacrylate).

[0076] The multifunctional monomer forms a cross-linked structure with the above-mentioned (meth) acrylic polymer in the adhesive sheet. It should be noted that the content of the multifunctional monomer in the adhesive composition is preferably 0.01 mass parts or more, more preferably 0.05 mass parts or more, relative to the total mass 100 mass parts of the (meth) acrylic polymer and the monomer constituting the (meth) acrylic polymer. In addition, the content of the multifunctional monomer in the adhesive composition is preferably 10 mass parts or less, more preferably 5 mass parts or less, relative to the total mass 100 mass parts of the (meth) acrylic polymer and the monomer constituting the (meth) acrylic polymer. By making the content of the multifunctional monomer be within the above-mentioned range, the hardness of the adhesive sheet can be improved, and the durability, processability and adhesion of the adhesive sheet can be improved.

[0077] <Cross-linking agent>

[0078] The adhesive composition may further include a crosslinking agent. The crosslinking agent may be appropriately selected in consideration of the reactivity with the crosslinking functional group possessed by the (meth) acrylic polymer. For example, it may be selected from known crosslinking agents such as isocyanate compounds, epoxy compounds, oxazoline compounds, aziridine compounds, metal chelate compounds, and butylated melamine compounds. Among them, the crosslinking agent preferably includes at least one selected from isocyanate compounds, epoxy compounds, and metal chelate compounds.

[0079] As isocyanate compounds, for example, toluene diisocyanate, xylene diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, blocked isocyanate, etc. can be cited. As examples of commercial products, toluene diisocyanate compounds (TOSOH CORPORATION, CORONATE L), xylene diisocyanate compounds (Mitsui Chemicals, TAKENATE D-110N), Asahi Chemicals WM44-L70G, etc. can be cited. As epoxy compounds, for example, TETRAD-C (Mitsubishi Gas Chemical Co., Ltd.), TETRAD-X (Mitsubishi Gas Chemical Co., Ltd.) can be cited. As metal chelate compounds, for example, aluminum chelate A (Kawaken Fine Chemicals Co., Ltd.) can be cited.

[0080] The crosslinking agent forms a crosslinked structure with the above-mentioned (meth) acrylic polymer in the adhesive sheet. It should be noted that the content of the crosslinking agent in the adhesive composition is preferably 0.01 parts by mass or more, more preferably 0.05 parts by mass or more, relative to 100 parts by mass of the total mass of the (meth) acrylic polymer and the monomers constituting the (meth) acrylic polymer. In addition, the content of the crosslinking agent in the adhesive composition is preferably 10 parts by mass or less, more preferably 5 parts by mass or less, relative to 100 parts by mass of the total mass of the (meth) acrylic polymer and the monomers constituting the (meth) acrylic polymer. By making the content of the crosslinking agent within the above range, the hardness of the adhesive sheet can be improved, and the durability, processability and adhesion of the adhesive sheet can be improved.

[0081] <Photopolymerization initiator>

[0082] The adhesive composition may further include a photopolymerization initiator. The photopolymerization initiator initiates polymerization of the multifunctional monomer by irradiation with active energy rays. Here, "active energy rays" refer to electromagnetic waves or charged particle rays having energy quanta, and examples thereof include ultraviolet rays, electron beams, visible rays, X-rays, ion beams, etc. Among them, ultraviolet rays or electron beams are preferred, and ultraviolet rays are particularly preferred from the perspective of versatility.

[0083] The photopolymerization initiator is not particularly limited, and examples thereof include acetophenone-based photopolymerization initiators such as 2,2-dimethoxy-2-phenylacetophenone, 1-hydroxycyclohexyl-phenyl ketone, 2-hydroxy-2-methyl-1-phenylpropanone, 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-methylpropanone, and 2-hydroxy-1-(4-(4-(2-hydroxy-2-methylpropionyl)benzyl)phenyl)-2-methyl-1-propanone, acylphosphine oxide-based photopolymerization initiators such as 2,4,6-trimethylbenzoyl-diphenylphosphine oxide and bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, and intramolecular hydrogen abstraction-type photopolymerization initiators such as methyl benzoylformate and 4-methylbenzophenone, as well as oil-soluble polymerization initiators such as oxime ester-based photopolymerization initiators and cationic photopolymerization initiators. Among them, the photopolymerization initiator is preferably at least one selected from the group consisting of acetophenone-based photopolymerization initiators, acylphosphine oxide-based photopolymerization initiators, and oxime ester-based photopolymerization initiators.

[0084] Examples of commercially available products of such acetophenone-based photopolymerization initiators include Esacure One (oligo(2-hydroxy-2-methyl-1-[4-(1-methylvinyl)phenylpropanone], a photoinitiator manufactured by IGM RESINS BV), Omnirad 651 (2,2-dimethoxy-2-phenylacetophenone, manufactured by IGM RESINS BV), Omnirad 184 (1-hydroxycyclohexyl-phenylketone, manufactured by IGM RESINS BV), and Omnirad 1173 (2-hydroxy-2-methyl-1-phenylpropanone, manufactured by IGM RESINS B.V.). Examples of commercially available products of acylphosphine oxide-based photopolymerization initiators include Omnirad 819 (bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, manufactured by IGM RESINS BV), Omnirad TPO (2,4,6-trimethylbenzoyl-diphenylphosphine oxide, manufactured by IGM RESINS BV). RESINS BV), etc.

[0085] The content of the photopolymerization initiator in the adhesive composition is preferably 0.01 parts by mass or more, more preferably 0.05 parts by mass or more, relative to 100 parts by mass of the total mass of the (meth) acrylic polymer and the monomers constituting the (meth) acrylic polymer. In addition, the content of the photopolymerization initiator in the adhesive composition is preferably 10 parts by mass or less, more preferably 5 parts by mass or less, relative to 100 parts by mass of the total mass of the (meth) acrylic polymer and the monomers constituting the (meth) acrylic polymer. By setting the content of the photopolymerization initiator within the above range, the hardness of the adhesive sheet can be increased, and the durability, processability, and adhesion of the adhesive sheet can be improved.

[0086] <Silane coupling agent>

[0087] The adhesive composition may further contain a silane coupling agent. When the adhesive composition contains a silane coupling agent, the adhesion between the adhesive sheet formed from the adhesive composition and the adherend can be further improved.

[0088] Examples of the silane coupling agent include a mercapto-based silane coupling agent containing a mercapto group, an epoxy-based silane coupling agent having an epoxy group, a vinyl-based silane coupling agent having a vinyl group, and an isocyanurate-based silane coupling agent.

[0089] The content of the silane coupling agent in the adhesive composition is preferably 0.01 parts by mass or more, more preferably 0.05 parts by mass or more, and further preferably 0.1 parts by mass or more relative to 100 parts by mass of the total mass of the (meth) acrylic polymer and the monomers constituting the (meth) acrylic polymer. In addition, the content of the silane coupling agent in the adhesive composition is preferably 10 parts by mass or less relative to 100 parts by mass of the total mass of the (meth) acrylic polymer and the monomers constituting the (meth) acrylic polymer. By setting the content of the silane coupling agent within the above range, the adhesion of the adhesive sheet can be more effectively improved.

[0090] <Solvent>

[0091] The adhesive composition may contain a solvent. In this case, the solvent is used to improve the coating suitability of the adhesive composition. Examples of the solvent include hydrocarbons such as hexane, heptane, octane, toluene, xylene, ethylbenzene, cyclohexane, and methylcyclohexane; alcohols such as methanol, ethanol, propanol, isopropanol, butanol, isobutanol, and diacetone alcohol; ethers such as ethyl ether, diisopropyl ether, dioxane, and tetrahydrofuran; ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, isophorone, and cyclohexanone; esters such as methyl acetate, ethyl acetate, butyl acetate, isobutyl acetate, amyl acetate, and ethyl butyrate; polyols such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monomethyl ether acetate, propylene glycol monomethyl ether, propylene glycol monoethyl ether, and propylene glycol monomethyl ether acetate, and derivatives thereof.

[0092] <Other ingredients>

[0093] The adhesive composition may contain other ingredients other than the above within the scope that does not impair the effect of the present invention. As other ingredients, known ingredients used as additives for adhesives can be cited. For example, plasticizers, antioxidants, metal corrosion inhibitors, ultraviolet absorbers, hindered amine compounds and other light stabilizers can be selected as needed. In addition, dyes and pigments can also be added for the purpose of coloring.

[0094] As the plasticizer, for example, a non-functional acrylic polymer may be used. Examples of the non-functional acrylic polymer include a polymer containing only acrylic monomer units having no functional groups other than acrylate groups, and a polymer containing acrylic monomer units having no functional groups other than acrylate groups and non-functional acrylic monomer units. The non-functional acrylic polymer is not cross-linked, and therefore can improve the height difference followability when laminating with the adherend without affecting the adhesiveness.

[0095] Examples of the antioxidant include phenolic antioxidants, amine antioxidants, lactone antioxidants, phosphorus antioxidants, sulfur antioxidants, etc. These antioxidants may be used alone or in combination of two or more.

[0096] As the metal corrosion inhibitor, benzotriazole resins are preferred examples in view of compatibility with the binder and the degree of effect.

[0097] Examples of the ultraviolet absorber include benzotriazole compounds, benzophenone compounds, and triazine compounds.

[0098] (Adhesive Sheet)

[0099] The present invention relates to an adhesive sheet, which is formed by curing the above-mentioned adhesive composition. The adhesive sheet of the present invention may also be formed by thermally drying the above-mentioned adhesive composition, or may be formed by photocuring the above-mentioned adhesive composition. Among them, the adhesive sheet is preferably formed by photocuring the above-mentioned adhesive composition, and when forming the adhesive sheet of the present invention, it is preferred that the adhesive composition is irradiated with active energy rays for a curing reaction. As active energy rays, ultraviolet rays, electron beams, visible rays, X-rays, ion beams, etc. can be cited. Among them, from the viewpoint of versatility, ultraviolet rays or electron beams are preferred, and ultraviolet rays are particularly preferred.

[0100] The adhesive sheet of the present invention is preferably an adhesive sheet and a double-sided adhesive sheet consisting only of an adhesive layer. As a double-sided adhesive sheet, a single-layer adhesive sheet consisting of an adhesive layer, a multi-layer adhesive sheet laminated with a multi-layer adhesive layer, and a multi-layer adhesive sheet laminated with other adhesive layers between an adhesive layer and an adhesive layer can be cited. It should be noted that the adhesive sheet of the present invention can also be a multi-layer adhesive sheet laminated with a support between an adhesive layer and an adhesive layer. In the case where the double-sided adhesive sheet has a support, a transparent support is preferably used as the support. As a support, a general film used in the optical field can be used in the same manner as a transparent substrate. The transparency of this double-sided adhesive sheet as an adhesive sheet as a whole is also excellent, and therefore, it can be suitable for bonding optical components to each other.

[0101] The present invention may also relate to an adhesive sheet with a release sheet, wherein the adhesive sheet has release sheets on both surfaces. In the case where the adhesive sheet of the present invention has release sheets on both surfaces, Figure 1 As shown, the pressure-sensitive adhesive sheet 10 with a release sheet preferably has release sheets 12 a and 12 b on both surfaces of the pressure-sensitive adhesive layer 11 .

[0102] Examples of the release sheet include a release laminate sheet having a release sheet substrate and a release agent layer provided on one surface of the release sheet substrate, or a polyolefin film such as a polyethylene film and a polypropylene film as a polar substrate.

[0103] The release sheet substrate in the release laminate can be made of paper or polymer film. As the release agent constituting the release agent layer, for example, a general-purpose addition-type or condensation-type silicone release agent or a long-chain alkyl compound can be used. It is particularly preferred to use a highly reactive addition-type silicone release agent.

[0104] Specific examples of the silicone-based release agent include BY24-4527 and SD-7220 manufactured by Dow Corning Toray Silicone Co., Ltd. and KS-3600, KS-774 and X62-2600 manufactured by Shin-Etsu Chemical Co., Ltd. In addition, the silicone-based release agent preferably contains a silicon-containing compound having SiO2 units and (CH3)3SiO 1 / 2 Unit or CH2=CH(CH3)SiO 1 / 2 Specific examples of the silicone resin include BY24-843, SD-7292, SHR-1404, etc. manufactured by Dow Corning Toray Silicone Co., Ltd., and KS-3800, X92-183, etc. manufactured by Shin-Etsu Chemical Co., Ltd.

[0105] As the releasable laminated sheet, commercially available products may be used, for example, heavy separator film A71 which is a release-treated polyethylene terephthalate film manufactured by DuPont Teijin Films Co., Ltd. and light separator film A38ST which is a release-treated polyethylene terephthalate film manufactured by DuPont Teijin Films Co., Ltd.

[0106] The adhesive sheet with a release sheet preferably has a pair of release sheets with different release forces on both surfaces of the adhesive sheet. That is, the release sheet is easy to peel off, so it is preferred that the release properties of the release sheet 12a and the release sheet 12b are different. If the release property from one is different from the release property from the other, it becomes easy to peel off only the release sheet with high release property first. In this case, the release properties of the release sheet 12a and the release sheet 12b can be adjusted according to the laminating method and laminating order.

[0107] The thickness of the adhesive sheet can be appropriately set according to the purpose, and is not particularly limited, preferably 5 to 1000 μm, more preferably 8 to 500 μm, and particularly preferably 10 to 300 μm. By setting the thickness of the adhesive sheet to within the above range, the adhesive performance can be maintained, and the oozing and stickiness of the adhesive can be suppressed, so that the processability can be improved. Furthermore, by setting the thickness of the adhesive layer to within the above range, the manufacture of the double-sided adhesive sheet becomes easy.

[0108] <Method for producing adhesive sheet>

[0109] The method for manufacturing the adhesive sheet of the present invention preferably includes the following steps: a step of coating the adhesive composition on the release sheet to form a coating film; a step of heating the coating film, or a step of irradiating the coating film with active energy rays. It should be noted that when the adhesive composition contains a solvent, it preferably includes a heating and drying step. The solvent is removed in the heating and drying step to form an adhesive layer.

[0110] The coating of the adhesive composition can be implemented by using a known coating device. As the coating device, for example, a blade coater, an air knife coater, a roll coater, a rod coater, a gravure coater, a micro gravure coater, a rod blade coater, a lip coater, a die coater, a curtain coater, etc. can be cited.

[0111] In the process of heating the coating film, it is preferred to place the coating film under heating conditions and dry it. The temperature in the heating process is preferably 70°C or higher, more preferably 80°C or higher, and further preferably 85°C or higher. In addition, the temperature in the heating process is preferably 150°C or lower. The treatment time in the heating process is preferably 10 seconds or more, more preferably 1 minute or more, and further preferably 2 minutes or more. In addition, the treatment time in the heating process is preferably 1 hour or less.

[0112] In the step of irradiating the coating film with active energy rays, it is preferred that the accumulated light intensity be 100 to 10,000 mJ / cm 2 The active energy ray is preferably irradiated in a manner of 500 to 5000 mJ / cm 2In the step of irradiating the coating film with active energy rays, the active energy rays may be irradiated in two stages. For example, the irradiation intensity in the second stage may be increased compared to the first stage. By performing such two-stage irradiation, the molecular weight of the polymer contained in the obtained adhesive sheet can be adjusted, and thermal shrinkage of the separator etc. can be suppressed.

[0113] <Application of adhesive sheets>

[0114] The adhesive sheet of the present invention is used to adhere to an adherend, and the adherend is preferably an optical component. As an optical component, each component in an optical product such as a touch panel and an image display device can be cited. As a component of a touch panel, for example, an ITO film having an ITO film on a transparent resin film, an ITO glass having an ITO film on the surface of a glass plate, a transparent conductive film coated with a conductive polymer on a transparent resin film, a hard coating film, a fingerprint-resistant film, etc. can be cited. As a component of an image display device, for example, an anti-reflection film, an orientation film, a polarizing film, a phase difference film, a brightness improvement film, etc. used in a liquid crystal display device can be cited. In addition, the adhesive sheet of the present invention can also be used for the lamination of components such as a liquid crystal component and a touch panel component.

[0115] As materials used in these optical components, glass, polycarbonate, polyethylene terephthalate, polymethyl methacrylate (PMMA), polyethylene naphthalate, cycloolefin polymer, cellulose triacetate, polyimide, cellulose acylate, etc. can be cited. Among them, the adherend preferably contains a resin having a carbonyl group, and particularly preferably contains at least one selected from polycarbonate and PMMA. That is, the adhesive sheet of the present invention is preferably an adhesive sheet for laminating a polycarbonate or PMMA plate.

[0116] Furthermore, in order to improve the adhesion between these optical members and the pressure-sensitive adhesive sheet, the surfaces of the optical members may be subjected to corona treatment or plasma treatment.

[0117] (Laminated body)

[0118] The present invention may also relate to a laminate comprising the above-mentioned adhesive sheet and an adherend. Here, the adherend is preferably an optical component, and the adherend preferably comprises a resin having a carbonyl group, and particularly preferably comprises at least one selected from polycarbonate and PMMA. The laminate of the present invention is preferably a laminate comprising the above-mentioned adhesive sheet and a polycarbonate plate or a PMMA plate. The adhesive sheet of the present invention can exhibit excellent adhesion, particularly to a polycarbonate plate.

[0119] Example

[0120] Below, enumerate embodiment and comparative example, feature of the present invention is further specifically described.Material, dosage, ratio, processing content, processing step etc. shown in following embodiment just can be suitably changed as long as do not depart from the gist of the present invention.Therefore, the scope of the present invention should not be interpreted as the specific example shown below in a limiting sense.

[0121] (Example 1)

[0122] <Method for producing acrylic polymer A>

[0123] In a 2L flask equipped with a stirrer, a nitrogen inlet tube, a condenser, and a thermometer, 325 g of butyl acrylate, 150 g of 4-hydroxybutyl acrylate, 25 g of dicyclopentyl acrylate, and 750 g of ethyl acetate were added, and nitrogen replacement was performed at a nitrogen flow rate of 300 ml / min for 60 minutes. The nitrogen flow rate was then reduced to 100 ml / min, and the temperature was raised to 70°C in a water bath and heated. 0.1 g of AIBN was added, and the reaction was carried out for 1 hour while controlling the exotherm, and then 0.5 g of AIBN was added. After reacting for 6 hours, the reaction was cooled to 50°C. As described above, an acrylic polymer A having a solid content concentration of 40% by mass and a weight average molecular weight of about 500,000 was obtained.

[0124] <Manufacturing of adhesive sheets>

[0125] 0.5 g of polycarbodiimide (Carbodilite V-02B manufactured by Nisshinbo Chemical Inc.) and 0.5 g of a crosslinking agent (CORONATE L manufactured by Tosoh) were added to 100 g of acrylic polymer A, and stirred and degassed to obtain an adhesive composition. The adhesive composition was applied to a 100 μm thick polyester film coated with a silicone release agent so that the thickness of the adhesive layer after drying was 88 μm, and dried in a dryer at 90° C. for 3 minutes. Thereafter, the adhesive layer obtained in the same manner was laminated and left to stand at room temperature for 7 days to obtain an adhesive sheet having a thickness of 175 μm.

[0126] (Example 2)

[0127] <Method for producing acrylic polymer B>

[0128] In a 2L flask equipped with a stirrer, a nitrogen inlet tube, a condenser, and a thermometer, 620 g of 2-ethylhexyl acrylate, 290 g of 4-hydroxybutyl acrylate, 90 g of cyclohexyl methacrylate, and 0.2 g of n-dodecyl mercaptan were added, and nitrogen replacement was performed at a nitrogen flow rate of 300 ml / min for 60 minutes. The nitrogen flow rate was reduced to 100 ml / min, and the temperature was raised to 65°C in a water bath and heated. 0.15 g of AIBN was added, and the reaction was carried out for 30 minutes while controlling the exotherm, and then cooled to 50°C. Additional monomers were added to the flask in such a manner as to achieve the above-mentioned monomer ratio, and the solid content concentration was adjusted to 20%. As described above, a slurry B containing an acrylic polymer B having a solid content concentration of 20% by mass and a weight average molecular weight of about 800,000 was obtained.

[0129] <Method for producing tackifier resin a>

[0130] In a 2L flask equipped with a stirrer, a nitrogen inlet tube, a condenser, and a thermometer, 250 g of methyl methacrylate, 250 g of isobornyl methacrylate, 20 g of n-dodecyl mercaptan, 500 g of ethyl acetate, and 200 g of methyl ethyl ketone were added, and nitrogen replacement was performed at a nitrogen flow rate of 300 ml / min for 60 minutes, and then the nitrogen flow rate was reduced to 100 ml / min, and the temperature was raised to 70°C in a water bath, and heating was stopped. 2 g of AIBN was added, and the reaction was carried out for 3 hours while controlling the exotherm, and then 3 g of AIBN was added. After reacting for 4 hours, it was cooled to 30°C. As above, a tackifying resin a with a weight average molecular weight of 6000 and a glass transition temperature of 95°C was obtained.

[0131] <Manufacturing of adhesive sheets>

[0132] Tackifying resin a was dried at 100°C for 5 hours to remove the solvent. 7 g of tackifying resin a from which the solvent was removed, 0.3 g of polycarbodiimide (Carbodilite V-03 manufactured by Nisshinbo Chemical Inc.), 0.4 g of multifunctional monomer (NK ester A-200 manufactured by Shin-Nakamura Chemical Co., Ltd.), and 0.3 g of photopolymerization initiator (Esacure One manufactured by IGM Resins BV) were added to 100 g of slurry B, and stirred and degassed to obtain an adhesive composition. The adhesive composition was coated on a 100 μm thick polyester film coated with a silicone release agent to a thickness of 175 μm, and after lamination with a 75 μm thick polyester film coated with a silicone release agent, the illuminance was 5 mW / cm 2 , the cumulative illuminance becomes 900mJ / cm 2 The chemical lamp is irradiated in such a way that the illumination becomes 200mW / cm 2 , the cumulative illuminance becomes 2000mJ / cm 2The adhesive sheet was obtained by irradiating the sample with a high pressure mercury lamp.

[0133] (Example 3)

[0134] <Method for producing acrylic polymer C>

[0135] In a 2L flask equipped with a stirrer, a nitrogen inlet tube, a condenser, and a thermometer, 650 g of butyl acrylate, 270 g of 4-hydroxybutyl acrylate, 80 g of dicyclopentyl acrylate, and 0.2 g of n-dodecyl mercaptan were added, and nitrogen replacement was performed at a nitrogen flow rate of 300 ml / min for 60 minutes. The nitrogen flow rate was reduced to 100 ml / min, and the temperature was raised to 60°C in a water bath and heated. 0.15 g of AIBN was added, and the reaction was controlled while exothermic reaction for 30 minutes, and then cooled to 50°C. Additional monomers were added to the flask in such a manner as to achieve the above-mentioned monomer ratio, and the heating surplus was adjusted to 20%. As described above, a slurry C containing an acrylic polymer C having a solid content concentration of 20% by mass and a weight average molecular weight of about 800,000 was obtained.

[0136] <Method for producing tackifier resin b>

[0137] In a 2L flask equipped with a stirrer, a nitrogen inlet tube, a condenser, and a thermometer, 250 g of methyl methacrylate, 250 g of dicyclopentyl methacrylate, 25 g of n-dodecyl mercaptan, 500 g of ethyl acetate, and 200 g of methyl ethyl ketone were added, and nitrogen replacement was performed for 60 minutes at a nitrogen flow rate of 300 ml / min, and then the nitrogen flow rate was reduced to 100 ml / min, and the temperature was raised to 70°C in a water bath, and heating was stopped. 2 g of AIBN was added, and the reaction was carried out for 3 hours while controlling the exotherm, and then 3 g of AIBN was added. After reacting for 4 hours, it was cooled to 30°C. As above, a tackifying resin b with a weight average molecular weight of 5000 and a glass transition temperature of 90°C was obtained.

[0138] <Manufacturing of adhesive sheets>

[0139] Tackifying resin b was dried at 100°C for 5 hours to remove the solvent. 5 g of tackifying resin b from which the solvent was removed, 0.2 g of polycarbodiimide (Carbodilite V-05 manufactured by Nisshinbo Chemical Inc.), 0.3 g of multifunctional monomer (NK ester A-200 manufactured by Shin-Nakamura Chemical Co., Ltd.), and 0.3 g of photopolymerization initiator (Esacure One manufactured by IGM Resins BV) were added to 100 g of slurry C, and stirred and degassed to obtain an adhesive composition. Using this adhesive composition, an adhesive sheet was obtained in the same manner as in Example 2 except for the above.

[0140] (Comparative Example 1)

[0141] <Method for producing acrylic polymer D>

[0142] In a 2L flask equipped with a stirrer, a nitrogen inlet tube, a condenser, and a thermometer, 350 g of butyl acrylate, 150 g of 4-hydroxybutyl acrylate, and 750 g of ethyl acetate were added, and nitrogen replacement was performed at a nitrogen flow rate of 300 ml / min for 60 minutes. The nitrogen flow rate was then reduced to 100 ml / min, and the temperature was raised to 70°C in a water bath and heated. 0.1 g of AIBN was added, and the reaction was carried out for 1 hour while controlling the exotherm, and then 0.5 g of AIBN was added, and the reaction was carried out for 6 hours, and then cooled to 50°C. As described above, an acrylic polymer D having a solid content concentration of 40% by mass and a weight average molecular weight of about 500,000 was obtained.

[0143] <Method for producing tackifier resin a>

[0144] In the same manner as in Example 2, tackifier resin a was obtained.

[0145] <Manufacturing of adhesive sheets>

[0146] Tackifier resin a was dried at 100°C for 5 hours to remove the solvent. 3 g of tackifier resin a from which the solvent was removed and 0.5 g of a crosslinking agent (CORONATE L manufactured by Tosoh) were added to 100 g of acrylic polymer D, and stirred and degassed to obtain an adhesive composition. Using this adhesive composition, an adhesive sheet was obtained in the same manner as in Example 1 except for the above.

[0147] (Comparative Example 2)

[0148] <Method for producing acrylic polymer B>

[0149] In the same manner as in Example 2, a syrup B containing an acrylic polymer B was obtained.

[0150] <Method for producing tackifier resin a>

[0151] In the same manner as in Example 2, tackifier resin a was obtained.

[0152] <Manufacturing of adhesive sheets>

[0153] Tackifying resin a was dried at 100°C for 5 hours to remove the solvent. 7 g of tackifying resin a from which the solvent was removed, 0.5 g of carbodiimide compound (Lanxess Energizing Chemistry, Stabaxol I (N,N'-bis(2,6-diisopropylphenyl)carbodiimide)), 0.4 g of multifunctional monomer (NKester A-200, Shin-Nakamura Chemical Co., Ltd.), and 0.3 g of photopolymerization initiator (IGM Resins BV, Esacure One) were added to 100 g of slurry B, and stirred and degassed to obtain an adhesive composition. Using this adhesive composition, an adhesive sheet was obtained in the same manner as in Example 2 except that.

[0154] (Comparative Example 3)

[0155] <Method for producing acrylic polymer E>

[0156] In a 2L flask equipped with a stirrer, a nitrogen inlet tube, a condenser, and a thermometer, 900 g of butyl acrylate, 100 g of 4-hydroxybutyl acrylate, and 0.2 g of n-dodecyl mercaptan were added, and nitrogen replacement was performed at a nitrogen flow rate of 300 ml / min for 60 minutes. The nitrogen flow rate was reduced to 100 ml / min, and the temperature was raised to 60°C in a water bath and heated. 0.15 g of AIBN was added, and the reaction was controlled while exothermic reaction was performed for 30 minutes, and then cooled to 50°C. Additional monomers were added to the flask in such a manner as to achieve the above-mentioned monomer ratio, and the heating surplus was adjusted to 20%. As described above, a slurry E containing an acrylic polymer E having a solid content concentration of 20% by mass and a weight average molecular weight of about 800,000 was obtained.

[0157] <Method for producing tackifier resin b>

[0158] In the same manner as in Example 3, tackifier resin b was obtained.

[0159] <Manufacturing of adhesive sheets>

[0160] Tackifier resin b was dried at 100°C for 5 hours to remove the solvent. 7 g of tackifier resin b from which the solvent was removed, 0.25 g of polycarbodiimide (Carbodilite V-02B manufactured by Nisshinbo Chemical Inc.), 0.5 g of multifunctional monomer (NK ester A-200 manufactured by Shin-Nakamura Chemical Co., Ltd.), and 0.3 g of photopolymerization initiator (Esacure One manufactured by IGM Resins BV) were added to 100 g of slurry E, and stirred and degassed to obtain an adhesive composition. Using this adhesive composition, an adhesive sheet was obtained in the same manner as in Example 2 except for the above.

[0161] (Measurement and evaluation)

[0162] (Calculation of Glass Transition Temperature of (Meth)Acrylic Polymer)

[0163] The glass transition temperature of the acrylic polymer can be obtained according to the following FOX formula.

[0164] 1 / Tgp=W1 / Tg1+W2 / Tg2+···+Wn / Tgn

[0165] Tgp is the glass transition temperature of the acrylic polymer, Wn is the weight fraction of each monomer, and Tgn is the glass transition temperature when each monomer forms a homopolymer.

[0166] (Determination of glass transition temperature of tackifying resin)

[0167] The glass transition temperature of the tackifier resin was measured using DSC6200 manufactured by Seiko Instruments Inc. A control was set to 10 mg of aluminum oxide, and about 10 mg of the solvent-free product of the tackifier resin was placed in an aluminum sample pan with a diameter of 5 mm, and the temperature was raised from 0° C. to 150° C. at a heating rate of 10° C. / min in an environment with a nitrogen flow rate of 50 ml / min. At this time, the inflection point at which the specific heat changes was read as the glass transition temperature of the tackifier resin.

[0168] (Wet heat constant load)

[0169] The adhesive sheets obtained in the examples and comparative examples were bonded to a 100 μm thick polyester film (Toyobo A4300) that was treated for easy bonding, and cut so that the bonded portion had a width of 25 mm and a length of 50 mm. Next, they were adhered to a 1 mm thick polycarbonate sheet (Teijin Panlite 1151) or a 1 mm thick polymethyl methacrylate laminate sheet (Kuraray MT3LTR), and then pressed with a 2 kg roller twice. After that, they were treated in an autoclave at a temperature of 30°C and a pressure of 0.5 MPa for 30 minutes, and left to stand for 1 day at atmospheric pressure and room temperature to serve as an evaluation laminate.

[0170] The evaluation laminate was placed in a constant temperature and humidity chamber at 85°C and 85% relative humidity for 30 minutes, and then placed on a table with the polyester film side facing downward. Next, a 100 g weight was hung on the end of the polyester film, and the time from when the adhesive layer was peeled off from the polycarbonate sheet or polymethyl methacrylate laminate sheet surface to when the weight fell was measured, and the adhesion to the adherend was evaluated using the following criteria.

[0171] A: The weight does not fall even after 30 minutes.

[0172] B: The weight does not fall even after 15 minutes, but falls before 30 minutes.

[0173] C: The weight falls before 15 minutes have passed

[0174] (Whitening resistance (transparency))

[0175] A glass plate (Matsunami, width 52 mm, length 76 mm, thickness 1 mm) and a PMMA-PC laminate sheet (Kuraray, MT3LTR, width 55 mm, length 80 mm, thickness 1 mm) were respectively bonded to the respective surfaces of the adhesive sheets obtained in the embodiments and comparative examples, and then treated in an autoclave at a temperature of 30° C. and a pressure of 0.5 MPa for 30 minutes, and then left to stand at atmospheric pressure and room temperature for 1 day to prepare a laminate for evaluation.

[0176] The evaluation laminate was left standing in a constant temperature and humidity chamber at 85°C and 85% relative humidity for 7 days, then left standing at room temperature for 1 hour. The haze value of the evaluation laminate was measured using HM-150 from Murakami Color Research Laboratory and evaluated based on the following criteria.

[0177] A: Haze value is less than 1.5

[0178] B: Haze value is 1.5 or more and less than 3

[0179] C: Haze value is 3 or more

[0180] [Table 1]

[0181]

[0182] BA: Butyl acrylate

[0183] 2EHA: 2-Ethylhexyl acrylate

[0184] 4HBA: 4-Hydroxybutyl acrylate

[0185] CHMA: Cyclohexyl methacrylate

[0186] DCPA: Dicyclopentyl acrylate

[0187] MMA: Methyl Methacrylate

[0188] IBXMA: Isobornyl methacrylate

[0189] DCPMA: Dicyclopentyl methacrylate

[0190] In the examples, the adhesion to the adherend was improved compared to the comparative examples. In particular, the adhesion to the polycarbonate plate was good in the examples. In addition, in the examples, an adhesive sheet with excellent transparency (excellent whitening resistance) was obtained.

Claims

1. An adhesive sheet, which is formed from the following adhesive composition, wherein the adhesive composition comprises: polycarbodiimide and a (meth)acrylic polymer having a glass transition temperature of 0° C. or less, The (meth)acrylic polymer comprises a (meth)acrylic monomer unit having a hydroxyl group. The content of the (meth)acrylic monomer unit having a hydroxyl group in the (meth)acrylic polymer is 20% by mass or more relative to the total mass of the (meth)acrylic polymer. The content of the (meth)acrylic acid monomer unit having a carboxylic acid group in the (meth)acrylic acid polymer is 0.1% by mass or less, In the adhesive sheet, the polycarbodiimide is present without forming a cross-linked structure. The weight average molecular weight of the polycarbodiimide is greater than 1000, and the carbodiimide equivalent is 100 to 2000.

2. The adhesive sheet according to claim 1, wherein The adhesive composition further includes a resin having a glass transition temperature of 20° C. or higher.

3. The adhesive sheet according to claim 1, wherein The adhesive composition further includes a multifunctional monomer.

4. The adhesive sheet according to claim 1, wherein The adhesive composition further includes a cross-linking agent.

5. The adhesive sheet according to claim 1, wherein The adhesive composition further includes a photopolymerization initiator.

6. The adhesive sheet according to any one of claims 1 to 5, which is used for bonding an adherend. in, The adherend contains a resin having a carbonyl group.

7. The adhesive sheet according to claim 6, wherein The adherend includes at least one selected from the group consisting of polycarbonate and polymethyl methacrylate.

8. A laminate comprising an adherend and the pressure-sensitive adhesive sheet according to any one of claims 1 to 5, in, The adherend includes at least one selected from the group consisting of polycarbonate and polymethyl methacrylate.

Citation Information

Patent Citations

  • Pressure-sensitive adhesive composition, pressure-sensitive adhesive and pressure-sensitive adhesive sheet each obtained using the same

    JP2020143211A

  • Adhesive composition

    JP2004067803A

  • Adhesive composition, adhesive and adhesive sheet

    JP2014169382A