A method for producing martensitic steel based on twin-roll casting process

Through the double-roll casting and rolling process, aerosol cooling, temperature-controlled coiling and online tempering technology, the problems of poor molding performance and high energy consumption in traditional martensitic steel production are solved, and the combination of high strength and good molding performance is achieved. Reduces production costs and energy consumption.

CN117431374BActive Publication Date: 2024-11-19ZHANGJIAGANG ZHONGMEI UCS TECH CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311604899.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-29
Publication Date
2024-11-19
Estimated Expiration
2043-11-29

AI Technical Summary

Technical Problem

The traditional martensite steel production process has problems such as poor molding performance, high energy consumption and high cost. Especially when producing thin-specification martensite steel, it is difficult to achieve a combination of high strength and good molding performance.

Method used

The double-roll casting and rolling process is used to produce martensite steel, which is carried out through aerosol cooling and temperature-controlled coiling, and is tempered online using the residual heat of the steel coil, which avoids high-temperature annealing and secondary heating in traditional processes, and controls the precipitation behavior of carbides. Achieve a combination of high strength and good molding performance.

Benefits of technology

It significantly reduces production costs and energy consumption, achieves high strength and good molding performance of martensitic steel, with a minimum bending radius of 90° bending reaching 2mm, and there is no need to add microalloy elements to stabilize the production of high-strength hot-rolled strips.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117431374B_ABST
    Figure CN117431374B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of steel production, and specifically relates to a method for producing martensitic steel based on a twin-roll casting process. The method of the present invention is based on a short-process production process of twin-roll casting to continuously cast thin strips, and then the hot-rolled strip is subjected to aerosol cooling, and the cooling rate of the aerosol cooling is 60-180°C / s. f ‑150℃~M f The steel strip can be coiled in the range of ‑30°C. After coiling, the online waste heat is fully utilized, or the steel strip is tempered in a hood for heat preservation, so that martensitic ultra-high strength steel with good cold bending performance can be obtained. The martensitic steel produced according to the method of the present invention has the characteristics of thin thickness and high strength. The process design of self-tempering using waste heat also solves the problems of poor cold bending performance of traditional martensitic steel and easy cracking under strong cold process, so that the production cost and energy consumption of martensitic steel are significantly reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of steel production, and in particular relates to a method for producing martensitic steel based on a twin-roll casting process. Background Art

[0002] Ultra-high strength steel is an important direction for the development of lightweight automobiles. Advanced high strength steel (AHSS) has been increasingly researched and developed. The main structure of advanced high strength steel (AHSS) generally contains two or more phases of bainite, martensite, residual austenite and ferrite. The strength is further improved through phase transformation on the basis of strengthening mechanisms such as solid solution strengthening, precipitation strengthening, dispersion strengthening and fine grain strengthening. Martensitic steel is the highest strength steel grade among the current lightweight steels for automobiles, and is mainly used for structural parts of passenger cars.

[0003] Martensitic steel has high strength, but its formability is poor. Therefore, it is difficult to manufacture complex structural parts using traditional stamping processes. At present, martensitic steel is generally formed into door anti-collision bars, bumper reinforcement beams, A-pillars, B-pillars, door frame reinforcement beams and other cross-section parts through multiple cold bending processes. Therefore, the minimum bending radius of the 90° bending test is an important indicator that determines the formability of martensitic steel.

[0004] At present, the thin-gauge martensitic steel with a thickness of 0.8~1.8mm on the market is all produced by cold rolling process. During the annealing process, the strip steel needs to be heated to above the A3 critical point, then cooled to room temperature by water cooling, high hydrogen, etc., and then reheated to 200~280℃ for several minutes, and then coiled at room temperature after air cooling. This process has defects, mainly in: high requirements for continuous annealing equipment, high cost of high hydrogen cooling, and high energy consumption in the annealing process.

[0005] Thin-gauge martensitic steel with a thickness of 0.8-1.8 mm cannot be produced using traditional hot rolling processes. The strength level of traditional hot-rolled martensitic steel is generally 800-1200 MPa, the thickness specification is generally 2.0-6.0 mm, and there are problems such as poor plate shape, large performance fluctuations, and poor dimensional accuracy control. Summary of the invention

[0006] Therefore, the object of the present invention is to provide a method for producing high-formability martensitic steel based on a twin-roll casting process to overcome the shortcomings of the prior art.

[0007] In the twin-roll casting process, the solidification rate of the molten steel after contacting the cooling casting rolls can reach more than 1000℃ / s. Under sub-rapid solidification conditions, alloy elements and residual harmful elements in the molten steel are not easy to be segregated and precipitated. The cast strip is rolled through a single hot rolling, and the martensitic steel coil can be obtained by mist cooling to a certain temperature. The martensitic steel produced by the twin-roll casting process of the present invention does not need to be heated after coiling, and can be tempered using online waste heat or insulation under a heat preservation hood. The minimum bending radius of the produced martensitic steel at 90° can reach 2mm. Furthermore, the present invention regulates the precipitation behavior of martensitic steel carbides by changing the coiling temperature, and has good forming properties while achieving high strength and thin specifications, producing technical effects that are difficult to achieve with traditional hot-rolled products.

[0008] Specifically, the present invention adopts the following technical solutions:

[0009] According to a first aspect of the present invention, a method for producing martensitic steel based on a twin-roll casting process is proposed, the method comprising the following steps:

[0010] 1) Strip casting:

[0011] A twin-roll casting process is used to continuously cast a thin strip to obtain a cast strip, and the cast strip is subjected to a single hot rolling to obtain a rolled strip with a thickness of 0.8 to 1.8 mm;

[0012] 2) Aerosol cooling:

[0013] The rolled strip obtained in step 1) is subjected to gas mist cooling to obtain a martensitic thin strip, wherein the cooling rate of the gas mist cooling is 60-180°C / s;

[0014] 3) Temperature controlled coiling:

[0015] The martensitic thin strip obtained in step 2) is coiled at a controlled temperature to obtain a martensitic hot coil, wherein the coiling temperature is controlled to be M f -150℃ ~ M f -30℃,M f is the martensitic transformation completion temperature of the thin strip, M f Determined according to the following formula:

[0016] Mf(℃)=539-423*C-30.4*Mn-20*Si-12.1*Cr-110;

[0017] 4) Tempering treatment:

[0018] The martensitic hot coil obtained in step 3) is tempered online using the residual heat of the steel coil, or is placed in a hood for low-temperature tempering to obtain a martensitic finished coil.

[0019] According to the method for producing martensitic steel based on the twin-roll casting process of the present invention, preferably, the method further comprises: after the mist cooling in step 2), spraying high-pressure gas onto the plate surface of the rolled strip to dry the cooling water, thereby eliminating water marks or water stains on the surface of the strip at the cooling outlet.

[0020] According to the method for producing martensitic steel based on twin-roll casting process of the present invention, preferably, in step 4), utilizing the residual heat of the steel coil for online tempering further comprises: online tempering of the hot coil in the intermediate warehouse: placing the martensitic hot coil in the intermediate warehouse, wherein the storage temperature of the martensitic hot coil is no more than 20°C lower than the coiling temperature, and the steel coil is left to stand for more than 2 days and slowly cooled to room temperature, wherein the slow cooling rate is lower than 4°C / h, so as to utilize the residual heat of the steel coil to perform long-term online tempering of the martensitic structure in this process.

[0021] According to the method for producing martensitic steel based on twin-roll casting process of the present invention, preferably, in step 4), utilizing the waste heat of the steel coil for online tempering further comprises: online tempering in a fully enclosed insulation pit: placing the hot martensitic coil in a fully enclosed insulation pit for more than 2 days and slowly cooling it to room temperature, wherein the pit entry temperature drops by no more than 20°C compared to the coiling temperature, and the slow cooling rate is less than 2.5°C / h.

[0022] According to the method for producing martensitic steel based on twin-roll casting process of the present invention, preferably, in step 4), the heat preservation and low-temperature tempering in the hood further comprises: placing the martensitic hot coil in a heatable heat preservation hood for heat preservation for 1 to 2 days, wherein the temperature entering the hood drops by no more than 20°C compared with the coiling temperature, wherein the temperature fluctuation in the hood does not exceed 20°C, and air cooling to room temperature after exiting the hood.

[0023] According to a second aspect of the present invention, a martensitic steel is provided. The martensitic steel is produced using the method for producing martensitic steel based on a twin-roll casting process according to the present invention.

[0024] According to the martensitic steel of the present invention, preferably, a 90° bending test is performed on the martensitic steel thin strip obtained after online tempering in the hot coil intermediate warehouse or online tempering in the fully enclosed insulation pit. When the bending radius is ≥2a, the bending part will not crack, where a is the thickness of the steel plate.

[0025] According to the martensitic steel of the present invention, preferably, a 90° bending test is performed on the martensitic steel thin strip obtained after being heat-insulated and low-temperature tempered in a hood, and no cracks will occur at the bending point when the bending radius is ≥1.5a, wherein a is the thickness of the steel plate.

[0026] According to the martensitic steel of the present invention, preferably, the microstructure of the martensitic steel mainly comprises lath-shaped tempered martensite, and the rest comprises a small amount of retained austenite and lower bainite.

[0027] According to the martensitic steel of the present invention, preferably, the lath-shaped tempered martensite contains dispersed thin rod-shaped ε carbides between its structures.

[0028] Beneficial technical effects

[0029] Compared with the prior art, the technical concept and corresponding technical solution of the present invention can at least achieve the following beneficial technical effects:

[0030] (1) It can be seen from the above technical scheme that the present invention provides a method for producing high-formability martensitic steel based on a twin-roll casting process. This method does not require heating the steel strip to a temperature above the Ac3 critical point for forced cooling, nor does it require secondary heating of the steel strip for online tempering. Instead, it only requires controlling the coiling temperature to achieve tempering using the waste heat of the production line. Compared with traditional cold-rolled martensitic steel, this method significantly reduces production costs and energy consumption.

[0031] (2) The martensitic steel hot-rolled strip provided by the present invention is thin in thickness and high in strength, and can replace the traditional thick-gauge high-strength hot-rolled strip products. By adjusting the mist cooling process, the martensitic-based hot-rolled thin strip can be stably produced. Compared with the traditional hot-rolled martensitic steel, the strength grade and specification span have obvious advantages.

[0032] (3) The hot-rolled thin strip of martensitic steel provided by the present invention can control the decomposition behavior of C supersaturated martensite by regulating the cooling intensity and the residual heat tempering process, and the martensitic steel thin strip is tempered at a temperature range of 50 to 250°C for a long time at low temperature, which effectively eliminates the internal stress generated by the strong cooling process and more effectively avoids the coarse ε carbides between the martensitic laths formed by tempering in the temperature range of 250 to 400°C, so that there is no need to strictly control P and S in the molten steel to suppress temper brittleness, nor is there any need to increase the silicon content to regulate the precipitation behavior of ε carbides. Finally, the present invention can produce hot-rolled thin strips of martensitic steel with high strength and good cold bending properties without adding microalloying elements. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings of the embodiments are briefly introduced below. Obviously, the drawings in the following description only relate to some embodiments of the present invention, but are not intended to limit the present invention.

[0034] Figures 1 to 3 The microstructure photographs of the martensitic steel produced according to Examples 1 to 3 of the present invention, wherein the scale in the figure is 100 μm. DETAILED DESCRIPTION

[0035] In order to make the purpose, technical solution and advantages of the embodiment of the present invention clearer, the technical solution of the embodiment of the present invention will be clearly and completely described below. Obviously, the described embodiment is a part of the embodiment of the present invention, not all of the embodiments. Based on the described embodiment of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0036] Unless otherwise defined, technical or scientific terms used in the present invention shall have the common meanings understood by one of ordinary skill in the art to which the present invention belongs.

[0037] The following are embodiments of the present invention. The described embodiments are only a part of the embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments that can be obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0038] The present invention discloses a method for producing high-formability martensitic steel based on a twin-roll casting process, comprising the steps of:

[0039] 1) Thin strip continuous casting is carried out based on the short process production process of twin-roll casting and rolling, and the cast strip is hot rolled in one pass to obtain a rolled strip;

[0040] 2) performing mist cooling on the rolled strip obtained in step 1) to obtain a primary martensitic structure;

[0041] 3) coiling the thin strip in step 2) under controlled temperature to obtain a martensitic steel hot coil;

[0042] 4) The martensitic hot coil obtained in step 3) is tempered online using the residual heat of the steel coil, or is placed in a hood for low-temperature tempering to obtain a finished coil.

[0043] The present invention is described in detail below based on specific embodiments.

[0044] Example 1

[0045] (1) Smelting: Electric furnace steelmaking, VD furnace degassing, LF refining, to obtain qualified molten steel, the weight percentage is:

[0046] C: 0.23%; Si: 0.41%; Mn: 1.68%; Cr: 0.63%; the balance is iron and inevitable impurity elements.

[0047] (2) Strip casting: The molten steel with qualified composition is cast into thin strips by twin-roll casting to obtain a cast strip with a thickness of 2.1 mm. The cast strip is then hot-rolled into a 1.7 mm thin strip at a temperature of 1030°C with a reduction of 19%.

[0048] (3) Cooling and coiling: The hot-rolled thin strip is cooled to 170°C at a rate of 105°C / s. After cooling, high-pressure gas is sprayed onto the plate surface and the hot-rolled coil is obtained after coiling at 145°C.

[0049] (4) Residual heat tempering: After the thin strip steel coil is placed in the intermediate warehouse for slow cooling for 3 days, the hot-rolled thin strip product is obtained.

[0050] Table 1 Mechanical properties of martensitic steel obtained in Example 1

[0051]

[0052] Figure 1 This is a microstructure photograph of the martensitic steel obtained in Example 1.

[0053] Example 2

[0054] (1) Smelting: Electric furnace steelmaking, VD furnace degassing, LF refining, to obtain qualified molten steel, the weight percentage is:

[0055] C: 0.22%; Si: 0.40%; Mn: 1.53%; Cr: 0.42%; the balance is iron and inevitable impurity elements.

[0056] (2) Strip casting: The molten steel with qualified composition is cast into thin strips by twin-roll casting to obtain a cast strip with a thickness of 1.9 mm. The cast strip is then hot-rolled into a 1.5 mm thin strip at a temperature of 1050°C with a reduction of 21%.

[0057] (3) Cooling and coiling: The hot-rolled thin strip is cooled to 200°C at a rate of 100°C / s. After cooling, high-pressure gas is sprayed onto the plate surface and the hot-rolled coil is obtained after being coiled at 150°C.

[0058] (4) Residual heat tempering: After the thin strip steel coil is placed in a fully enclosed insulation pit and left to stand for 3 days, the hot-rolled thin strip product is obtained.

[0059] Table 2 Mechanical properties of martensitic steel obtained in Example 2

[0060]

[0061] Figure 2 This is a microstructure photograph of the martensitic steel obtained in Example 2.

[0062] Example 3

[0063] (1) Smelting: Electric furnace steelmaking, VD furnace degassing, LF refining, to obtain qualified molten steel with the following weight percentages: C: 0.24%; Si: 0.43%; Mn: 1.72%; Cr: 0.65%; the remainder is iron and unavoidable impurity elements.

[0064] (2) Strip casting: The molten steel with qualified composition is cast into thin strips by twin-roll casting to obtain a cast strip with a thickness of 1.85 mm. The cast strip is then hot-rolled into a 1.4 mm thin strip at a temperature of 1000°C with a reduction of 24% in one pass.

[0065] (3) Cooling and coiling: The hot-rolled thin strip is cooled to 300°C at a rate of 80°C / s. After cooling, high-pressure gas is sprayed onto the plate surface and the hot-rolled coil is obtained after coiling at 220°C.

[0066] (4) Insulation and tempering: The thin strip steel coil is placed in an insulation cover for 4 days and then taken out and air-cooled to obtain a hot-rolled thin strip product.

[0067] Table 3 shows the mechanical properties of the martensitic steel obtained in Example 3

[0068]

[0069] Figure 3 This is a microstructure photograph of the martensitic steel obtained in Example 3.

[0070] The above description is only a specific implementation of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for producing martensitic steel based on a twin-roll casting process, characterized in that: The method comprises the following steps: 1) Thin strip continuous casting: A twin-roll casting process is used to continuously cast a thin strip to obtain a cast strip, and the cast strip is subjected to a hot rolling process to obtain a rolled strip with a thickness of 0.8 to 1.8 mm; 2) Aerosol cooling: The strip obtained in step 1) is subjected to mist cooling to obtain a martensitic thin strip, wherein the cooling rate of the mist cooling is 60 to 180° C. / s, and after the mist cooling, high-pressure gas is sprayed on the plate surface of the strip to dry the cooling water, thereby eliminating water marks or water stains on the strip surface at the cooling outlet; 3) Temperature controlled coiling: The martensitic thin strip obtained in step 2) is temperature-controlled coiled to obtain a martensitic hot coil, wherein the coiling temperature is controlled to be M f -150℃~M f -30℃,M f is the martensitic transformation completion temperature of the thin strip, M f Determined according to the following formula: Mf(℃)=539-423*C-30.4*Mn-20*Si-12.1*Cr-110; 4) Tempering treatment: The martensitic hot coil obtained in step 3) is placed in an intermediate warehouse, wherein the storage temperature of the martensitic hot coil is not more than 20°C lower than the coiling temperature, and the steel coil is left to stand for more than 2 days and slowly cooled to room temperature, wherein the slow cooling rate is lower than 4°C / h, so that in this process, the residual heat of the steel coil is used to perform long-term online tempering of the martensitic structure to obtain a martensitic finished coil, wherein the microstructure of the martensitic steel in the martensitic finished coil is mainly lath-shaped tempered martensite, and the rest is a small amount of residual austenite and lower bainite, wherein the lath-shaped tempered martensite contains dispersed fine rod-shaped ε carbides between the structures.

2. A method for producing martensitic steel based on a twin-roll casting process, characterized in that: The method comprises the following steps: 1) Thin strip continuous casting: A twin-roll casting process is used to continuously cast a thin strip to obtain a cast strip, and the cast strip is subjected to a hot rolling process to obtain a rolled strip with a thickness of 0.8 to 1.8 mm; 2) Aerosol cooling: The strip obtained in step 1) is subjected to mist cooling to obtain a martensitic thin strip, wherein the cooling rate of the mist cooling is 60 to 180° C. / s, and after the mist cooling, high-pressure gas is sprayed on the plate surface of the strip to dry the cooling water, thereby eliminating water marks or water stains on the strip surface at the cooling outlet; 3) Temperature controlled coiling: The martensitic thin strip obtained in step 2) is temperature-controlled coiled to obtain a martensitic hot coil, wherein the coiling temperature is controlled to be M f -150℃~M f -30℃,M f is the martensitic transformation completion temperature of the thin strip, M f Determined according to the following formula: Mf(℃)=539-423*C-30.4*Mn-20*Si-12.1*Cr-110; 4) Tempering treatment: The martensitic hot coil obtained in step 3) is placed in a fully enclosed insulation pit for more than 2 days to be slowly cooled to room temperature, wherein the pit entry temperature is no lower than the coiling temperature by no more than 20°C, wherein the slow cooling rate is less than 2.5°C / h, so as to obtain a martensitic finished coil. The martensitic hot coil is rolled, and the microstructure of the martensitic steel in the martensitic finished coil is mainly lath-shaped tempered martensite, and the rest is a small amount of residual austenite and lower bainite, wherein the lath-shaped tempered martensite contains dispersed fine rod-shaped ε carbides between its tissues.

3. A method for producing martensitic steel based on a twin-roll casting process, characterized in that: The method comprises the following steps: 1) Thin strip continuous casting: A twin-roll casting process is used to continuously cast a thin strip to obtain a cast strip, and the cast strip is subjected to a hot rolling process to obtain a rolled strip with a thickness of 0.8 to 1.8 mm; 2) Aerosol cooling: The strip obtained in step 1) is subjected to mist cooling to obtain a martensitic thin strip, wherein the cooling rate of the mist cooling is 60 to 180° C. / s, and after the mist cooling, high-pressure gas is sprayed on the plate surface of the strip to dry the cooling water, thereby eliminating water marks or water stains on the strip surface at the cooling outlet; 3) Temperature controlled coiling: The martensitic thin strip obtained in step 2) is temperature-controlled coiled to obtain a martensitic hot coil, wherein the coiling temperature is controlled to be M f -150℃~M f -30℃,M f is the martensitic transformation completion temperature of the thin strip, M f Determined according to the following formula: Mf(℃)=539-423*C-30.4*Mn-20*Si-12.1*Cr-110; 4) Tempering treatment: The martensitic hot coil obtained in step 3) is placed in a heatable heat-insulating hood for 1 to 2 days, wherein the temperature entering the hood drops by no more than 20°C compared with the coiling temperature, wherein the temperature fluctuation in the hood does not exceed 20°C, and air-cooled to room temperature after exiting the hood to obtain a martensitic finished coil. The martensitic hot coil is rolled, and the microstructure of the martensitic steel in the martensitic finished coil is mainly lath-shaped tempered martensite, and the rest is a small amount of residual austenite and lower bainite, wherein the lath-shaped tempered martensite contains dispersed fine rod-shaped ε carbides between its tissues.

4. A martensitic steel, characterized in that: The martensitic steel is produced using the method according to any one of claims 1 to 3.

5. The martensitic steel according to claim 4, characterized in that: The martensitic steel strip obtained after online tempering in the hot coil intermediate warehouse or online tempering in the fully enclosed insulation pit is subjected to a 90° bending test. When the bending radius is ≥ 2a, the bending part will not crack, where a is the thickness of the steel plate.

6. The martensitic steel according to claim 4, characterized in that: The martensitic steel strip obtained after low-temperature tempering in a hood is subjected to a 90° bending test. When the bending radius is ≥1.5a, the bending portion will not crack, where a is the thickness of the steel plate.