A backing plate for drilling a printed circuit board and a preparation method thereof
By applying lubricating heat dissipation resin to the upper and lower surfaces of the metal core layer and setting the surface layer during the drilling process of PCB board, the problem of the existing pad cannot be lubricated and heat dissipated is solved, the hole position accuracy and hole wall quality are improved, and the hole wall quality is reduced. It has a production cost and is suitable for industrial production.
Patent Information
- Application Number
- CN202311613511.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-29
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-11-29
AI Technical Summary
The existing PCB board drilling special pads or aluminum-based cover plates cannot effectively lubricate and dissipate heat during the drilling process, resulting in broken drill needles, rough hole walls, high production costs and low hole position accuracy, which cannot meet quality requirements.
The metal core layer is coated with lubricating heat dissipation resin to form a lubricating heat dissipation resin layer, and a surface layer is installed on its surface to increase the lubricating heat dissipation function of the pad, reduce internal stress, improve the hole position accuracy and hole wall quality, and reduce drilling Needle temperature.
Effectively reduce the internal stress of the pad during use, improve the hole position accuracy and hole wall quality, reduce the drilling needle temperature, avoid the problems of hole wall roughness and redness of the metal core layer, and reduce production costs. Suitable for industrial production.
Smart Images

Figure CN117528938B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of PCB processing and preparation, and in particular to a pad for drilling a printed circuit board and a preparation method thereof. Background Art
[0002] In the production of printed circuit boards (PCBs), holes need to be arranged on the substrate to match the predetermined circuit design. In the process of arranging holes, in order to prevent damage to the processing table and uneven force on the circuit board, a pad is often used as a buffer protection device at the bottom of the base. As an important auxiliary material in the field of PCB manufacturing drilling, the pad plays a very important role in ensuring the quality of the tinning and copper plating process of the circuit board, protecting the drilling machine table, improving the hole position accuracy, suppressing the outlet flash, and playing the role of heat dissipation, guiding and protecting the drill needle, as well as improving the quality of the hole wall.
[0003] The existing PCB drilling pads or aluminum-based cover plates do not provide good lubrication and heat dissipation, which not only makes it easy for the drill bit to break when drilling, but also damages the drilling equipment, increasing production costs; and the PCB hole wall after drilling is not smooth enough and is rough, which indirectly increases the resistance of the PCB and cannot meet the quality requirements of production. Summary of the invention
[0004] In order to overcome the shortcomings and deficiencies in the prior art, the purpose of the present invention is to provide a pad for drilling printed circuit boards, which pad is formed by coating the upper and lower surfaces of a metal core material layer with a lubricating heat dissipation resin to form a lubricating heat dissipation resin layer and arranging surface materials on the surface of the lubricating heat dissipation resin layer. When used for drilling holes in printed circuit boards, the pad can minimize the internal stress generated during use of the pad, has good flatness and surface hardness, can reduce the burr at the outlet of the PCB board, low hole position accuracy and other problems; and because the lubricating heat dissipation resin is added to the pad, the pad has good lubrication and heat dissipation functions, thereby increasing the hole position accuracy of the drill when drilling, improving the hole wall quality and reducing the drill temperature, and avoiding the hole wall roughness caused by the existing pad.
[0005] Another object of the present invention is to provide a method for preparing a pad for drilling holes in a printed circuit board. The preparation method is simple, easy to operate and control, produces products of high quality and low cost, is conducive to industrial production, and can effectively overcome the disadvantages of previous PCB board drilling pads or aluminum-based cover plates that have no lubrication and heat dissipation effects.
[0006] The purpose of the present invention is achieved through the following technical scheme: a pad for drilling a printed circuit board, comprising an upper material layer, an upper lubricating heat dissipation resin layer arranged on the lower surface of the upper material layer, a metal core material layer arranged on the lower surface of the upper lubricating heat dissipation resin layer, a lower lubricating heat dissipation resin layer arranged on the lower surface of the metal core material layer, and a lower material layer arranged on the lower surface of the lower lubricating heat dissipation resin layer; wherein the upper lubricating heat dissipation resin layer and the lower lubricating heat dissipation resin layer are formed by coating with lubricating heat dissipation resin.
[0007] The pad in the present invention is formed by coating the upper and lower surfaces of the metal core layer with lubricating heat dissipation resin to form a lubricating heat dissipation resin layer and arranging surface materials on the surface of the lubricating heat dissipation resin layer. When used for drilling holes in a printed circuit board, the pad can minimize the internal stress generated during use of the pad, has good flatness and surface hardness, can reduce the problems of PCB board outlet burr, low hole position accuracy, etc.; and because the lubricating heat dissipation resin is added to the pad, the pad has good lubrication and heat dissipation functions, thereby increasing the hole position accuracy of the drill when drilling, improving the hole wall quality and reducing the drill temperature, avoiding the hole wall roughness caused by the existing pad and the redness of the metal core layer, and has good industrial production value and application prospects.
[0008] Preferably, the metal core material layer is made of a metal material having a foam structure or a honeycomb structure, and the metal material is one of aluminum, copper, iron, and nickel.
[0009] Preferably, the upper material layer and the lower material layer are composed of metal sheets or impregnated and cured sheets or adhesive layers.
[0010] Preferably, the impregnated solidified sheet is a sheet-like resin material formed by impregnating paper or glass fiber cloth with thermosetting resin; the thermosetting resin is urea-formaldehyde resin.
[0011] Preferably, the adhesive is an epoxy resin adhesive, which includes 30-40 parts of epoxy resin, 1-3 parts of modified filler, 1-5 parts of graphene chloride, 20-40 parts of acetone, and 10-20 parts of acrylic resin.
[0012] The above adhesive in the present invention has greatly improved thermal conductivity without affecting the mechanical properties and tribological properties of the resin, which can reduce the continuous high temperature and failure of mechanical devices using the adhesive. The adhesive uses epoxy resin and acrylic resin as a water-based system, so that the stability of the entire surface material layer is good. At the same time, epoxy resin and acrylic resin are both low-melting-point polymer materials, which will completely melt into liquid when drilling, giving the drill bit good lubricity and heat dissipation and cooling performance; and adding modified fillers to the adhesive helps to improve the strength, toughness and wear resistance of the resin.
[0013] Preferably, the modified filler is at least one of calcium carbonate, carbon black, calcium sulfate, carbon fiber, silicon dioxide, graphene, carbon nanotubes, boron nitride, zirconium oxide, and modified titanium dioxide. More preferably, the modified filler is composed of calcium carbonate, graphene, and modified titanium dioxide in a weight ratio of 0.4-0.8:0.6-1.0:0.8-1.2.
[0014] Preferably, the modified titanium dioxide is prepared by the following method: polyacrylic acid, propylene glycol and titanium dioxide in a mass ratio of 1:0.8-1.2:40-60 are mixed, heated to 50-60°C for reaction for 60-90 minutes, then heated to 65°C, 0.8-1.6% of the mass of titanium dioxide silane coupling agent KH560 is added, the reaction time is 1-2 hours, filtered and washed with ethanol to obtain modified titanium dioxide.
[0015] The modified titanium dioxide in the present invention can provide the adhesive with a suitable viscosity conducive to low-temperature curing through an adjustment effect, thereby giving the drill bit good lubricity and heat dissipation and cooling performance.
[0016] Preferably, the lubricating heat dissipating resin comprises the following raw materials in parts by weight: 10-20 parts of polyethylene oxide, 5-10 parts of polyvinyl alcohol, 10-20 parts of binder, 3-7 parts of thixotropic agent, 5-10 parts of lubricant, 1-3 parts of defoaming agent, 4-8 parts of heat absorbent, 30-60 parts of solvent and 1-5 parts of surfactant.
[0017] The lubricating heat dissipation resin using the above raw materials in the present invention has a good lubricating and heat dissipation effect. The polyethylene oxide and the adhesive grease used therein are both water-based systems, so that the entire drilling lubricant has good compatibility and stability, and can be stored for a long time at room temperature; at the same time, it has a low melting point and will completely melt into liquid when drilling, giving the drill bit good lubricity and heat dissipation and cooling performance, so that the pad has good lubrication and heat dissipation functions, thereby increasing the hole position when the drill needle is drilled, and can also improve the hole wall quality and reduce the temperature of the drill needle, avoiding the hole wall roughness caused by the existing pad and the redness of the metal core layer, and has good industrial production value and application prospects.
[0018] Preferably, the binder is at least one of epoxy resin, modified polymer resin, acrylic resin and polyurethane resin.
[0019] Preferably, the thixotropic agent is at least one of fumed silica, polyamide wax, nitrile rubber, styrene-butadiene rubber, and ethyl cellulose.
[0020] The thixotropic agent used in the present invention mainly increases the viscosity of the lubricating heat dissipating resin coating and changes the rheological properties of the lubricating heat dissipating resin layer, so that the lubricating heat dissipating resin layer can produce tunnel patterns on the metal core material layer, making it less likely for glue to flow during the heating and drying process, thereby avoiding the problem of rough hole walls of the existing pads.
[0021] Preferably, the lubricant is at least one of polyamide wax, polyethylene wax and talcum powder, which improves the lubrication effect of the drilling process.
[0022] Preferably, the defoaming agent is at least one of defoaming agent AFE-3168 and defoaming agent AFE-1410.
[0023] Preferably, the heat absorbent is at least one of lithium tetrafluoroborate, sodium tetrafluoroborate and potassium hexafluoroaluminate; and the surfactant is an organosilicon surfactant.
[0024] In the present invention, a heat absorbent is added to the lubricating heat dissipation resin, and the heat absorbent will melt into liquid during the drilling process to absorb the heat generated during drilling, thereby preventing the workpiece from being damaged by excessive heat. The heat absorbent will also take away the grinding debris generated by drilling when it falls off, thereby improving the hole position accuracy, suppressing the outlet flash, and playing a very important role in heat dissipation and improving the hole wall quality.
[0025] Preferably, the solvent is a mixture of deionized water, butanone and isophorone in a weight ratio of 10-16:0.8-1.2:1-2.
[0026] The present invention also provides a method for preparing a backing plate for drilling a printed circuit board, comprising the following steps:
[0027] S1, coating the upper and lower surfaces of the metal core material layer with a lubricating heat dissipation resin to form an upper lubricating heat dissipation resin layer and a lower lubricating heat dissipation resin layer for standby use;
[0028] S2. When the lubricating heat dissipation resin coated on the upper surface of the metal core material layer is not completely dry, the surface of the lubricating heat dissipation resin layer is bonded to the upper material layer upward, and the surface of the lubricating heat dissipation resin layer is bonded to the lower material layer downward to obtain a pad for drilling a printed circuit board.
[0029] The beneficial effects of the present invention are as follows: the pad for drilling holes in a printed circuit board of the present invention adopts a metal core material layer, the upper and lower surfaces of which are coated with lubricating heat dissipation resin to form a lubricating heat dissipation resin layer, and surface materials are respectively arranged on the surface of the lubricating heat dissipation resin layer. When used for drilling holes in a printed circuit board, the internal stress generated by the pad during use can be reduced to the greatest extent, and the pad has good flatness and surface hardness, and can reduce the problems of PCB board outlet burr, low hole position accuracy, etc.; and because the lubricating heat dissipation resin is added to the pad, the pad has good lubrication and heat dissipation functions, thereby increasing the hole position accuracy of the drill when drilling, improving the hole wall quality and reducing the drill temperature, and avoiding the hole wall roughness caused by the existing pad.
[0030] The preparation method of the pad for drilling a printed circuit board of the present invention is simple, the operation and control are convenient, the product quality is high, the cost is low, and it is conducive to industrial production. At the same time, it can effectively overcome the disadvantages that the previous pads or aluminum-based cover plates for drilling PCB boards cannot play the role of lubrication and heat dissipation. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 It is a schematic diagram of the cross-sectional structure of the present invention.
[0032] The reference numerals are: 1 - upper material layer, 2 - upper lubricating heat dissipating resin layer, 3 - metal core material layer, 4 - lower lubricating heat dissipating resin layer and 5 - lower material layer. DETAILED DESCRIPTION
[0033] In order to facilitate the understanding of those skilled in the art, the following embodiments and attached Figure 1 The present invention is further described, and the contents mentioned in the implementation modes are not intended to limit the present invention.
[0034] Example 1
[0035] A pad for drilling a printed circuit board comprises an upper material layer 1, an upper lubricating heat dissipation resin layer 2 arranged on the lower surface of the upper material layer 1, a metal core material layer 3 arranged on the lower surface of the upper lubricating heat dissipation resin layer 2, a lower lubricating heat dissipation resin layer 4 arranged on the lower surface of the metal core material layer 3, and a lower material layer 5 arranged on the lower surface of the lower lubricating heat dissipation resin layer 4; wherein the upper lubricating heat dissipation resin layer 2 and the lower lubricating heat dissipation resin layer 4 are formed by coating with lubricating heat dissipation resin.
[0036] The metal core material layer 3 is made of a metal material having a foam structure or a honeycomb structure, and the metal material is aluminum.
[0037] The upper surface material layer 1 and the lower surface material layer 5 are composed of adhesive layers.
[0038] The adhesive is an epoxy resin adhesive, which includes 30 parts of epoxy resin, 1 part of modified filler, 1 part of graphene chloride, 20 parts of acetone, and 10 parts of acrylic resin; the acrylic resin is 518 acrylic resin provided by Chenyou Paint (Shandong) Co., Ltd.
[0039] The modified filler is composed of calcium carbonate, graphene and modified titanium dioxide in a weight ratio of 0.4:0.6:0.8.
[0040] The modified titanium dioxide is prepared by the following method: polyacrylic acid, propylene glycol and titanium dioxide in a mass ratio of 1:0.8:40 are mixed, heated to 50° C. for reaction for 90 minutes, then heated to 65° C., 0.8% of the mass of the titanium dioxide silane coupling agent KH560 is added, the reaction time is 2 hours, filtered and washed with ethanol to obtain the modified titanium dioxide.
[0041] The lubricating heat dissipation resin includes the following raw materials in parts by weight: 10 parts of polyethylene oxide, 5 parts of polyvinyl alcohol, 10 parts of binder, 3 parts of thixotropic agent, 5 parts of lubricant, 1 part of defoaming agent, 4 parts of heat absorbent, 30 parts of solvent and 1 part of surfactant; the polyethylene oxide adopts the model POLYOX WSR 308 polyethylene oxide provided by DOW Chemical of the United States.
[0042] The binder is epoxy resin. The thixotropic agent is fumed silica.
[0043] The lubricant is polyamide wax. The defoamer is defoamer AFE-3168.
[0044] The heat absorbent is lithium tetrafluoroborate; and the surfactant is BYK306 leveling agent.
[0045] The solvent is a mixture of deionized water, butanone and isophorone in a weight ratio of 10:0.8:1.
[0046] The printed circuit board drilling pad is prepared by the following steps:
[0047] S1, applying lubricating heat dissipation resin on the upper and lower surfaces of the metal core material layer 3 to form an upper lubricating heat dissipation resin layer 2 and a lower lubricating heat dissipation resin layer 4, for standby use;
[0048] S2. When the lubricating heat dissipation resin coated on the upper surface of the metal core material layer 3 is not completely dry, the surface of the lubricating heat dissipation resin layer 2 is bonded to the upper material layer 1, and the surface of the lubricating heat dissipation resin layer 4 is bonded to the lower material layer 5 to obtain a pad for drilling holes in a printed circuit board.
[0049] Example 2
[0050] A pad for drilling a printed circuit board comprises an upper material layer 1, an upper lubricating heat dissipation resin layer 2 arranged on the lower surface of the upper material layer 1, a metal core material layer 3 arranged on the lower surface of the upper lubricating heat dissipation resin layer 2, a lower lubricating heat dissipation resin layer 4 arranged on the lower surface of the metal core material layer 3, and a lower material layer 5 arranged on the lower surface of the lower lubricating heat dissipation resin layer 4; wherein the upper lubricating heat dissipation resin layer 2 and the lower lubricating heat dissipation resin layer 4 are formed by coating with lubricating heat dissipation resin.
[0051] The metal core material layer 3 is made of a metal material having a foam structure or a honeycomb structure, and the metal material is copper.
[0052] The upper surface material layer 1 and the lower surface material layer 5 are composed of adhesive layers.
[0053] The adhesive is an epoxy resin adhesive, which includes 35 parts of epoxy resin, 2 parts of modified filler, 3 parts of graphene chloride, 30 parts of acetone, and 15 parts of acrylic resin; the acrylic resin is 518 acrylic resin provided by Chenyou Paint (Shandong) Co., Ltd.
[0054] The modified filler is composed of calcium carbonate, graphene and modified titanium dioxide in a weight ratio of 0.6:0.8:1.0.
[0055] The modified titanium dioxide is prepared by the following method: polyacrylic acid, propylene glycol and titanium dioxide in a mass ratio of 1:1.0:50 are mixed, heated to 55°C for reaction for 80 minutes, then heated to 65°C, 1.2% of the mass of the titanium dioxide silane coupling agent KH560 is added, the reaction time is 1.5 hours, filtered and washed with ethanol to obtain the modified titanium dioxide.
[0056] The lubricating heat dissipation resin comprises the following raw materials in parts by weight: 15 parts of polyethylene oxide, 8 parts of polyvinyl alcohol, 15 parts of binder, 5 parts of thixotropic agent, 8 parts of lubricant, 2 parts of defoaming agent, 6 parts of heat absorbent, 45 parts of solvent and 3 parts of surfactant; the polyethylene oxide adopts the model POLYOX WSR 308 polyethylene oxide provided by DOW Chemical of the United States.
[0057] The adhesive is composed of epoxy resin, acrylic resin and polyurethane resin in a weight ratio of 1:1.0:0.8.
[0058] The thixotropic agent is composed of fumed silica, polyamide wax and styrene-butadiene rubber in a weight ratio of 0.8:1.0:0.4.
[0059] The lubricant is composed of polyamide wax, polyethylene wax and talcum powder in a weight ratio of 1.0:0.8:0.4.
[0060] The defoamer is defoamer AFE-1410.
[0061] The heat absorbent is composed of lithium tetrafluoroborate, sodium tetrafluoroborate and potassium hexafluoroaluminate in a weight ratio of 0.8:0.4:1.0; and the surfactant is BYK306 leveling agent.
[0062] The solvent is a mixture of deionized water, butanone and isophorone in a weight ratio of 13:1.0:1.5.
[0063] The printed circuit board drilling pad is prepared by the following steps:
[0064] S1, applying lubricating heat dissipation resin on the upper and lower surfaces of the metal core material layer 3 to form an upper lubricating heat dissipation resin layer 2 and a lower lubricating heat dissipation resin layer 4, for standby use;
[0065] S2. When the lubricating heat dissipation resin coated on the upper surface of the metal core material layer 3 is not completely dry, the surface of the lubricating heat dissipation resin layer 2 is bonded to the upper material layer 1, and the surface of the lubricating heat dissipation resin layer 4 is bonded to the lower material layer 5 to obtain a pad for drilling holes in a printed circuit board.
[0066] Example 3
[0067] A pad for drilling a printed circuit board comprises an upper material layer 1, an upper lubricating heat dissipation resin layer 2 arranged on the lower surface of the upper material layer 1, a metal core material layer 3 arranged on the lower surface of the upper lubricating heat dissipation resin layer 2, a lower lubricating heat dissipation resin layer 4 arranged on the lower surface of the metal core material layer 3, and a lower material layer 5 arranged on the lower surface of the lower lubricating heat dissipation resin layer 4; wherein the upper lubricating heat dissipation resin layer 2 and the lower lubricating heat dissipation resin layer 4 are formed by coating with lubricating heat dissipation resin.
[0068] The metal core material layer 3 is made of a metal material having a foam structure or a honeycomb structure, and the metal material is iron.
[0069] The upper surface material layer 1 and the lower surface material layer 5 are composed of adhesive layers.
[0070] The adhesive is an epoxy resin adhesive, which includes 40 parts of epoxy resin, 3 parts of modified filler, 5 parts of graphene chloride, 40 parts of acetone, and 20 parts of acrylic resin; the acrylic resin is 518 acrylic resin provided by Chenyou Paint (Shandong) Co., Ltd.
[0071] The modified filler is composed of calcium carbonate, graphene and modified titanium dioxide in a weight ratio of 0.8:1.0:1.2.
[0072] The modified titanium dioxide is prepared by the following method: polyacrylic acid, propylene glycol and titanium dioxide in a mass ratio of 1:1.2:60 are mixed, heated to 60°C for reaction for 60 minutes, then heated to 65°C, 1.6% of the mass of the titanium dioxide silane coupling agent KH560 is added, the reaction time is 1 hour, and the modified titanium dioxide is obtained by suction filtration and washing with ethanol.
[0073] The lubricating heat dissipation resin comprises the following raw materials in parts by weight: 20 parts of polyethylene oxide, 10 parts of polyvinyl alcohol, 20 parts of binder, 7 parts of thixotropic agent, 10 parts of lubricant, 3 parts of defoaming agent, 8 parts of heat absorbent, 60 parts of solvent and 5 parts of surfactant; the polyethylene oxide adopts the model POLYOX WSR 308 polyethylene oxide provided by DOW Chemical of the United States.
[0074] The binder is acrylic resin. The thixotropic agent is styrene-butadiene rubber.
[0075] The lubricant is talcum powder. The defoamer is defoamer AFE-3168.
[0076] The heat absorbent is potassium hexafluoroaluminate; and the surfactant is BYK306 leveling agent.
[0077] The solvent is a mixture of deionized water, butanone and isophorone in a weight ratio of 16:1.2:2.
[0078] The printed circuit board drilling pad is prepared by the following steps:
[0079] S1, applying lubricating heat dissipation resin on the upper and lower surfaces of the metal core material layer 3 to form an upper lubricating heat dissipation resin layer 2 and a lower lubricating heat dissipation resin layer 4, for standby use;
[0080] S2. When the lubricating heat dissipation resin coated on the upper surface of the metal core material layer 3 is not completely dry, the surface of the lubricating heat dissipation resin layer 2 is bonded to the upper material layer 1, and the surface of the lubricating heat dissipation resin layer 4 is bonded to the lower material layer 5 to obtain a pad for drilling holes in a printed circuit board.
[0081] Comparative Example 1
[0082] The difference between this comparative example and the above-mentioned embodiment 2 is that no thixotropic agent and heat-absorbing agent are added to the raw materials of the lubricating heat-dissipating resin in this comparative example. The rest of the contents of this comparative example are the same as those in embodiment 2 and will not be repeated here.
[0083] Comparative Example 2
[0084] The difference between this comparative example and the above-mentioned Example 2 is that no modified filler is added to the raw materials of the adhesive in this comparative example. The rest of the contents of this comparative example are the same as those of Example 2 and will not be repeated here.
[0085] The lubricating and heat dissipating resins obtained in Example 2 and Comparative Example 1 were subjected to performance tests, and the test results are shown in the following table:
[0086] Friction coefficient: According to SHT 0190-1992 Liquid Lubricant Friction Coefficient Determination Method (MM-200 Method), under the maximum load capacity of the testing machine (10kN), the test time reaches 150s.
[0087] Table 1
[0088] project Example 2 Comparative Example 1 Friction coefficient 0.07 0.27 Thermal conductivity (W / (m·K)) 2.358 0.642
[0089] From the comparison between Example 2 and Comparative Example 1, it can be seen that the lubricating and heat-dissipating resin using a thixotropic agent and a heat-absorbing agent has good lubrication and heat-dissipating effects, and has broad market prospects and application value.
[0090] The adhesives prepared in Example 2 and Comparative Example 2 were subjected to performance tests, and the test results are shown in the following 2 tables:
[0091] Friction coefficient: According to SHT 0190-1992 Liquid Lubricant Friction Coefficient Determination Method (MM-200 Method), under the maximum load capacity of the testing machine (10kN), the test time reaches 150s.
[0092] Table 2
[0093] project Example 2 Comparative Example 2 Friction coefficient 0.18 0.27 Tensile strength(MPa) 5.9 3.5 Shore 76 62
[0094] From the comparison between Example 2 and Comparative Example 2, it can be seen that the adhesive using the modified filler has good tensile strength and hardness, and has broad market prospects and application value.
[0095] The above embodiments are preferred implementation schemes of the present invention. In addition, the present invention may also be implemented in other ways. Any obvious replacement without departing from the concept of the present invention is within the protection scope of the present invention.
Claims
1. A pad for drilling a printed circuit board, characterized in that: The invention comprises an upper material layer, an upper lubricating heat dissipating resin layer arranged on the lower surface of the upper material layer, a metal core material layer arranged on the lower surface of the upper lubricating heat dissipating resin layer, a lower lubricating heat dissipating resin layer arranged on the lower surface of the metal core material layer, and a lower material layer arranged on the lower surface of the lower lubricating heat dissipating resin layer; wherein the upper lubricating heat dissipating resin layer and the lower lubricating heat dissipating resin layer are coated with lubricating heat dissipating resin; The upper material layer and the lower material layer are composed of adhesive layers; The adhesive is an epoxy resin adhesive, which includes 30-40 parts of epoxy resin, 1-3 parts of modified filler, 1-5 parts of chlorinated graphene, 20-40 parts of acetone, and 10-20 parts of acrylic resin; The modified filler is composed of calcium carbonate, graphene and modified titanium dioxide in a weight ratio of 0.4-0.8:0.6-1.0:0.8-1.2; The modified titanium dioxide is prepared by the following method: polyacrylic acid, propylene glycol and titanium dioxide in a mass ratio of 1:0.8-1.2:40-60 are mixed, heated to 50-60° C. for reaction for 60-90 minutes, then heated to 65° C., 0.8-1.6% of the mass of the titanium dioxide silane coupling agent KH560 is added, the reaction time is 1-2 hours, and the modified titanium dioxide is obtained by suction filtration and washing with ethanol; The lubricating heat dissipating resin comprises the following raw materials in parts by weight: 10-20 parts of polyethylene oxide, 5-10 parts of polyvinyl alcohol, 10-20 parts of a binder, 3-7 parts of a thixotropic agent, 5-10 parts of a lubricant, 1-3 parts of a defoaming agent, 4-8 parts of a heat absorbent, 30-60 parts of a solvent and 1-5 parts of a surfactant; The thixotropic agent is at least one of fumed silica, polyamide wax, nitrile rubber, styrene-butadiene rubber, and ethyl cellulose; The heat absorbent is at least one of lithium tetrafluoroborate, sodium tetrafluoroborate and potassium hexafluoroaluminate.
2. A printed circuit board drilling pad according to claim 1, characterized in that: The metal core material layer is made of a metal material having a foam structure or a honeycomb structure, and the metal material is one of aluminum, copper, iron, and nickel.
3. A printed circuit board drilling pad according to claim 1, characterized in that: The binder is at least one of epoxy resin, modified polymer resin, acrylic resin and polyurethane resin.
4. A printed circuit board drilling pad according to claim 1, characterized in that: The lubricant is at least one of polyamide wax, polyethylene wax and talcum powder.
5. A printed circuit board drilling pad according to claim 1, characterized in that: The defoaming agent is at least one of defoaming agent AFE-3168 and defoaming agent AFE-1410.
6. A method for preparing a backing plate for drilling a printed circuit board according to any one of claims 1 to 5, characterized in that: The steps include: S1, coating the upper and lower surfaces of the metal core material layer with a lubricating heat dissipation resin to form an upper lubricating heat dissipation resin layer and a lower lubricating heat dissipation resin layer for standby use; S2. When the lubricating heat dissipation resin coated on the upper surface of the metal core material layer is not completely dry, the surface of the lubricating heat dissipation resin layer is bonded to the upper material layer upward, and the surface of the lubricating heat dissipation resin layer is bonded to the lower material layer downward to obtain a pad for drilling a printed circuit board.