A method for producing metallurgical coke by blending low-rank bituminous coal, blended coal and its products
By using non-stick coal in low-order bituminous coal in coking process to replace weakly bonded coal and adjust the ratio of coal types, the shortage of high-quality coking coal resources and coke quality stability are solved, and the cost of coal distribution and the cost of low-order Effects of bituminous coal utilization efficiency.
Patent Information
- Application Number
- CN202311551693.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-20
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2043-11-20
AI Technical Summary
The existing coking process is seriously dependent on high-quality coking coal resources, and the low-order bituminous coal resources are insufficiently utilized, which makes it difficult to guarantee the quality of coke and production stability.
Use non-stick coal in low-grade bituminous coal to replace weakly bonded coal, and use specific coal ratios (non-stick coal: 1 to 5 parts, weakly sticky coal: 2 to 6 parts, gas coal: 15 to 25 parts, 1 /3 Coking coal: 5 to 25 parts, coking coal: 40 to 70 parts, lean coal: 5 to 10 parts), so as to reduce the cost of coal distribution and ensure the quality of coke.
It effectively reduces the cost of coal mixing, broadens the resource utilization pathways for coking coal, and meets the coke performance requirements of secondary metallurgical cokes in the national standards without affecting the quality of coke.
Smart Images

Figure CN117603717B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of coking coal blending in the coking industry, and specifically relates to a method for producing metallurgical coke by blending low-rank bituminous coal, blended coal and products thereof. Background Art
[0002] Research and production practice have shown that the quality of coke directly affects the blast furnace condition, blast furnace coal injection amount and blast furnace smooth operation. However, the existing coking process is heavily dependent on raw coal, and high-quality coking coal resources are becoming increasingly scarce. The quality of coal entering the factory is complex and the overall coal quality has seriously declined, and stability is difficult to guarantee. Therefore, all coking plants are committed to the research of coal blending solutions, and under the premise of ensuring coke quality and stabilizing blast furnace production, low-rank bituminous coal is applied to coal blending coking. This not only expands the source of coking coal, but also provides a high-quality utilization method for low-rank bituminous coal. Summary of the invention
[0003] Based on the above problems, the present invention provides a method for producing metallurgical coke by blending low-rank bituminous coal, blended coal and its products. The present invention uses non-caking coal in low-rank bituminous coal to partially replace weakly caking coal, which ensures the quality of coke and reduces the cost of coal blending.
[0004] In a first aspect of the present invention, there is provided a method for producing metallurgical coke by blending low-rank bituminous coal, which comprises using the following blended coals in proportion by mass:
[0005] Non-sticky coal: 1-5 parts, weakly sticky coal: 2-6 parts, gas coal: 15-25 parts, 1 / 3 coking coal: 5-25 parts, coking coal: 40-70 parts, lean coal: 5-10 parts.
[0006] In a specific embodiment, the method comprises using the following blended coal in proportion by mass:
[0007] Non-sticky coal: 1-4 parts, weakly sticky coal: 2-6 parts, gas coal: 18-22 parts, 1 / 3 coking coal: 15-20 parts, coking coal: 45-50 parts, lean coal: 5-10 parts.
[0008] In a specific embodiment, the non-sticky coal V daf The range is 33% to 37%, with an average value of about 35.8%; the range of ash yield is 4% to 7%, with an average value of about 5%; the total sulfur content is 0.1% to 0.5%, with an average value of 0.21%. In one embodiment, the non-caking coal is selected from the Ordos Baopingwan Coal Mine in Inner Mongolia, preferably low-ash and extra-low-sulfur non-caking coal.
[0009] In a specific embodiment, the weakly caking coal V dafThe range is between 31% and 34%, with an average value of about 32.5%; the ash yield range is between 5.5% and 6.8%, with an average value of about 6.3%; the total sulfur content ranges from 0.35% to 0.58%, with an average value of 0.42%; the bonding index G value ranges from 10 to 15, with an average value of about 11.8.
[0010] In a specific embodiment, the V of the gas coal daf The range is between 37% and 42%, with an average value of about 37.3%; the ash yield range is between 8.1% and 11.2%, with an average value of about 9.8%; the total sulfur content ranges from 0.47% to 0.75%, with an average value of 0.56%; the adhesion index G value ranges from 61 to 85, with an average value of about 76.5; the maximum cuticle thickness Y ranges from 11.6 mm to 18.5 mm, with an average value of 15.7 mm.
[0011] In a specific embodiment, the 1 / 3 coking coal is low-ash coal, and its V daf The range is between 32% and 36%, with an average value of about 34.7%; the ash yield range is between 5.1% and 7.7%, with an average value of about 6.3%; the total sulfur content ranges from 0.36% to 0.65%, with an average value of 0.51%; the maximum cuticle thickness Y ranges from 6mm to 11.2mm, with an average value of 8.1mm.
[0012] In a specific embodiment, the coking coal is the skeleton coal in the coking blended coal, which accounts for more than 40% of the blended coal. daf The range is between 21% and 28%, with an average of 26.5%.
[0013] In a specific embodiment, different types of coking coals with different ash yield, total sulfur content, G value and Y value can be selected for use in combination to adjust the ash yield, total sulfur content and other index requirements of the blended coal. In one embodiment, Mengsan coking coal, Laoshidan 2.0 coking coal and Wuhushan 3.0 coking coal are selected for use in combination.
[0014] Among them, the total sulfur content of Mengsan coking coal is 0.60% to 0.75%, the ash yield ranges from 9.5% to 12.24%, with an average value of about 10.8%, the G value ranges from 75 to 85, with an average value of 79.3; the maximum cuticle thickness Y ranges from 15.1mm to 16.9mm, with an average value of 15.8mm;
[0015] The total sulfur content of Laoshidan 2.0 coking coal is 1.5% to 1.8%, the ash yield ranges from 9.5% to 12.24%, with an average value of 10.8%, the G value ranges from 82 to 100, with an average value of 94.3; the maximum cuticle thickness Y value ranges from 16.5mm to 25mm, with an average value of 21.5%;
[0016] The total sulfur content of Wuhushan 3.0 coking coal is 2.7% to 3.0%, the ash yield ranges from 5.83% to 7.72%, with an average value of 6.9%, the G value ranges from 82 to 100, with an average value of 94.3; the maximum cuticle thickness Y value ranges from 16.5mm to 25mm, with an average value of 21.5%;
[0017] In a specific embodiment, the V of the lean coal daf The range is between 16% and 21%, with an average value of about 18.2%; the ash yield range is between 9.1% and 10.9%, with an average value of about 10.2%; the total sulfur content ranges from 0.47% to 0.75%, with an average value of about 0.56%; the bonding index G value ranges from 37 to 65, with an average value of about 53.3.
[0018] The second aspect of the present invention provides a blended coal for producing metallurgical coke, wherein the blended coal raw material has a blending ratio of:
[0019] Non-sticky coal: 1-5 parts, weakly sticky coal: 2-6 parts, gas coal: 15-25 parts, 1 / 3 coking coal: 5-25 parts, coking coal: 40-70 parts, lean coal: 5-10 parts.
[0020] The preferred coal blending ratio and coal types for producing metallurgical coke are as defined in the first aspect of the present invention.
[0021] The third aspect of the present invention provides metallurgical coke produced from the above-mentioned blended coal.
[0022] In a specific embodiment, in the above-mentioned coal blending method and blended coal, the blended coal satisfies the following parameters: V daf In the range of 29% to 32%, ash content A d ≤10%, total sulfur content S t,d ≤0.8%, bonding index G≥70, maximum thickness of the colloid layer Y≥13mm.
[0023] In a specific embodiment, the above-mentioned coal blending method uses a 40kg test coke oven for coking to obtain coke that meets the following parameters: reactivity CRI ≤ 39.5%, post-reaction strength CSR ≥ 47.5%, ash content A d ≤14%, sulfur content S t,d ≤0.7%.
[0024] Beneficial Effects
[0025] The non-caking coal used in the present invention has a low price advantage compared to weakly caking coal, and can effectively reduce the coal blending cost. At the same time, it also broadens the coking coal resources and provides a new way for the efficient utilization of low-rank bituminous coal.
[0026] The present invention adds Baopingwan non-sticky coal to the basic blended coal without affecting the quality of coke, and the coke produced can at least meet the requirements of secondary metallurgical coke in national standards. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 It is a trend chart of the change in hot strength of coke produced by adding Baopingwan non-sticky coal in different proportions to the embodiments of the present invention and the comparative examples. DETAILED DESCRIPTION
[0028] To make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be clearly and completely described below. The described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present invention. In addition, in order to better illustrate the present invention, many specific details are given in the specific embodiments below. It should be understood by those skilled in the art that the present invention can also be implemented without certain specific details. In some embodiments, raw materials, components, methods, means, etc. known to those skilled in the art are not described in detail to highlight the purport of the present invention.
[0029] Unless otherwise specified, the coal varieties involved in the present invention are the coal varieties defined in the national standard GB / T5751-2009 "China Coal Classification".
[0030] Experimental coal
[0031] The specific test index data of the experimental coal used in the examples and comparative examples of the present invention are shown in Table 1.
[0032] Table 1 Test indexes of coal used in the experiment
[0033]
[0034]
[0035] Test standards and methods
[0036] Ash content of coal sample (A d ) and volatile matter (V daf ) is to complete the test and analysis according to the process specified in the national standard GB / T 212-2008 "Industrial Analysis Methods of Coal".
[0037] Total sulfur (S t,d ) and total sulfur of coke (S t,d ), the coulometric method specified in the national standard GB / T 214-2007 “Determination of total sulfur in coal” was used to complete the test analysis.
[0038] The adhesion index (G value) of the coal sample is tested and analyzed according to the method specified in the national standard GB / T 5447-2014 "Determination method of adhesion index of bituminous coal".
[0039] The Y value of the coal sample is determined using the national standard GB / T 479-2000 "Determination method for bituminous coal colloid index".
[0040] The thermal indicators of coke include coke reactivity (CRI) and post-reaction strength (CSR), which are completed according to the methods specified in the national standard GB / T4000-2017 "Test Method for Coke Reactivity and Post-Reaction Strength".
[0041] The coking process of the experimental 40kg coke oven is carried out in accordance with the national industry standard YB / T 4526-2016 "Technical Specifications for Small Coke Ovens for Coking Experiments".
[0042] Example 1 This example provides a method for producing metallurgical coke by blending low-rank bituminous coal. On the basis of the basic blended coal, Baopingwan non-caking coal is used to replace 2% of Datong weakly caking coal. The specific blended coal composition is shown in Table 2. The specific steps are as follows:
[0043] (1) Coal blending was performed according to the coal blending ratio of Example 1 in Table 2, the blended coal was crushed and mixed, and the proportion of coal particles smaller than 3 mm was not less than 89%, and blended coal was obtained, and quality testing was performed on the blended coal. The quality indicators are shown in Table 3;
[0044] (2) The performance of coke produced in a 40 kg test coke oven was tested. The moisture content of the coking coal was controlled at 12%. The coal sample was rammed and loaded into the oven at the bottom. The furnace temperature during loading was 800 °C and the final coking temperature was 1050 °C. The specific heating program is shown in Table 4.
[0045] (3) The quenching method after decoking is wet quenching. The quality of the obtained coke is tested, and the quality indicators are shown in Table 5 and Figure 1 .
[0046] Example 2 This example provides a method for producing metallurgical coke with low-rank bituminous coal. On the basis of the basic blended coal, 3% of Datong weakly caking coal is replaced with Baopingwan non-caking coal. The specific blended coal composition is shown in Table 2. The specific steps are as follows:
[0047] (1) Blending coal according to the coal blending ratio of Example 2 in Table 2, crushing and mixing the blended coal, and making sure that the proportion of coal particles smaller than 3 mm is not less than 89%, to obtain blended coal, and conducting quality inspection on the blended coal. The quality indicators are shown in Table 3;
[0048] (2) The performance of coke produced in a 40 kg test coke oven was tested. The moisture content of the coking coal was controlled at 12%. The coal sample was rammed and loaded into the oven at the bottom. The furnace temperature during loading was 800 °C and the final coking temperature was 1050 °C. The specific heating program is shown in Table 4.
[0049] (3) The quenching method after decoking is wet quenching. Then, the quality of the obtained coke is tested. The quality indicators are shown in Table 5 and Figure 1 .
[0050] Example 3 This example provides a method for producing metallurgical coke by blending low-rank bituminous coal. On the basis of the basic blended coal, 4% of Datong weakly caking coal is replaced by Baopingwan non-caking coal. The specific blended coal composition is shown in Table 2. The specific steps are as follows:
[0051] (1) Coal blending was performed according to the coal blending ratio of Example 3 in Table 2, the blended coal was crushed and mixed, and the proportion of coal particles smaller than 3 mm was not less than 89%, and blended coal was obtained, and quality testing was performed on the blended coal. The quality indicators are shown in Table 3;
[0052] (2) The performance of coke produced in a 40 kg test coke oven was tested. The moisture content of the coking coal was controlled at 12%. The coal sample was rammed and loaded into the oven at the bottom. The furnace temperature during loading was 800 °C and the final coking temperature was 1050 °C. The specific heating program is shown in Table 4.
[0053] (3) The quenching method after decoking is wet quenching. The quality of the obtained coke is tested, and the quality indicators are shown in Table 5 and Figure 1 .
[0054] Comparative Example 1 This comparative example provides a coal blending method for coking. On the basis of the basic blended coal, 6% of the Baopingwan non-sticky coal is used to replace all 6% of the Datong weakly sticky coal. The specific blended coal composition is shown in Table 2. The specific steps are as follows:
[0055] (1) Blending coal according to the coal blending ratio of Comparative Example 1 in Table 2, crushing and mixing the blended coal, and making sure that the proportion of coal particles smaller than 3 mm is not less than 89%, to obtain blended coal, and conducting quality inspection on the blended coal. The quality indicators are shown in Table 3;
[0056] (2) The performance of coke produced in a 40 kg test coke oven was tested. The moisture content of the coking coal was 12%. The coal sample was rammed and loaded into the oven at the bottom. The furnace temperature during loading was 800 °C and the final coking temperature was 1050 °C. The specific heating program is shown in Table 4.
[0057] (3) The quenching method after decoking is wet quenching. The quality of the obtained coke is tested, and the quality indicators are shown in Table 5 and Figure 1 .
[0058] Comparative Example 2 This comparative example provides a coal blending coking method. On the basis of the basic blended coal, 10% of Baopingwan non-sticky coal is used to replace 6% of Datong weakly sticky coal. The specific blended coal composition is shown in Table 2. The specific steps are as follows:
[0059] (1) Blending coal according to the coal blending ratio of Comparative Example 2 in Table 2, crushing and mixing the blended coal, and making sure that the proportion of coal particles smaller than 3 mm is not less than 89%, obtaining blended coal, and conducting quality inspection on the blended coal. The quality indicators are shown in Table 3;
[0060] (2) The performance of coke produced in a 40 kg test coke oven was tested. The moisture content of the coking coal was 12%. The coal sample was rammed and loaded into the oven at the bottom. The furnace temperature during loading was 800 °C and the final coking temperature was 1050 °C. The specific heating program is shown in Table 4.
[0061] (3) The quenching method after decoking is wet quenching. The quality of the obtained coke is tested, and the quality indicators are shown in Table 5 and Figure 1 .
[0062] Table 2 Proportion of coal blended in each embodiment and comparative example (%)
[0063]
[0064] Table 3 Test indexes of coal blends in the embodiments and comparative examples
[0065]
[0066] Table 440kg test coke oven heating program
[0067]
[0068] Table 5: Test indexes of coke produced in Examples and Comparative Examples
[0069]
[0070] It can be seen from Table 3 that as the proportion of Baopingwan non-caking coal increases, the ash and sulfur content of the blended coal gradually decrease, while the volatile matter gradually increases. This is because the ash and sulfur content of low-rank bituminous coal itself is low, the volatile matter is high, and the ash, sulfur and volatile matter of the coal sample are additive. After the non-caking coal is added, the G value and Y value of the blended coal are lower than those of the blended coal without non-caking coal. However, as the proportion of non-caking coal increases, the G value and Y value of the blended coal tend to increase first and then decrease. When the blending ratio is 4%, the G value and Y value reach the maximum value at the same time. It is speculated that at this ratio, the inert components and active components in the blended coal reach the optimal ratio, showing a higher G value and Y value. It can be seen from Table 5 that the volatile matter of coke made from blended coal also increases with the increase of the proportion of Baopingwan non-caking coal, while the change trend of ash and sulfur is opposite. The conversion rate of sulfur and ash in the blended coal remains almost unchanged with the proportion of Baopingwan non-caking coal added. This is because the proportion of added coal is small, which has little effect on the conversion rate of sulfur and ash in the blended coal.
[0071] Depend on Figure 1 It can be seen that the reactivity (CRI) of coke made from blended coal first decreases and then increases gradually with the increase of the proportion of Baopingwan non-caking coal, and the strength after reaction (CSR) first increases and then decreases gradually. When the proportion of Baopingwan non-caking coal is 4%, the thermal strength and thermal reactivity of coke reach the best, and the performance is closest to the coke made from blended coal without non-caking coal. Since Baopingwan non-caking coal itself cannot form coke, the ratio of inert components to active components will change with the increase of the proportion. When the proportion is 4%, the two reach the best ratio after the addition of non-caking coal, and the coking performance of the blended coal is also the best.
[0072] The addition of non-sticky coal has a tendency to worsen the thermal strength of coke. When the proportion of Baopingwan non-sticky coal is 4% or less, the thermal strength (CSR) of coke decreases slowly, and is 0.98% to 2.93% lower than the coke of the basic blended coal. When the proportion is 4%, the decrease is 0.98%, which is the smallest decrease. When the proportion increases to 6% and 10%, the thermal strength (CSR) of coke decreases significantly, with decreases of approximately 6.84% and 15.63%, respectively. Therefore, when the current proportion of Baopingwan non-sticky coal is controlled at 4%, the performance of the coke produced is the best. Based on the blended coal with the same structure, the corresponding relationship between the thermal state of coke produced by the experimental coke oven and the production coke oven is shown. [1] It can be predicted that the blended coal prepared in the proportions according to the specific implementation mode of the present invention can produce coke that at least meets the requirements of secondary metallurgical coke in the national standard in the production coke oven.
[0073] Non-sticky coal has no adhesiveness and cannot form coke by itself during the coking process. Generally speaking, adding non-sticky coal to low-rank bituminous coal will reduce the strength of the coke made from the blended coal. In the present invention, the proportion of non-sticky coal is controlled at about 4%, and the decrease in the thermal strength of the coke is minimal, which exceeds the expected effect. The main reasons for the analysis include: 1. Adding a certain proportion of high-quality gas fertilizer coal with good adhesiveness to compensate for the non-sticky characteristics of non-sticky coal; 2. Controlling the proportion of coking coal with good coking properties to be no less than 40%; 3. The adhesiveness and coking properties of lean coal are not significant, and its addition ratio is controlled not to exceed 10%. 4. When the proportion of non-sticky coal is 4%, the ratio of inert components to active components of the blended coal reaches the best, and the performance of the coke produced is the best.
[0074] In summary, without affecting the quality of coke, the optimal proportion of Baopingwan non-caking coal in the basic blend is 4%. Compared with Datong weakly caking coal, Baopingwan non-caking coal has the advantage of low price, which can effectively reduce the blending price. At the same time, it also broadens the coking coal resources and provides a new utilization path for the application of low-grade bituminous coal.
[0075] References
[0076] [1] Zhang Wencheng, Wang Chunhua, Lu Yongliang. Research on the simulation of experimental coke oven to production coke oven [C]. Proceedings of the 2005 China Iron and Steel Annual Conference. 2005, 2: 179-181.
[0077] Although the present application is disclosed as above with preferred embodiments, it is not intended to limit the claims. Any technical personnel in this field may make several possible changes and modifications without departing from the concept of the present application. Therefore, the scope of protection of the present application shall be based on the scope defined by the claims of the present application.
Claims
1. A method for producing metallurgical coke by blending low-rank bituminous coal, the method comprising using blended coal composed of the following proportions by mass: Non-sticky coal: 3-4 parts, weakly sticky coal: 2-6 parts, gas coal: 18-22 parts, 1 / 3 coking coal: 15-20 parts, coking coal: 45-50 parts, lean coal: 5-10 parts; The non-sticky coal V daf The range is between 33% and 37%, the ash yield is between 4% and 7%, and the total sulfur content is between 0.1% and 0.5%; The weakly caking coal V daf The range of the ash content is 31% to 34%, the range of the ash yield is 5.5% to 6.8%, the total sulfur content is 0.35% to 0.58%, and the range of the bonding index G value is 10 to 15; The V of the gas coal daf The range is 37% to 42%, the ash yield is 8.1% to 11.2%, the total sulfur content is 0.47% to 0.75%, the bonding index G value is 61 to 85, and the maximum cuticle thickness Y is 11.6 mm to 18.5 mm; The 1 / 3 V of coking coal daf The range is between 32% and 36%, the ash yield is between 5.1% and 7.7%, the total sulfur content is between 0.36% and 0.65%, and the maximum cuticle thickness Y is between 6mm and 11.2mm; The V of the coking coal daf The range is between 21% and 28%; The V of the lean coal daf The range is 16% to 21%, the ash yield range is 9.1% to 10.9%, the total sulfur content range is 0.47% to 0.75%, and the bonding index G value range is 37 to 65.
2. The method for producing metallurgical coke with low-rank bituminous coal according to claim 1, characterized in that: The coking coal includes Mengsan coking coal, Laoshidan 2.0 coking coal and Wuhushan 3.0 coking coal; Among them, the total sulfur content of Mongolian coking coal is 0.60% to 0.75%, the ash yield ranges from 9.5% to 12.24%, the G value ranges from 75 to 85, and the maximum cuticle thickness Y ranges from 15.1 mm to 16.9 mm; The total sulfur content of Laoshidan 2.0 coking coal is 1.5% to 1.8%, the ash yield ranges from 9.5% to 12.24%, the G value ranges from 82 to 100, and the maximum cuticle thickness Y value ranges from 16.5mm to 25mm; The total sulfur content of Wuhushan 3.0 coking coal is 2.7% to 3.0%, the ash yield ranges from 5.83% to 7.72%, the G value ranges from 82 to 100; the maximum cuticle thickness Y value ranges from 16.5mm to 25mm.
3. The method for producing metallurgical coke with low-rank bituminous coal according to claim 1 or 2, characterized in that: The blended coal meets the following parameters: V daf In the range of 29% to 32%, ash content A d ≤10%, total sulfur content S t, d ≤0.8%, bonding index G≥70, maximum thickness of the colloid layer Y≥13mm.
4. A blended coal for producing metallurgical coke, wherein the raw materials of the blended coal are composed of the following components in parts by weight: Non-sticky coal: 3-4 parts, weakly sticky coal: 2-6 parts, gas coal: 18-22 parts, 1 / 3 coking coal: 15-20 parts, coking coal: 45-50 parts, lean coal: 5-10 parts; Wherein, the non-sticky coal V daf The range is between 33% and 37%, the ash yield is between 4% and 7%, and the total sulfur content is between 0.1% and 0.5%; The weakly caking coal V daf The range of the ash content is 31% to 34%, the range of the ash yield is 5.5% to 6.8%, the total sulfur content is 0.35% to 0.58%, and the range of the bonding index G value is 10 to 15; The V of the gas coal daf The range is 37% to 42%, the ash yield is 8.1% to 11.2%, the total sulfur content is 0.47% to 0.75%, the bonding index G value is 61 to 85, and the maximum cuticle thickness Y is 11.6 mm to 18.5 mm; The 1 / 3 V of coking coal daf The range is between 32% and 36%, the ash yield is between 5.1% and 7.7%, the total sulfur content is between 0.36% and 0.65%, and the maximum cuticle thickness Y is between 6mm and 11.2mm; The V of the coking coal daf The range is between 21% and 28%; The V of the lean coal daf The range is 16% to 21%, the ash yield range is 9.1% to 10.9%, the total sulfur content range is 0.47% to 0.75%, and the bonding index G value range is 37 to 65.
5. The blended coal for producing metallurgical coke according to claim 4, characterized in that: The coking coal includes Mengsan coking coal, Laoshidan 2.0 coking coal and Wuhushan 3.0 coking coal; Among them, the total sulfur content of Mongolian coking coal is 0.60% to 0.75%, the ash yield ranges from 9.5% to 12.24%, the G value ranges from 75 to 85, and the maximum cuticle thickness Y ranges from 15.1 mm to 16.9 mm; The total sulfur content of Laoshidan 2.0 coking coal is 1.5% to 1.8%, the ash yield ranges from 9.5% to 12.24%, the G value ranges from 82 to 100, and the maximum cuticle thickness Y value ranges from 16.5mm to 25mm; The total sulfur content of Wuhushan 3.0 coking coal is 2.7% to 3.0%, the ash yield ranges from 5.83% to 7.72%, the G value ranges from 82 to 100; the maximum cuticle thickness Y value ranges from 16.5mm to 25mm.
6. The blended coal for producing metallurgical coke according to claim 4 or 5, characterized in that: The blended coal meets the following parameters: volatile matter V daf In the range of 29% to 32%, ash content A d ≤10%, total sulfur content S t, d ≤0.8%, bonding index G≥70, maximum thickness of the colloid layer Y≥13mm.