Preparation method and application of heteroatom-doped biochar

Through one-step pyrolysis method and directional design method, the problems of high development cost and limited performance of heteroatom-doped biochar are solved, and low-cost, high-performance CO2 adsorption and cycle stability are achieved, which is suitable for efficient CO2 removal in flue gas. capture.

CN117623302BActive Publication Date: 2024-10-11ZHEJIANG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311639615.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-01
Publication Date
2024-10-11
Estimated Expiration
2043-12-01

AI Technical Summary

Technical Problem

Research on heteroatom-doped biochar in the existing technology has problems such as high development costs and limited carbon capture performance. This is mainly due to the wide variety of heteroatom doping forms and the lack of directional theoretical guidance, which results in a complicated and expensive preparation process and is harmful to other atoms. There are few researches on doping.

Method used

A one-step pyrolysis method is used to prepare heteroatom-doped biochar, DFT calculations are used to screen excellent doping forms, and GCMC simulation is used to verify the CO2 adsorption performance. Combined with cheap carbon source materials and activators, directional design and low-cost preparation of materials are achieved. .

Benefits of technology

It reduces the number of experimental trials and errors, reduces material development costs, improves CO2 adsorption capacity and CO2/N2 selectivity, achieves high-performance capture of CO2 in flue gas, and demonstrates excellent cycle performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117623302B_ABST
    Figure CN117623302B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing heteroatom-doped biochar: 1 part of carbon source material, 1-6 parts of activator and 0.5-1.5 parts of heteroatom dopant are placed in a grinder for physical grinding and fully mixing; the mixture is heated to 600-1000°C under a protective gas environment and maintained for 45-90 minutes; the mixture is cooled naturally, and the carbonized black substance is stirred with deionized water at room temperature for 10-20 hours; the solid substance is repeatedly washed with deionized water until the solution is neutral; the washed material is placed in an oven for drying to obtain heteroatom-doped biochar. Boron atoms, phosphorus atoms and sulfur atoms are selected as heteroatom dopants to prepare corresponding boron-doped, phosphorus-doped and sulfur-doped biochars respectively. The specific doping form of the biochar is a monomer. The preparation adopts a one-step pyrolysis method, and there is no acid-base solvent involved in the whole process. The process is simple and environmentally friendly. The prepared heteroatom-doped biochar is not only rich in a large number of ultra-microporous structures, but also has abundant surface functional groups, and can achieve high-performance adsorption of flue gas CO2.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of doped biochar preparation, and in particular to a preparation method and application of heteroatom-doped biochar. Background Art

[0002] Excessive CO2 emissions have caused a series of problems such as global warming. Although the world has proposed corresponding carbon emission reduction measures, according to the "CO2 Emissions in 2022" report released by the IEA, global CO2 emissions in 2022 exceeded 36.8 billion tons, reaching a historical high. Among them, emissions from the power industry accounted for 39.3% of the total emissions. Therefore, it is imperative to reduce CO2 emissions in the global power industry. Among them, the solid adsorption method is considered to be one of the most promising carbon capture technologies in the future due to its low capture energy consumption, good thermal stability, excellent cycle performance, and high selectivity.

[0003] At present, solid adsorbents that have been widely used for CO2 capture include zeolite molecular sieves, organic metal frameworks, mesoporous silicon, alkali metal carbonates, porous carbon materials, organic polymers, etc. The biggest common point of these materials is that they have rich pore structures, and the adsorption of CO2 by porous structures is a typical physical adsorption, and the CO2 concentration and adsorption temperature have a great influence on physical adsorption. The CO2 concentration in flue gas is low and the adsorption temperature is relatively high. Therefore, relying solely on rich pore structures is obviously not enough to achieve high-performance capture of CO2 in flue gas. Many functionalized materials have been developed for efficient capture of low-concentration CO2 at high temperatures. Among them, heteroatom doping technology can change the polarity of the material by changing the skeleton structure and electronic configuration of the original material, thereby improving the capture performance of CO2. Heteroatom-doped biochar combines the advantages of simple biochar preparation method, wide source of raw materials, low cost and specific adsorption brought by heteroatom doping, and is a very promising solid adsorbent.

[0004] At present, the main atoms used for doping are boron, nitrogen, phosphorus, sulfur, etc., which are mainly used in adsorption separation, organic catalysis, sensors, energy conversion and storage, etc. The heteroatom-doped carbon materials used for CO2 adsorption are mainly focused on nitrogen doping, and the research on other types of atomic doping is very limited. The main reasons are as follows: On the one hand, due to the various forms of heteroatom doping and the lack of directional theoretical guidance, the development process is complicated and expensive. On the other hand, there is no systematic research on heteroatom-doped biochar, and the adsorption performance of the prepared materials is relatively limited. Zaman et al. [1] A sulfur-doped carbon material was prepared using p-toluenesulfonic acid as a precursor and sodium chloride as a pore-forming agent. However, the maximum CO2 adsorption capacity of this material at 0.15 bar and 25°C was only 0.78 mmol / g, which was relatively limited.

[0005] In summary, there are two problems in the current research on heteroatom-doped biochar: First, due to the various forms of heteroatom doping, each doping form has a different effect on carbon capture performance, so a large number of trial experiments are required to optimize the performance. A large number of trial and error times lead to a high cost for the development of heteroatom-doped biochar. Second, the research on heteroatom-doped biochar is mainly nitrogen-doped biochar, and there is less research on other atomic doping, and there is no systematic research to reveal the impact of each heteroatom doping form on the carbon capture performance of biochar. Therefore, the carbon capture performance of the prepared heteroatom-doped biochar is limited.

[0006] [1]Zaman AC, Karaaslan O F.Sulfur / Oxygen-Doped Porous Carbon viaNaCl-Assisted Thermolysis of Molecular Precursor for CO2 Capture[J].MaterialsChemistry and Physics,2021:125288. Summary of the invention

[0007] In order to solve at least one of the problems existing in the preparation of heteroatom-doped biochar in the prior art, the present invention provides a preparation method and application of heteroatom-doped biochar. The preparation adopts a one-step pyrolysis method without the participation of acid, alkali and solvent in the whole process. The process is simple and environmentally friendly. The prepared heteroatom-doped biochar is not only rich in a large number of ultra-microporous structures, but also has abundant surface functional groups, which can achieve high-performance adsorption of flue gas CO2.

[0008] To achieve the above object, the present invention provides the following technical solutions:

[0009] The first aspect of the present invention provides a method for preparing heteroatom-doped biochar, comprising the following steps:

[0010] S1, placing 1 part of carbon source material, 1-6 parts of activator and 0.5-1.5 parts of heteroatom dopant in a grinder and physically grinding and mixing them thoroughly;

[0011] S2, heating the mixture to 600-1000°C under a protective gas environment and maintaining the temperature for 45-90 minutes;

[0012] S3, after step S2 is completed, the temperature is naturally lowered, and the carbonized black substance is stirred with deionized water at room temperature for 10-20 hours;

[0013] S4. After step S3 is completed, the solid material is repeatedly washed with deionized water until the solution is neutral;

[0014] S5. The washed material is placed in an oven to dry to obtain heteroatom-doped biochar; in some specific embodiments, the washed material is placed in an oven at 105° C. to dry for 12 hours.

[0015] In some embodiments of the present invention, the heteroatom dopant is one of a boron atom dopant, a phosphorus atom dopant, and a sulfur atom dopant.

[0016] In some embodiments of the present invention, the boron atom dopant is a borate, preferably one of potassium metaborate, potassium borate, sodium metaborate, sodium borate, calcium metaborate, calcium borate, and magnesium borate.

[0017] In some embodiments of the present invention, the phosphorus atom dopant is a phosphate, preferably one of tripotassium phosphate, potassium dihydrogen phosphate, potassium hydrogen phosphate, sodium phosphate, sodium dihydrogen phosphate, sodium hydrogen phosphate, magnesium phosphate, magnesium dihydrogen phosphate, and magnesium hydrogen phosphate.

[0018] In some embodiments of the present invention, the sulfur atom dopant is a sulfate, preferably one of potassium sulfate, sodium sulfate, calcium sulfate and magnesium sulfate.

[0019] In some embodiments of the present invention, the carbon source material is a biomass carbon source material, such as corn cob powder, wood powder, bamboo powder, agricultural waste, straw powder, etc.

[0020] In some embodiments of the invention, the activator is potassium carbonate.

[0021] In some embodiments of the present invention, the protective gas environment in step S2 is: the protective gas is nitrogen, the flow rate is 100-200 mL / min, and the heating rate is 5-10°C / min. In some embodiments of the present invention, the mixture is heated to 800°C at a heating rate of 5-10°C / min under a nitrogen atmosphere of 100-200 mL / min and maintained for 1 hour.

[0022] The second aspect of the present invention provides heteroatom-doped biochar prepared according to the method described in the first aspect.

[0023] The third aspect of the present invention provides the use of the heteroatom-doped biochar described in the second aspect in carbon capture, such as the adsorption of CO2 in flue gas.

[0024] The present invention also provides a method for directional design of heteroatom-doped biochar, comprising the following steps: firstly, constructing biochar molecular models doped with different heteroatom forms, using DFT to calculate CO2 adsorption energy, N2 adsorption energy and CO2 / N2 theoretical selectivity on different biochar models, and selecting a suitable specific doping form according to the CO2 adsorption energy and theoretical selectivity.

[0025] Subsequently, the specific doping form selected by DFT calculation was selected as a monomer, and a nanoscale porous material model was constructed. GCMC was used to simulate the CO2 adsorption isotherms and other performance data on different nanoscale porous material models to further verify the results of DFT calculation screening.

[0026] Finally, a one-step pyrolysis method was used to prepare biochar doped with the above heteroatom forms.

[0027] Beneficial Effects of the Invention

[0028] Compared with the prior art, the present invention has the following beneficial effects: Based on DFT screening, the present invention provides a directional design idea and method for heteroatom-doped biochar, and uses DFT theoretical calculations to screen out heteroatom-doped forms BCO2, PC and CSC with excellent adsorption performance from the perspective of molecular atoms through CO2 adsorption energy, N2 adsorption energy and CO2 / N2 theoretical selectivity, providing a specific doping direction for subsequent research. Subsequently, GCMC molecular simulation was used to further verify the results of DFT calculations at the nanoscale by calculating the CO2 adsorption isotherms on the above three forms of doped biochar. The CO2 adsorption isotherm results show that heteroatom doping can improve the CO2 adsorption capacity of biochar under low pressure. The specific doping form selected according to the DFT calculation is a monomer, and finally a one-step pyrolysis method is used to directionally prepare biochar doped with the above-screened doping form to achieve excellent CO2 adsorption. The theoretical calculation-guided experiment proposed in the present invention realizes the directional preparation of heteroatom doping, reduces the number of trial and error experiments, and reduces the cost of material development.

[0029] The heteroatom-doped biochar prepared by the present invention uses waste biomass carbon source materials such as corn cobs as raw materials, and the activator and dopant are both cheap chemicals. Moreover, activation and modification can be achieved in one step, and the preparation cost is low.

[0030] The one-step pyrolysis method adopted in the present invention does not involve any acid, alkali or solvent throughout the process, and the process is simple and environmentally friendly. The prepared heteroatom-doped biochar is not only rich in a large number of ultra-microporous structures, but also has abundant surface functional groups. The heteroatom-doped biochar prepared in the present invention has excellent CO2 adsorption performance and CO2 / N2 selectivity, as well as excellent cycle performance, can achieve high-performance adsorption of flue gas CO2, and can be reused. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 The SEM images of biochar prepared in Example 1, Example 5, Example 8 and Comparative Example 1 of the present invention; wherein A corresponds to the result of Example 1, B corresponds to the result of Example 5, C corresponds to the result of Example 8, and D corresponds to the result of Comparative Example 1;

[0032] Figure 2A comparison chart of the adsorption capacity and CO2 / N2 selectivity of the biochar prepared in Example 1, Example 5, Example 8 and Comparative Example 1 of the present invention at 37°C;

[0033] Figure 3 A comparison chart of the adsorption capacity and CO2 / N2 selectivity of the biochar prepared in Example 1, Example 5, Example 8 and Comparative Example 1 of the present invention at 55°C;

[0034] Figure 4 A comparison chart of the adsorption capacity and CO2 / N2 selectivity of the biochar prepared in Example 1, Example 5, Example 8 and Comparative Example 1 of the present invention at 72°C;

[0035] Figure 5 This is a cycle performance test curve of the boron-doped biochar prepared in Example 1 of the present invention;

[0036] Figure 6 This is a cycle performance test curve of the phosphorus-doped biochar prepared in Example 5 of the present invention;

[0037] Figure 7 This is a cycle performance test curve of the sulfur-doped biochar prepared in Example 8 of the present invention;

[0038] Figure 8 A schematic diagram of the idea of ​​directional design of heteroatom-doped biochar and the corresponding preparation method in the present invention;

[0039] Fig. 9 The CO2 adsorption energy, N2 adsorption energy and theoretical selectivity of biochar doped with different heteroatom forms obtained by DFT calculation in the present invention;

[0040] Fig.10 This is the CO2 adsorption isotherm of biochar doped with different heteroatoms at 25°C and 0-1 bar obtained by GCMC simulation in the present invention. DETAILED DESCRIPTION

[0041] The following examples are used to demonstrate preferred embodiments of the present invention. It will be appreciated by those skilled in the art that the techniques disclosed in the following examples represent techniques that the inventors have discovered that can be used to implement the present invention and therefore can be considered as preferred embodiments of the present invention. However, it will be appreciated by those skilled in the art based on this specification that many modifications can be made to the specific embodiments disclosed herein and still achieve the same or similar results without departing from the spirit or scope of the present invention. Those skilled in the art will recognize or will understand through routine experimentation many equivalent techniques for the specific embodiments of the invention described herein. These equivalents will be included in the claims.

[0042] A method for preparing heteroatom-doped biochar comprises the following steps:

[0043] S1. Place 1 part of biomass carbon source material, 1-6 parts of potassium carbonate and 0.5-1.5 parts of heteroatom dopant: one of sulfate, phosphate and borate in a grinder, grind and mix them thoroughly;

[0044] S2, heating the mixture to 600-1000° C. at a heating rate of 5-10° C. / min under a nitrogen atmosphere of 100-200 mL / min and maintaining for 45-90 min;

[0045] S3. After natural cooling, the carbonized black substance is stirred with deionized water at room temperature for 10-20 hours;

[0046] S4. The solid material is repeatedly washed with deionized water until the solution is neutral;

[0047] S5. The washed material is placed in an oven at 105° C. and dried for 12 hours to obtain heteroatom-doped biochar.

[0048] Among them, the borate can be one of potassium metaborate, potassium borate, sodium metaborate, sodium borate, calcium metaborate, calcium borate, and magnesium borate; the phosphate can be one of tripotassium phosphate, potassium dihydrogen phosphate, potassium hydrogen phosphate, sodium phosphate, sodium dihydrogen phosphate, sodium hydrogen phosphate, magnesium phosphate, magnesium dihydrogen phosphate, and magnesium hydrogen phosphate; the sulfate can be one of potassium sulfate, sodium sulfate, calcium sulfate, and magnesium sulfate.

[0049] Example 1

[0050] First, 5g corn cob powder, 5g potassium metaborate and 15g potassium carbonate were physically ground in a mortar for 30 minutes for thorough mixing; then the mixture was heated to 800°C at a heating rate of 10°C / min under a nitrogen atmosphere of 100mL / min and maintained for 1 hour. After natural cooling, the carbonized black substance was transferred to a beaker and 200mL of deionized water was added and stirred at room temperature for 12 hours. The stirred material was repeatedly washed and filtered with 1000mL of deionized water until the solution was neutral. Finally, the washed material was dried in an oven at 105°C for 12 hours to obtain boron-doped biochar.

[0051] Example 2

[0052] First, 5g corn straw powder, 7.5g magnesium borate and 30g potassium carbonate were physically ground in a mortar for 30 minutes for thorough mixing; then the mixture was heated to 600℃ at a heating rate of 10℃ / min under a nitrogen atmosphere of 100mL / min and maintained for 1 hour. After natural cooling, the carbonized black substance was transferred to a beaker and 200mL deionized water was added and stirred at room temperature for 12 hours. The stirred material was repeatedly washed and filtered with 1000mL deionized water until the solution was neutral. Finally, the washed material was dried in an oven at 105℃ for 12 hours to obtain boron-doped biochar.

[0053] Example 3

[0054] First, 5g of sawdust, 2.5g of sodium metaborate and 5g of potassium carbonate were physically ground in a mortar for 30 minutes for thorough mixing; then the mixture was heated to 800°C at a heating rate of 10°C / min under a nitrogen atmosphere of 100mL / min and maintained for 1 hour. After natural cooling, the carbonized black substance was transferred to a beaker and 200mL of deionized water was added and stirred at room temperature for 12 hours. The stirred material was repeatedly washed and filtered with 1000mL of deionized water until the solution was neutral. Finally, the washed material was dried in an oven at 105°C for 12 hours to obtain boron-doped biochar.

[0055] Example 4

[0056] First, 5g of pine wood powder, 5g of calcium borate and 25g of potassium carbonate were physically ground in a mortar for 30 minutes for thorough mixing; then the mixture was heated to 800°C at a heating rate of 8°C / min under a nitrogen atmosphere of 100mL / min and maintained for 1 hour. After natural cooling, the carbonized black material was transferred to a beaker and 200mL of deionized water was added and stirred at room temperature for 12 hours. The stirred material was repeatedly washed and filtered with 1000mL of deionized water until the solution was neutral. Finally, the washed material was dried in an oven at 105°C for 12 hours to obtain boron-doped biochar.

[0057] Example 5

[0058] First, 5g corn cob powder, 5g tripotassium phosphate and 15g potassium carbonate were physically ground in a mortar for 30 minutes for thorough mixing. Then the mixture was heated to 800°C at a heating rate of 10°C / min under a nitrogen atmosphere of 100mL / min and maintained for 1 hour. After natural cooling, the carbonized black substance was transferred to a beaker and 200mL of deionized water was added and stirred at room temperature for 12 hours. The stirred material was repeatedly washed and filtered with 1000mL of deionized water until the solution was neutral. Finally, the washed material was dried in an oven at 105°C for 12 hours to obtain phosphorus-doped biochar.

[0059] Example 6

[0060] First, 5g of bamboo powder, 7.5g of sodium dihydrogen phosphate and 25g of potassium carbonate were physically ground in a mortar for 30 minutes for thorough mixing. Then the mixture was heated to 1000°C at a heating rate of 10°C / min under a nitrogen atmosphere of 100mL / min and maintained for 1 hour. After natural cooling, the carbonized black substance was transferred to a beaker and 200mL of deionized water was added and stirred at room temperature for 12 hours. The stirred material was repeatedly washed and filtered with 1000mL of deionized water until the solution was neutral. Finally, the washed material was dried in an oven at 105°C for 12 hours to obtain phosphorus-doped biochar.

[0061] Example 7

[0062] First, 5g of bark powder, 2.5g of magnesium hydrogen phosphate and 7.5g of potassium carbonate were physically ground in a mortar for 30 minutes for thorough mixing. Then the mixture was heated to 800°C at a heating rate of 10°C / min under a nitrogen atmosphere of 100mL / min and maintained for 1 hour. After natural cooling, the carbonized black substance was transferred to a beaker and 200mL of deionized water was added and stirred at room temperature for 12 hours. The stirred material was repeatedly washed and filtered with 1000mL of deionized water until the solution was neutral. Finally, the washed material was dried in an oven at 105°C for 12 hours to obtain phosphorus-doped biochar.

[0063] Example 8

[0064] First, 5g of wheat straw powder, 5g of potassium sulfate and 15g of potassium carbonate were physically ground in a mortar for 30 minutes for thorough mixing. Then the mixture was heated to 700°C at a heating rate of 10°C / min under a nitrogen atmosphere of 100mL / min and maintained for 1 hour. After natural cooling, the carbonized black substance was transferred to a beaker and 200mL of deionized water was added and stirred at room temperature for 12 hours. The stirred material was repeatedly washed and filtered with 1000mL of deionized water until the solution was neutral. Finally, the washed material was dried in an oven at 105°C for 12 hours to obtain sulfur-doped biochar.

[0065] Example 9

[0066] First, 5g corn cob powder, 6g sodium sulfate and 25g potassium carbonate were physically ground in a mortar for 30 minutes for thorough mixing. Then the mixture was heated to 800℃ at a heating rate of 10℃ / min under a nitrogen atmosphere of 100mL / min and maintained for 1 hour. After natural cooling, the carbonized black substance was transferred to a beaker and 200mL of deionized water was added and stirred at room temperature for 12 hours. The stirred material was repeatedly washed and filtered with 1000mL of deionized water until the solution was neutral. Finally, the washed material was dried in an oven at 105℃ for 12 hours to obtain sulfur-doped biochar.

[0067] Example 10

[0068] First, 5g of pine wood powder, 3g of calcium sulfate and 6g of potassium carbonate were physically ground in a mortar for 30 minutes for thorough mixing. Then the mixture was heated to 1000°C at a heating rate of 10°C / min under a nitrogen atmosphere of 100mL / min and maintained for 1 hour. After natural cooling, the carbonized black substance was transferred to a beaker and 200mL of deionized water was added and stirred at room temperature for 12 hours. The stirred material was repeatedly washed and filtered with 1000mL of deionized water until the solution was neutral. Finally, the washed material was dried in an oven at 105°C for 12 hours to obtain sulfur-doped biochar.

[0069] Embodiment 11

[0070] First, 5g of yellow bamboo powder, 5g of magnesium sulfate and 20g of potassium carbonate were physically ground in a mortar for 30 minutes for thorough mixing. Then the mixture was heated to 800°C at a heating rate of 10°C / min under a nitrogen atmosphere of 100mL / min and maintained for 1 hour. After natural cooling, the carbonized black substance was transferred to a beaker and 200mL of deionized water was added and stirred at room temperature for 12 hours. The stirred material was repeatedly washed and filtered with 1000mL of deionized water until the solution was neutral. Finally, the washed material was dried in an oven at 105°C for 12 hours to obtain sulfur-doped biochar.

[0071] Comparative Example 1

[0072] First, 5g corn cob powder and 15g potassium carbonate were physically ground in a mortar for 30 minutes for thorough mixing. Then the mixture was heated to 800℃ at a heating rate of 10℃ / min under a nitrogen atmosphere of 100mL / min and maintained for 1 hour. After natural cooling, the carbonized black substance was transferred to a beaker and 200mL of deionized water was added and stirred at room temperature for 12 hours. The stirred material was repeatedly washed and filtered with 1000mL of deionized water until the solution was neutral. Finally, the washed material was dried in an oven at 105℃ for 12 hours to obtain the original biochar.

[0073] Performance Testing and Characterization

[0074] (1) The biochar prepared in Example 1, Example 5, Example 8 and Comparative Example 1 was subjected to SEM testing. The results are as follows: Figure 1 shown.

[0075] Depend on Figure 1 It can be seen that heteroatom dopants have a certain promoting effect on the morphology of pores. Both boron-doped and phosphorus-doped biochars appear as blocks with a large number of circular pores, while sulfur-doped biochars appear as multilayer fragments with a large number of pores. Figure 1 It can be found that the pores of the original biochar are not completely etched, and it can be inferred that its specific surface area is relatively low.

[0076] (2) The pore structure of the biochar prepared in Example 1, Example 5, Example 8 and Comparative Example 1 was characterized. The results are shown in Table 1.

[0077] Table 1 Pore structure characterization results of biochar

[0078]

[0079] It can be seen from Table 1 above that heteroatom dopants can increase the specific surface area and total pore volume of biochar, which verifies the speculation that the original biochar has the lowest specific surface area in the SEM test. The ultramicropore area and ultramicropore volume of boron-doped and phosphorus-doped biochar are close to those of the original biochar. Although sulfur-doped biochar has the highest specific surface area and total pore volume, its ultramicropore structure is the least. From the distribution of pore structure, it can be inferred that boron-doped and phosphorus-doped biochars will have higher CO2 adsorption than sulfur-doped biochar because they have more ultramicropores.

[0080] (3) The XPS surface element test was performed on the biochar prepared in Example 1, Example 5, Example 8 and Comparative Example 1. The results are shown in Table 2.

[0081] Table 2 XPS element distribution of biochar

[0082]

[0083] It can be seen from Table 2 that the three heteroatom-doped biochars prepared in Example 1, Example 5, and Example 8 are all doped with corresponding elements, indicating that the heteroatom doping is successful. Among them, the sulfur doping and boron doping contents are relatively high, while the phosphorus doping ratio is relatively low. The original biochar prepared in Comparative Example 1 is not doped with other heteroatoms.

[0084] (4) The CO2 adsorption performance and CO2 / N2 selectivity of the biochar prepared in Example 1, Example 5, Example 8 and Comparative Example 1 were tested using a thermogravimetric analyzer at temperatures of 37°C, 55°C and 72°C, respectively.

[0085] The specific test process is as follows: First, add about 5 mg of biochar into the crucible, degas in 100 mL / min N2 at 100 ° C for 20 minutes to remove impurities in the biochar. The mass at this time is recorded as m1. Then adjust the temperature to the target adsorption temperature, and the mass at this time is recorded as m2. After reaching the target adsorption temperature, switch the pure nitrogen to 100 mL / min pure CO2 for a 1-hour adsorption experiment. The mass after the adsorption is completed is recorded as m3. Formulas (1) and (2) are used to calculate the N2 and CO2 adsorption capacity (Q) of biochar N2 and Q CO2 ):

[0086]

[0087]

[0088] The results of CO2 adsorption, N2 adsorption and CO2 / N2 selectivity of the biochar prepared in Example 1, Example 5, Example 8 and Comparative Example 1 are as follows: Figures 2 to 4 shown.

[0089] Depend on Figures 2 to 4 It can be found that at the same adsorption temperature, the CO2 adsorption capacity of phosphorus-doped and boron-doped biochars is higher than that of original biochar. Among them, the CO2 adsorption capacity of phosphorus-doped biochar at 72°C and 1 bar is 1.34 mmol / g, which is 10.7% higher than the adsorption capacity of original biochar and higher than most studies published so far. Combined with the results of pore structure analysis, it can be seen that the increase in CO2 adsorption capacity of phosphorus-doped and boron-doped biochars is mainly attributed to the doping of heteroatoms. In addition, the ratio of CO2 and N2 adsorption is defined as CO2 / N2 selectivity. It can be seen that at all temperatures, the selectivity of the three heteroatom-doped biochars is higher than that of the original biochar, which not only verifies the previous DFT calculation results, but also means that heteroatom-doped biochars can show better CO2 capture performance than original biochar in actual flue gas.

[0090] (5) The cycle performance of the boron-doped biochar, phosphorus-doped biochar and sulfur-doped biochar prepared in Example 1, Example 5 and Example 8 was tested. The test curve results are shown in FIG. Figures 5 to 7 shown.

[0091] Depend on Figure 5 It can be seen that the mass increase of boron-doped biochar after multi-temperature adsorption is only 0.19%, which basically achieves complete desorption of CO2, reflecting good chemical stability. In addition, the second CO2 adsorption of boron-doped biochar is as high as 113.4 mg / g, which is only 0.4% lower than the first 113.9 mg / g, showing excellent cycle performance.

[0092] Depend on Figure 6 It can be seen that the mass increase of phosphorus-doped biochar after multi-temperature adsorption is only 0.54%, and CO2 is basically completely desorbed, showing good chemical stability. The second CO2 adsorption of phosphorus-doped biochar reached 113.7 mg / g, which is only 0.7% lower than the first 114.5 mg / g, and also showed excellent cycle performance.

[0093] Depend on Figure 7 It can be seen that although the sulfur-doped biochar has a low adsorption capacity due to the small distribution of ultra-micropores, its mass increase after adsorption in multiple temperature sections is only 0.11%, and it also achieves complete desorption of CO2, reflecting good chemical stability. The second CO2 adsorption capacity of sulfur-doped biochar is only 0.6% lower than the first one, which also shows excellent cycle performance.

[0094] In summary, heteroatom-doped biochar can have excellent adsorption properties while also having excellent chemical stability and cyclic stability, and can be recycled multiple times in practical applications.

[0095] (6) Directed design and verification of heteroatom-doped biochar, see Figures 8 to 10 .

[0096] The idea of ​​directional design of heteroatom-doped biochar and the corresponding preparation method are as follows Figure 8 As shown, the following steps are included: first, DFT theoretical calculations are used to screen out heteroatom doped forms BCO2, PC and CSC with excellent adsorption performance from the perspective of molecular atoms through three aspects: CO2 adsorption energy, N2 adsorption energy and CO2 / N2 theoretical selectivity, such as Fig. 9As shown, it provides a specific doping direction for subsequent research. Subsequently, GCMC molecular simulation was used to further verify the results of DFT calculation by calculating the CO2 adsorption isotherms on the above three forms of doped biochar at the nanoscale. The CO2 adsorption isotherm results showed that heteroatom doping can improve the CO2 adsorption capacity of biochar at low pressure, such as Fig.10 shown.

[0097] Finally, a one-step pyrolysis method was used to directionally prepare biochar doped with the above-screened doping forms.

[0098] The relevant test results of the aforementioned embodiments show that the heteroatom-doped biochar prepared by the present invention has excellent CO2 adsorption performance and CO2 / N2 selectivity, and has excellent recycling performance, and can be reused in high-performance adsorption of flue gas CO2.

[0099] All documents mentioned in the present invention are cited as references in this application, just as each document is cited as references separately. In addition, after reading the above teachings of the present invention, those skilled in the art may make various changes or modifications to the present invention, and these equivalent forms also fall within the scope defined by the claims attached to this application.

Claims

1. An application of heteroatom-doped biochar in CO2 capture, characterized in that: The steps include: (1) Directed design of heteroatom-doped biochar: construct molecular models of biochar doped with different heteroatom forms, use DFT to calculate the CO2 adsorption energy, N2 adsorption energy and CO2 / N2 theoretical selectivity on different biochar models; select the appropriate specific doping form based on the CO2 adsorption energy and theoretical selectivity; (2) Verification of screening results: Based on the specific doping form screened out by DFT calculation, a nanoscale porous material model is constructed. GCMC is used to simulate the CO2 adsorption isotherm and other performance data on different nanoscale porous material models to further verify the results of DFT calculation screening; (3) One-step pyrolysis method for the preparation of heteroatom-doped biochar; the method is as follows: S1, placing 1 part of carbon source material, 1-6 parts of activator and 0.5-1.5 parts of heteroatom dopant in a grinder and physically grinding and mixing them thoroughly; S2, heating the mixture to 600-1000°C under a protective gas environment and maintaining the temperature for 45-90 minutes; S3, after step S2 is completed, the temperature is naturally lowered, and the carbonized black substance is stirred with deionized water at room temperature for 10-20 hours; S4. After step S3 is completed, the solid material is repeatedly washed with deionized water until the solution is neutral; S5, placing the washed material in an oven to dry to obtain heteroatom-doped biochar; The heteroatom dopant is one of a boron atom dopant, a phosphorus atom dopant, and a sulfur atom dopant; The boron atom dopant is a borate: one of potassium metaborate, potassium borate, sodium metaborate, sodium borate, calcium metaborate, calcium borate, and magnesium borate; The phosphorus atom dopant is a phosphate: one of tripotassium phosphate, potassium dihydrogen phosphate, potassium hydrogen phosphate, sodium phosphate, sodium dihydrogen phosphate, sodium hydrogen phosphate, magnesium phosphate, magnesium dihydrogen phosphate, and magnesium hydrogen phosphate; The sulfur atom dopant is a sulfate: one of potassium sulfate, sodium sulfate, calcium sulfate and magnesium sulfate.

2. The use according to claim 1, characterized in that: The carbon source material is a biomass carbon source material.

3. The use according to claim 1, characterized in that: The activator is potassium carbonate.

4. The use according to claim 1, characterized in that: The protective gas environment in step S2 is: the protective gas is nitrogen, the flow rate is 100-200 mL / min, and the heating rate is 5-10°C / min.