Two-component aspartame polyurea coating based on interpenetrating polymer network IPN and its application
By introducing polyurea modified polyaspartate and polyacrylate copolymers into asparagus polyurea coatings, combined with organic boronamine complexes, the adhesion of asparagus polyurea coatings on low-surface energy materials is solved. The problem of insufficient has achieved high adhesion and simplified coating process to meet the needs of high performance protection.
Patent Information
- Application Number
- CN202311630277.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-01
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2043-12-01
AI Technical Summary
Asparagus polyurea coatings have insufficient adhesion on low-surface energy materials such as EPDM and PP, and PP water primer is required to improve adhesion. The traditional two-coating coating process is complex and it is difficult to meet the needs of high-performance protection.
Using two-component asparagus polyurea coating based on interpenetrating polymer networks, the use of organic boronamine complex initiators is simplified to single The track coating process is applied directly to low-surface energy substrates.
It realizes high adhesion of asparagus polyurea coating on low surface energy materials, simplifies the coating process, has excellent properties such as high-temperature adhesion, low-temperature elasticity, aging resistance, moisture and heat resistance, salt spray resistance, etc., and meets high-performance protection requirements. .
Smart Images

Figure CN117625022B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to asparagine polyurea coatings, and in particular to two-component asparagine polyurea coatings based on interpenetrating polymer networks (IPNs) and their applications. Background Art
[0002] Aliphatic asparagus polyurea coating is a new type of polyurea coating. Due to the hindered amine structure and secondary amino active groups on its main chain, its coating performance has outstanding characteristics such as aging resistance, corrosion resistance, high gloss, high toughness, fast curing and easy construction. Therefore, it is more suitable for industrial application than traditional aromatic polyurea coatings. In recent years, the product forms of asparagus polyurea coatings cover solvent-based systems, high solid systems, solvent-free systems and water-based systems. Its application scope involves railway vehicles, rail transportation, bridge steel structures, automobile manufacturing and repair, construction machinery, containers, mining machinery and wood products. However, despite this, the defects of asparagus polyurea coatings are also quite obvious, that is, its adhesion to the substrate (including metal, rubber and plastic substrates) is significantly lower than that of traditional coatings such as acrylates and epoxies. The main reason for this is that the high polarity and high activity of the amino group lead to high surface tension and fast curing speed of the coating, which affects the bonding performance of the coating film with the substrate.
[0003] The defect of adhesion of asparagus polyurea coating seriously restricts its application in some special occasions, especially on low surface energy materials. For example, high-speed train EPDM windshield rubber and automobile polypropylene (PP) bumper need to use special coatings with high performance such as high aging resistance, high corrosion resistance, high flexibility and high impact resistance as protective layers, which are particularly suitable for the inherent characteristics of asparagus polyurea coating. However, these EPDM and PP materials are low surface energy materials. In the traditional coating process, a primer (PP water) that can improve adhesion must be applied first, and then the middle coating and top coating are applied. Although the performance of asparagus polyurea coating can combine the middle coating and top coating in the traditional process, it still needs to rely on PP water primer to ensure the adhesion of asparagus polyurea coating. Summary of the invention
[0004] Purpose of the Invention
[0005] The present invention provides a two-component aspartame polyurea coating based on an interpenetrating polymer network (IPN) for low surface energy synthetic materials such as EPDM and PP, so that the coating can be directly applied on low surface energy substrates such as EPDM and PP without the need for a PP water primer. At the same time, the traditional two-coat (midcoat + topcoat) process can be simplified to a single-coat (topcoat) process.
[0006] Technical Solution
[0007] The present invention patent firstly relates to a two-component asparagine polyurea coating based on an interpenetrating polymer network IPN; the present invention patent also relates to a preparation method of a two-component asparagine polyurea coating based on an interpenetrating polymer network IPN; the present invention patent further relates to a method for using a two-component asparagine polyurea coating based on an interpenetrating polymer network IPN on a low surface energy synthetic material base.
[0008] The present invention relates to a two-component asparagine polyurea coating based on an interpenetrating polymer network (IPN), characterized in that the first polymer constituting the IPN is an aliphatic polyurea crosslinker, and the second polymer constituting the IPN is a polyacrylate copolymer.
[0009] The aliphatic polyurea crosslinked product constituting the first polymer of the IPN is composed of:
[0010] 1Polyurea modified polyaspartic acid ester
[0011] 2-Polyaspartic acid
[0012] 3. Isocyanate curing agent
[0013] Cross-linked.
[0014] The polyurea-modified polyaspartic acid ester has the following structure (Formula 1):
[0015]
[0016] Wherein R1 is a C1-C6 fatty chain alkylene, a fatty cycloalkylene or a combination thereof; R2 is an alkylene of isophorone diisocyanate (IPDI), 6-methylene diisocyanate (HDI) or hydrogenated MDI (HMDI); R4 is a C10-C30 straight chain alkylene; R3 and R5 are hydrogen or a C1-C8 alkyl or ester group, which may be the same or different.
[0017] The polyacrylate copolymer constituting the second polymer of IPN is composed of:
[0018] 1Diacetone acrylamide DAAM,
[0019] 2 Hydroxyalkyl acrylate
[0020] 3 Alkyl acrylate
[0021] 4 Organic boron amine complex initiator
[0022] Combination.
[0023] The present invention also relates to a method for preparing a two-component asparagine polyurea coating based on an interpenetrating polymer network (IPN), characterized in that component A (resin component) is composed of:
[0024] 1Polyurea modified polyaspartic acid ester
[0025] 2-Polyaspartic acid
[0026] 3Diacetone acrylamide DAAM
[0027] 4 Hydroxyalkyl acrylate
[0028] 5 Alkyl acrylate
[0029] 6 Organic boron amine complex initiator
[0030] 7 Various coating additives
[0031] 8 Suitable diluent
[0032] Consists of.
[0033] Component B (curing agent component) is composed of:
[0034] 1 Isocyanate prepolymer
[0035] 2-isophorone diisocyanate (IPDI)
[0036] Consists of.
[0037] In the A component of the two-component aspartic acid polyurea coating based on the interpenetrating polymer network IPN, the preparation of the polyurea-modified polyaspartic acid ester is characterized by a two-step process, wherein the first step is to condense a bifunctional amino compound and a bifunctional aliphatic isocyanate to first obtain an isocyanate-terminated polyurea prepolymer. In the second step, the isocyanate-terminated polyurea prepolymer obtained in the first step is condensed with a polyaspartic acid ester resin to obtain the polyurea-modified polyaspartic acid ester.
[0038] In the first step, the bifunctional amino compound can be a primary amino-terminated amino polyether (such as Jeffamine D series) or a secondary amino-terminated amino polyether (such as Jeffamine SD series), including but not limited to amino-terminated polyethers with a molecular weight of 200-3000, among which secondary amino compounds with a molecular weight of 400-1000 are preferred.
[0039] The difunctional aliphatic isocyanate includes but is not limited to isophorone diisocyanate (IPDI), hexamethylene diisocyanate (HDI), hydrogenated MDI (HMDI), xylylene diisocyanate (XDI), among which IPDI and HMDI are preferred.
[0040] The equivalent ratio [NCO] / [N] of the aliphatic isocyanate and the difunctional amino compound is 2.05:1, preferably 2.0:1.
[0041] The condensation reaction of the difunctional amino compound and the aliphatic isocyanate can be carried out according to the synthesis method commonly used in the current polyurethane technology field, such as first slowly adding the difunctional amino compound dropwise into the aliphatic isocyanate at a temperature of 10-20°C, maintaining the temperature for reaction for 1-2 hours, then raising the temperature to 55-60°C to continue the reaction until the NCO% value reaches the theoretical design value, thereby obtaining an isocyanate-terminated polyurea prepolymer.
[0042] In the second step, the polyaspartic acid ester resin that undergoes a condensation reaction with the isocyanate-terminated polyurea prepolymer obtained in the first step includes but is not limited to polyaspartic acid ester products commonly used in the field of aspartic acid polyurea technology, such as Covestro's Desmophen NH1420, NH1520 and other specifications, and can also be synthesized by selecting suitable polyamines and suitable unsaturated compounds through the Michael addition process, such as the method reported in Chinese patent ZL201910161998.6.
[0043] The equivalent ratio [NCO] / [N] of the isocyanate-terminated polyurea prepolymer obtained in the first step and the polyaspartic acid ester resin is 1:1.05, preferably 1:1.
[0044] In the following descriptions, unless otherwise stated, the amounts or percentages of the components and ingredients are all calculated by weight.
[0045] The reaction of the isocyanate-terminated polyurea prepolymer and the polyaspartic acid ester resin in the second step may be carried out without adding a catalyst, or a suitable catalyst may be added to accelerate the reaction speed. Suitable catalysts include but are not limited to stannous octoate, dibutyltin dilaurate, and zinc neodecanoate. The addition amount is 0.02-0.1% of the total reaction components, preferably 0.05%.
[0046] In the second step, the reaction of the isocyanate-terminated polyurea prepolymer precursor with the polyaspartic acid ester resin may be carried out without adding a diluent, or a suitable diluent may be added to adjust the viscosity. Suitable diluents include but are not limited to toluene, xylene, tetrahydrofuran and butyl acetate. The added amount is 5-30% of the total reaction components, preferably 10-20%.
[0047] The condensation reaction of the isocyanate-terminated polyurea prepolymer and the polyaspartic acid ester resin in the second step can be carried out according to the commonly used synthesis method in the current polyurethane technical field, such as directly mixing the isocyanate-terminated polyurea prepolymer and the polyaspartic acid ester resin in a reactor, adding a solvent and a catalyst if necessary, and reacting at a temperature of 40-60° C. for 10-12 hours until the NCO% value is zero, or until the 2270 in the infrared spectrum is -1 The peaks near 147.4447.1% disappeared, thereby obtaining polyurea-modified polyaspartic acid ester.
[0048] In the A component of the two-component aspartic polyurea coating based on interpenetrating polymer network IPN, the proportion of polyurea-modified polyaspartic acid ester used can account for 10-40% of each polymer monomer in the A component, preferably 20-30%.
[0049] In the component A of the two-component aspartic polyurea coating based on interpenetrating polymer network IPN, the polyaspartic acid ester resin includes but is not limited to the polyaspartic acid ester products commonly used in the aspartic polyurea technology field, such as Covestro's Desmophen NH1420, NH1520, NH1220 and other specifications, and can also be synthesized by selecting suitable polyamines and suitable unsaturated compounds through the Michael addition process, such as the method reported in Chinese patent ZL201910161998.6. They can be used alone or in combination according to the required performance.
[0050] In the A component of the two-component aspartic polyurea coating based on interpenetrating polymer network IPN, the proportion of polyaspartic acid ester resin used can account for 10-40% of each polymer monomer in the A component, preferably 20-30%.
[0051] The polyacrylate copolymer constituting the second polymer of the IPN is diacetone acrylamide (DAAM), and its usage ratio can account for 10-30% of each polymer monomer in the A component, preferably 15-20%.
[0052] In the A component of the two-component aspartame polyurea coating based on interpenetrating polymer network IPN, the hydroxyalkyl acrylate can be hydroxyethyl acrylate or hydroxypropyl acrylate, preferably hydroxyethyl acrylate, and its usage ratio can account for 5-20% of each polymer monomer in the A component, preferably 5-10%.
[0053] In the component A of the two-component aspartame polyurea coating based on interpenetrating polymer network IPN, the alkyl acrylate can be methyl acrylate or ethyl acrylate, preferably methyl acrylate or not. Its usage amount can account for 0-10% of each polymer monomer in component A, preferably 0-5%.
[0054] In the A component of the two-component aspartame polyurea coating based on interpenetrating polymer network IPN, the organic boron amine complex is a latent initiator, which is a complex of alkyl boron and diamine. Its structural formula is shown below (Formula 2):
[0055]
[0056] In the formula, R1, R2, and R3 are C1-C10 alkyl groups, which may be the same or different. Am is a dibasic primary amine. The V value is the ratio coefficient of nitrogen atoms to boron atoms in the formula.
[0057] The diprimary amines include but are not limited to ethylenediamine, hexamethylenediamine or amino-terminated ethers with a molecular weight of 200-400, and amino-terminated polyethers with a molecular weight of 400 are preferably used.
[0058] The molar ratio of the organic borane and the diamine addition complex is determined by the V value, that is, the ratio of nitrogen atoms to boron atoms in the complex is determined to be within an effective range, and the effective ratio is 1-4:1, preferably 1:1.
[0059] The organoborane includes but is not limited to triphenylborane, triethylborane, tri-n-propylborane, tri-n-butylborane, preferably tri-n-butylborane.
[0060] The amount of the organic borane and diamine addition complex initiator used can make the boron content in the complex account for 0.05-0.8% of the total amount of the unsaturated polymerizable monomers in component A, preferably 0.1-0.3%.
[0061] The preparation method of the organoboron amine complex can be referred to the relevant literature (HC Brown "A Convenient, Highly Efficient Synthesis of Triorganylboranes via a Modified Organometallic Route", J. Org. Chem. 1986, Vol. 51, 527-432).
[0062] In component A of the two-component asparagine polyurea coating based on interpenetrating polymer network IPN, the coating additives include but are not limited to leveling agents, defoamers, wetting agents, dispersants, antioxidants, anti-aging agents, pigments and fillers, etc. The amount of each addition can be implemented according to the recommendations of the relevant suppliers, or can be used according to the technical experience and habits in the current field of coating technology.
[0063] In the component A of the two-component asparagine polyurea coating based on interpenetrating polymer network IPN, the diluent used includes but is not limited to toluene, xylene, tetrahydrofuran and butyl acetate, etc. The added amount is 0-20% of the total amount of component A, preferably 5-15%.
[0064] The preparation method of the two-component aspartame polyurea coating component A based on the interpenetrating polymer network IPN can be carried out in the following order:
[0065] 1. First, stir and mix the polyurea-modified polyaspartic acid ester, polyaspartic acid ester resin, hydroxyalkyl acrylate and alkyl acrylate in proportion and evenly.
[0066] 2 Add the calculated amount of diacetone acrylamide (DAAM) powder to the above mixture and stir thoroughly until the powder is completely dissolved.
[0067] 3. Weigh the calculated amount of organic boron amine complex initiator, add it into the above mixed solution, and stir evenly.
[0068] 4 According to the needs of the coating formula, add color paste, leveling agent, defoamer, wetting agent, dispersant, antioxidant, anti-aging agent and other additives to the above mixed solution in turn, and then stir and disperse at high speed (2000rpm) for 30 minutes.
[0069] 5. Add an appropriate amount of solvent to adjust the viscosity according to construction requirements, and stir evenly to obtain component A.
[0070] Component B includes: an isocyanate prepolymer and an isophorone diisocyanate monomer, wherein the isocyanate prepolymer is synthesized from a composite isocyanate and a polymeric diol, wherein the composite isocyanate is a mixture of 55-65% (weight percentage) of an HDI trimer and 35-45% (weight percentage) of IPDI, HDI or XDI.
[0071] The polymeric diol can be a polyether diol, including but not limited to polyoxypropylene diol, oxyethylene diol, polytetrahydrofuran diol, etc. Their molecular weight is 1000-3000, preferably 2000. As the polyether diol component, they can be used alone or mixed in any proportion.
[0072] The polymeric diol may also be a polyester diol, including but not limited to polyadipate diol, polycaprolactone diol and polycarbonate diol, with a molecular weight of 1000-3000, preferably 2000. As the polyester diol component, each of them can be used alone or mixed in any proportion.
[0073] When the isocyanate prepolymer is synthesized, the equivalent ratio [NCO] / [OH] of the total NCO of the composite isocyanate to the total OH of the polymerized diol is 3.0-6.0:1, preferably 4.0-5.0:1.
[0074] The synthesis of the isocyanate prepolymer may be performed without adding a catalyst, or a suitable catalyst may be added to accelerate the reaction rate. Suitable catalysts include, but are not limited to, stannous octoate, dibutyltin dilaurate, and zinc neodecanoate. The addition amount is 0.02-0.1% of the total reaction components, preferably 0.05%.
[0075] The isocyanate prepolymer synthesis may be performed without diluent, or with a suitable diluent to adjust the viscosity. Suitable diluents include but are not limited to toluene, xylene, tetrahydrofuran and butyl acetate. The added amount is 5-20% of the total reaction components, preferably 10% or no diluent.
[0076] The synthesis of the isocyanate prepolymer can be carried out according to the commonly used synthesis method in the current polyurethane technology field, such as mixing the isocyanate and the polymerized diol components in proportion, reacting at 60-70° C. for 4-6 hours until the NCO% content reaches the theoretical design value, thereby obtaining the modified curing agent.
[0077] The B component of the two-component aspartame polyurea coating based on interpenetrating polymer network IPN is compounded by isocyanate prepolymer and IPDI monomer, and their weight compounding ratio can be 8:2, preferably 9:1.
[0078] The preparation method of the B component of the two-component aspartame polyurea coating based on the interpenetrating polymer network IPN can be carried out in the following order:
[0079] 1. Mix isocyanate prepolymer and IPDI evenly according to the proportion.
[0080] 2 Add appropriate diluent as needed (the amount added is 0-5% of the total amount of component B) to adjust the viscosity, and stir evenly to obtain component B.
[0081] The patent of the present invention also relates to a method for preparing a two-component asparagine polyurea coating based on an interpenetrating polymer network IPN, wherein the weight mixing ratio of components A and B is in the range of 1:0.5-0.4, and the actual ratio needs to be determined based on the amino and NCO contents in the specific formulas of components A and B, and [NCO] / [N]=1.15.
[0082] The present invention further relates to a method for using a two-component aspartame polyurea coating based on an interpenetrating polymer network (IPN) on a low surface energy synthetic material substrate.
[0083] The low surface energy synthetic materials include but are not limited to polypropylene plastic (PP), polyethylene plastic (EP), ethylene propylene diene monomer rubber (EPDM), etc. In one example of the present invention, EPDM rubber is used as the low surface energy substrate.
[0084] Application of two-component aspartame polyurea coating based on interpenetrating polymer network (IPN) as low surface energy substrate coating.
[0085] According to the present invention, a two-component asparagine polyurea coating based on an interpenetrating polymer network (IPN) is provided, which can be directly coated on low surface energy substrates such as EPDM and PP. The substrate surface only needs simple grinding and cleaning, without the need to use PP water primer and other surface treatment technologies. The specific construction process is as follows:
[0086] 1. Grind the surface of the low surface energy substrate evenly with sandpaper of 800 mesh or above and clean it.
[0087] 2. Mix the A and B components of the two-component asparagine polyurea coating based on the interpenetrating polymer network IPN provided by the present invention in proportion and stir them thoroughly. Then add an appropriate amount of diluent as needed to adjust the spraying viscosity within the range of 18-25 seconds per coating-4 cups.
[0088] 3. Put the mixed paint liquid with adjusted viscosity into the air spray gun tank for spraying. The air pressure and nozzle diameter required by the spray gun should be adjusted according to the common experience and habits in the field of coating technology.
[0089] 4 The wet film after spraying can be cured into a film at room temperature for 12-24 hours, or baked at 80℃ for 30 minutes.
[0090] Beneficial Effects
[0091] 1. The so-called low surface energy materials are hydrophobic and oleophobic, and have very low surface energy, such as polytetrafluoroethylene (PTFE). Adhesives are not easy to wet and adhere to the surface of polytetrafluoroethylene, so polytetrafluoroethylene is also called non-stick coating. Common metals, concrete, etc. have high surface energy, so general coatings are easy to apply. However, for low surface energy materials, the coating needs to have a lower surface tension than the low surface energy material before it can be applied. Therefore, for low surface energy synthetic materials such as EPDM and PP, common coatings have poor adhesion properties. Therefore, in the traditional coating process, a high-adhesion water primer (PP water) must be applied first to increase adhesion.
[0092] In the relevant technologies for solving the adhesion of aspartic polyurea coatings, in addition to the traditional base surface treatment technologies such as primer, surface grinding, and sandblasting, there are also patent reports on the modification of polyaspartic acid resin to improve adhesion. For example: CN106854428 reported that polyaspartic acid resin was modified with hydrogenated epoxy resin to obtain a heavy-duty anti-corrosion coating with good flexibility and strong adhesion to metal substrates. CN116836028 reported that a new type of polyaspartic acid resin was synthesized using (dialkyl acyl) maleic acid monoester, which is said to significantly improve the adhesion to metal substrates. CN20201057243.5 reported a polyaspartic acid resin doubly modified with silicone and epoxy groups, thereby improving the low-temperature flexibility of the flexible anti-corrosion coating and the bonding strength with concrete, metal, and composite materials. The above patent documents all introduce foreign groups into the structure of polyaspartic acid ester resin in order to improve the adhesion of the coating, but the substrates described are mostly metal or concrete materials. The above are all high surface energy materials, but low surface energy synthetic materials such as EPDM and PP are not mentioned. In fact, to date, there are few public literature reports on improving the adhesion of aspartic acid polyurea coatings on low surface energy synthetic materials. In addition to high adhesion, it is also necessary to have resistance to high temperature adhesion, low temperature elasticity, aging resistance, moisture and heat resistance, salt spray resistance, etc. to meet product quality requirements; but in fact, even if the modified polyaspartic acid ester resin meets the high adhesion, other properties may face decline.
[0093] Therefore, synthesizing coatings with high adhesion, high temperature adhesion resistance, low temperature elasticity, aging resistance, moisture and heat resistance, and salt spray resistance for low surface energy synthetic materials is a technical problem that has been difficult to solve in the field of technology.
[0094] The polyurea modified polyaspartic acid ester resin provided by the present invention improves the flexibility and reactivity of the traditional alicyclic polyaspartic acid ester resin, so that it can provide better flexibility and adhesion when used as a surface coating for low surface energy synthetic materials. At the same time, the polyoxypropylene ether segment in the polyurea structure can produce good compatibility with hydroxyalkyl acrylate, thereby increasing the compatibility between the first polymer phase (aliphatic polyurea phase) and the second polymer phase (acrylic copolymer phase) in the interpenetrating polymer network. In this way, the excellent aging resistance, impact resistance and low-temperature flexibility of the polyurea polymer and the excellent bonding performance of the polyacrylate copolymer are maximized.
[0095] The key points of the present invention are: Component A: the first polymer aliphatic polyurea crosslinked product and the second polymer polyacrylate copolymer, Component B: modified curing agent (such as B1), and the above three are indispensable.
[0096] The aliphatic polyurea crosslinked product of the first polymer is synthesized from polyurea-modified polyaspartic acid ester, polyaspartic acid ester and isocyanate curing agent, wherein the polyurea-modified polyaspartic acid ester has a specific structure. The second polymer polyacrylate copolymer is copolymerized from diacetone acrylamide, hydroxyalkyl acrylate, alkyl acrylate and organic boron amine complex initiator. The modified curing agent (B1) is synthesized by components in a specific ratio.
[0097] further:
[0098] The second polymerized polyacrylate copolymer is formed by copolymerization of DAAM as the core monomer, hydroxyalkyl acrylate, alkyl acrylate and organic boron amine complex initiator in the present invention to form an acrylate copolymer with strong adhesion function. Among them: diacetone acrylamide (DAAM) is an N-substituted acrylamide derivative, and the molecule contains three functional groups, namely acylamino, carbonyl and double bond. The amide group and carbonyl group can give the polymer excellent adhesion performance, while the double bond can be copolymerized with other unsaturated monomers. As an initiator of acrylate copolymer, the organic boron amine complex has three advantages: first, because the polymerization initiated by organic borane is a free radical polymerization reaction initiated at the interface, the surface of the low surface energy material can be oxidized at the same time to form an active group. This ensures that the polymer can be well bonded to the low surface energy substrate. Second, the organic boron amine complex can be stably compatible and stored with other components in the A component involved in the present invention, so it can be used as a latent initiator to realize two-component coating packaging. Third, the organic borane complex initiator has the advantage of rapid initiation at low temperature, which can meet the requirements of actual coating construction and coating.
[0099] 2. The present invention uses IPDI curing agent monomer and modified curing agent in combination in component B involved in the present invention, and utilizes the relatively high reactivity of IPDI to enable it to react rapidly with the primary amine component in the organic boron amine complex to form polyurea, thereby improving the decomplexation efficiency of the organic boron amine complex, thereby improving the initiation efficiency of the copolymerization of acrylate monomers by organic borane. BRIEF DESCRIPTION OF THE DRAWINGS
[0100] Figure 1 Infrared spectrum of polyurea prepolymer;
[0101] Figure 2 IR spectrum of 104 type polyurea modified polyaspartic acid ester (PUR-104);
[0102] Figure 3 Infrared spectrum of 105 type polyurea modified polyaspartic acid ester (PUR-105). DETAILED DESCRIPTION
[0103] The information of the main raw materials used in the following examples is shown in Table 1.
[0104] Table 1 Specifications and manufacturers of main raw materials used in the examples
[0105]
[0106] Example 1 Preparation of 104-type urea-modified polyaspartic acid ester (PUR-104)
[0107] The first step is the preparation of polyurea prepolymer
[0108] Add 222.3 g (1 mol) of IPDI to a 2000 ml four-necked flask equipped with a stirrer, a thermometer, a nitrogen conduit, a reflux tube and a constant pressure dropping funnel. Use vacuum to replace the air in the flask with nitrogen and keep the nitrogen flowing. Turn on the stirrer and slowly drop a mixture of 287 g (0.5 mol) of AP-230S and 50 g of butyl acetate through a constant pressure funnel. Use a cold water bath to control the temperature of the reactants in the flask within the range of 30-40°C, and control the dropping time to about 20-30 minutes. After the dropwise addition is completed, keep the reaction at 40°C for 1 hour, then raise the temperature to 60°C for about 2 hours, until the NCO% content reaches 8.3%. Cool to 40°C to obtain a polyurea prepolymer (its infrared spectrum is shown in Figure 1 ),spare.
[0109] Step 2 PUR-104 preparation
[0110] Continue the reaction in the first step. Add 558 g (1 mol) of AP-104 resin and 50 g of butyl acetate to the above reaction flask, stir evenly, then add 0.5 g of stannous octoate, and heat to 60°C with nitrogen to react for about 10 hours until the NCO characteristic peak (2270 -1 PUR-104 with a solid content of 91% (its infrared spectrum is shown in Figure 2 ), the average amino equivalent is 1167.
[0111] Example 2 Preparation of 105-type urea-modified polyaspartic acid ester (PUR-105)
[0112] The first step is the same as the first step of Example 1
[0113] The second step of PUR-105 preparation
[0114] Continue the reaction in the first step. Add 580 g (1 mol) of AP-105 resin and 50 g of butyl acetate to the above reaction flask, stir evenly, then add 0.5 g of stannous octoate, heat to 60°C with nitrogen, and react for about 10 hours until the NCO characteristic peak (2270 -1The solid content of PUR-105 is 91% after cooling.
[0115] (Its infrared spectrum can be seen in Figure 3 ), the average amino equivalent is 1189.
[0116] Example 3 Preparation of curing agent component B1
[0117] (1) Preparation of modified curing agent
[0118] In a 1000ml four-necked flask equipped with a stirrer, a thermometer, a nitrogen conduit, and a reflux tube, add 200g (0.32mol) of HT-00, 108.49g (0.65mol) of HDI, and 26.32g (0.12mol) of IPDI. After stirring and mixing evenly, add 565.19g (0.28mol) of N220 and 4.5g of stannous octoate. Then, use vacuum to replace the air in the flask with nitrogen and keep nitrogen flowing. Raise the temperature to 60°C and react at a constant temperature for 4-6 hours until the NCO% reaches 9.2%.
[0119] After cooling, the modified curing agent is obtained.
[0120] (2) Preparation of curing agent component B1
[0121] The modified curing agent prepared in Example (1) was uniformly mixed with IPDI monomer in a weight ratio of 9:1 to obtain curing agent component B1, with an average NCO% content of 12%.
[0122] Comparative Example 1 Preparation of Curing Agent Component B2
[0123] (1) Preparation of modified curing agent
[0124] In a 1000ml four-necked flask equipped with a stirrer, a thermometer, a nitrogen conduit, and a reflux tube, 83.12g (0.13mol) of HT-00, 152.38g (0.91mol) of HDI, and 41.56g (0.19mol) of IPDI were added, and after stirring and mixing evenly, 622.95g (0.31mol) of N220 and 4.5g of stannous octoate were added, and then the air in the flask was replaced with nitrogen by vacuum and kept flowing with nitrogen, and the temperature was raised to 60°C for constant temperature reaction for 4-6 hours until the NCO% reached 9.2%. After cooling, the modified curing agent was obtained.
[0125] (2) Preparation of curing agent component B2
[0126] The modified curing agent prepared in Example (1) was uniformly mixed with IPDI monomer in a weight ratio of 9:1 to obtain curing agent component B2, with an average NCO% content of 12%.
[0127] Comparative Example 2 Preparation of Curing Agent Component B3
[0128] In a 1000ml four-necked flask equipped with a stirrer, a thermometer, a nitrogen conduit, and a reflux tube, add 200g (0.32mol) of HT-00, 108.49g (0.65mol) of HDI, and 126.32g (0.57mol) of IPDI. After stirring and mixing evenly, add 565.19g (0.28mol) of N220 and 5g of stannous octoate. Then, use vacuum to replace the air in the flask with nitrogen and keep nitrogen flowing. Raise the temperature to 60°C and react at a constant temperature for 4-6 hours until the NCO% reaches 12%.
[0129] After cooling, the modified curing agent B3 is obtained.
[0130] The following Examples 4-7 and Comparative Examples 3-6 are preparation examples of component A (resin component) with different formulations. The composition information of each formulation is shown in Table 2, and the composition of each raw material is measured in parts by weight.
[0131] Table 2 List of formulations of component A with different formulations
[0132]
[0133]
[0134] Example 4A1 Resin Component Preparation
[0135] 1 First, mix the raw material components numbered 1-5 in formula A1 in Table 2 evenly.
[0136] 2 Then add the raw material components numbered 6-9 into the mixed solution in sequence, stir them thoroughly and grind them with a sand mill to a fineness of ≤25μm to obtain a gray color paste containing resin components.
[0137] 3 Then add the raw material components No. 10-18 to the above gray color paste in sequence, stir and disperse at high speed (2000 rpm) for 30 minutes to obtain the resin component of formula A1.
[0138] Example 5A2 Resin component preparation
[0139] According to the formulation of A2 in Table 2, the resin component of formulation A2 was obtained by following the complete process of Example 4.
[0140] Example 6A3 Resin component preparation
[0141] According to the formulation of A3 in Table 2, the resin component of the formulation A3 was obtained by following the complete process of Example 4.
[0142] Example 7A4 Resin component preparation
[0143] According to the formulation of A4 in Table 2, the resin component of the formulation A4 was obtained by following the complete process of Example 4.
[0144] Comparative Example 3A5 Resin Component Preparation
[0145] According to the formulation of A5 in Table 2, the resin component of the formulation A5 was obtained by following the complete process of Example 4.
[0146] Comparative Example 4A6 Resin Component Preparation
[0147] According to the formulation of A6 in Table 2, the resin component of the formulation A6 was obtained by following the complete process of Example 4.
[0148] Comparative Example 5 The resin component of formula A7 was prepared according to the formula A7 in Table 2 and the complete process of Example 4 to obtain the resin component of formula A7.
[0149] The following examples are coating demonstrations of the two-component polyurethane polyurea coating based on the interpenetrating polymer network provided by the present invention on an EPDM substrate, wherein the surface of each 4A-sized EPDM test piece is only lightly polished and cleaned with 800-grit sandpaper, and no PP water primer is applied.
[0150] Table 3 shows the ratio of each coating film composed of resin components A1-A7 and curing agent components B1-B3 and their main performance test results, and each corresponding coating film is represented by F1-F11. Each component is measured by weight.
[0151] Example 8
[0152] 1 Weigh components A1 and B1 according to the formula ratio of F1 in Table 3, and stir and mix thoroughly. Then add appropriate amount of diluent as needed to adjust the viscosity to the range of 18-25 seconds for coating 4 cups.
[0153] 2. Load the mixed paint liquid with adjusted viscosity into the SATA air spray gun with a nozzle diameter of 2.0 mm and an air pressure of 3 kg / cm 2, .
[0154] 3 Spray on the EPDM test piece once to a wet film thickness of 85-90μm.
[0155] 4 The wet film test piece after spraying was left to stand at room temperature for 25-20 minutes, and then placed in an oven at 80°C for 30 minutes to solidify into a film, obtaining test piece F1. After 7 days, the performance was tested.
[0156] Examples 9-18
[0157] Weigh the corresponding A and B components according to the formula ratios of F2-F11 in Table 3, and then operate according to the complete process of Example 8 to obtain test pieces F2-F11.
[0158] Table 3 List of the coating compositions and main properties in Examples 9-18
[0159]
[0160] Note: OK means passed; NG means NO GOOD, i.e. failed.
[0161] As shown in Table 3, A1-A4 in F1-F4 is respectively mixed with B1 and other materials to form a coating, wherein the polyurea modified polyaspartic acid ester resin PUR-104 or PUR-105 in A1-A4 has equivalent effects, and is mixed with AP-105 or AP-104 and DAAM in the proportion shown in the table, and then B1 and other materials are added to synthesize a coating with good performance. It should be pointed out that the key to the present invention is that PUR-104 or PUR-105, AP-105 or AP-104, DAAM, and B1 cooperate with each other to form a coating, which has the best adhesion to the EPDM substrate (grade 0), and at the same time, the high temperature adhesion resistance, low temperature elasticity, aging resistance, moisture resistance, and salt spray resistance meet the product quality requirements.
[0162] A5 in F5 lacks DAAM, and its adhesion to the EPDM substrate is loose, which is unqualified.
[0163] A6 in F6 lacks polyurea-modified polyaspartic acid ester resin PUR-104 or PUR-105, and its adhesion to the EPDM substrate is loose, which is unqualified.
[0164] A7 in F7 lacks AP-104 or AP-105, and its adhesion to the EPDM substrate is loose, which is unqualified.
[0165] F8 uses A1, but uses B2 instead of B1. Its adhesion to EPDM substrate is level 1, which is lower than F1-F4.
[0166] F9 uses A1, but uses B3 instead of B1, and its adhesion to the EPDM substrate is lost and it fails.
[0167] F10 uses A2, but uses B2 instead of B1. Its adhesion to EPDM substrate is level 1, which is lower than F1-F4.
[0168] F11 uses A2, but uses B3 instead of B1, and its adhesion to the EPDM substrate is lost and it fails.
[0169] The above-mentioned F7-F11 is unqualified in terms of high temperature adhesion resistance, low temperature elasticity, aging resistance, moisture and heat resistance or salt spray resistance.
Claims
1. A two-component aspartame polyurea coating based on an interpenetrating polymer network IPN, characterized in that: It includes component A and component B; Component A includes a first polymer which is an amino component of an aliphatic polyurea crosslinker and a second polymer which is a polyacrylate copolymer; The aliphatic polyurea crosslinked product of the first polymer is formed by crosslinking polyurea-modified polyaspartic acid ester, polyaspartic acid ester and isocyanate curing agent; wherein the polyurea-modified polyaspartic acid ester has a structural formula as shown in Formula 1: In Formula 1, R1 is a C1-C6 aliphatic chain alkylene, aliphatic cycloalkylene or a combination thereof; R2 is an alkylene of isophorone diisocyanate, 6-methylene diisocyanate HDI or hydrogenated MDI; R4 is a C10-C30 straight chain alkylene; R3 and R5 are hydrogen or a C1-C8 alkyl or ester group respectively; The polyacrylate copolymer of the second polymer is prepared by copolymerization of diacetone acrylamide, hydroxyalkyl acrylate or alkyl acrylate, and organic boron amine complex; Component B includes: a compound of isocyanate prepolymer and isophorone diisocyanate monomer, which is a curing agent component of the aliphatic polyurea crosslinked product of the first polymer; wherein the isocyanate prepolymer is formed by the reaction of a composite isocyanate and a polymeric diol, wherein the composite isocyanate includes 55-65% by weight of a 6-methylene diisocyanate trimer and 45-35% by weight of isophorone diisocyanate, 6-methylene diisocyanate or xylylene diisocyanate.
2. The two-component aspartame polyurea coating based on interpenetrating polymer network IPN according to claim 1, characterized in that: The first polymer in component A is a polyurea-modified polyaspartic acid ester in an aliphatic polyurea crosslinker prepared by the following steps: In the first step, a bifunctional amino compound and a bifunctional aliphatic isocyanate are condensed to obtain an isocyanate-terminated polyurea prepolymer. In the second step, the isocyanate-terminated polyurea prepolymer obtained in the first step is condensed with a polyaspartic acid ester resin to obtain the polyurea-modified polyaspartic acid ester; In the first step, the difunctional amino compound is a primary amino-terminated amino polyether or a secondary amino-terminated amino polyether; the difunctional aliphatic isocyanate includes isophorone diisocyanate, 6-methylene diisocyanate or xylylene diisocyanate; the equivalent ratio [NCO] / [N] of the aliphatic isocyanate and the difunctional amino compound is 2.05:1; In the second step, the polyaspartic acid ester resin includes NH1420 and NH1520; the equivalent ratio [NCO] / [N] of the isocyanate-terminated polyurea prepolymer and the polyaspartic acid ester resin is 1:1.
05.
3. The two-component aspartame polyurea coating based on interpenetrating polymer network IPN according to claim 1, characterized in that: The hydroxyalkyl acrylate in component A is hydroxyethyl acrylate or hydroxypropyl acrylate; The alkyl acrylate is methyl acrylate or ethyl acrylate; The structural formula of the organic boron amine is shown in Formula 2, In the formula, R1, R2, and R3 are C1-C10 alkyl groups respectively; Am is a dibasic primary amine; and V is 1-4:
1.
4. The two-component aspartame polyurea coating based on interpenetrating polymer network IPN according to claim 3, characterized in that: The organoborane in the organoboron amine is triphenylborane, triethylborane, tri-n-propylborane or tri-n-butylborane.
5. The two-component aspartame polyurea coating based on interpenetrating polymer network IPN according to claim 1, characterized in that: By weight percentage, the usage of polyurea modified polyaspartic acid ester accounts for 20-40% of component A; the usage of polyaspartic acid ester resin accounts for 20-40% of component A; the usage of diacetone acrylamide DAAM accounts for 15-35% of component A, the usage of hydroxyalkyl acrylate accounts for 5-20% of component A; the usage of alkyl acrylate accounts for 0-10% of component A; the boron content in organic borane accounts for 0.05-0.8% of component A.
6. The two-component aspartame polyurea coating based on interpenetrating polymer network IPN according to any one of claims 1 to 5, characterized in that: Component A is prepared by the following steps: in terms of weight percentage, (1) firstly, 20-30% of the total weight of component A of polyurea-modified polyaspartic acid ester, 20-30% of the total weight of component A of polyaspartic acid ester resin, 5-10% of the total weight of component A of hydroxyalkyl acrylate and 0-5% of alkyl acrylate are stirred and mixed uniformly to form a mixed solution; (2) adding 15-20% of the total weight of component A of diacetone acrylamide DAAM powder to the above mixed solution and stirring thoroughly until the powder is completely dissolved; (3) Weighing an organoboronamine complex, wherein the boron content of the complex accounts for 0.1-0.3% of the total weight of component A, adding it to the above mixed solution and stirring evenly; (4) According to the requirements of the coating formulation, color paste, leveling agent, defoamer, wetting agent, dispersant, antioxidant, anti-aging agent and filler are added to the above mixed solution in sequence, and then stirred and dispersed at 2000 rpm for 30 minutes; the leveling agent, defoamer, wetting agent, dispersant, antioxidant and anti-aging agent are used in the amounts recommended by various suppliers, and their total amount does not exceed 3% of the total weight of component A; the amount of color paste and filler accounts for 20-25% of the total weight of component A; (5) Add 5-15% solvent based on the total weight of component A to adjust the viscosity according to construction requirements, and stir evenly to obtain component A.
7. The two-component aspartame polyurea coating based on interpenetrating polymer network (IPN) according to claim 1, characterized in that: Calculated by weight percentage, the isocyanate prepolymer in component B is synthesized from a composite isocyanate and a polymeric diol; wherein the composite isocyanate is a mixture of 55-65% of HDI trimer and 35-45% of isophorone diisocyanate, 6-methylene diisocyanate or xylylene diisocyanate; The equivalent ratio [NCO] / [OH] of the composite isocyanate and the polymeric diol is 3.0-6.0:1; The polymeric diol is a polyether diol or a polyester diol; the polyether diol includes polyoxypropylene diol, oxyethylene diol, polytetrahydrofuran diol, which can be used alone or in any combination of two or more in any proportion; The polyester diol includes polyadipate diol, polycaprolactone diol and polycarbonate diol, which are used alone or in any proportion as a mixture of any two or more thereof; The weight ratio of the isocyanate prepolymer to the isophorone diisocyanate monomer is 8:
2.
8. The two-component aspartame polyurea coating based on interpenetrating polymer network (IPN) according to claim 1, characterized in that: The weight ratio of components A to B is 1:0.5-0.
4.
9. The two-component aspartame polyurea coating based on interpenetrating polymer network (IPN) according to claim 8, characterized in that: Calculated by amino group and NCO content, [NCO] / [N] of components A and B is 1.
15.
10. Use of the two-component aspartame polyurea coating based on interpenetrating polymer network (IPN) according to any one of claims 1 to 9 as a low surface energy substrate coating.
Citation Information
Patent Citations
Aspartate resin of novel structure, polyurea coating as well as preparation method and application of polyurea coating
CN109912442A
Application of benzothioxanthene derivative
CN111635754A
Fertilizer containing reduced glutathione and preparation method thereof
CN116836028A
Preparation of polyaspartate polyurea waterproof coating material
CN101469246A
Photo-curable two-component polyurea waterproofing coating and preparation method therefor
WO2022148082A1
Cited By
Aluminum hub three-in-one polyurea coating as well as preparation method and application thereof