A nano-TiO2 self-cleaning ceramic glaze and its preparation method and application method

By forming a nano-scale rough surface in the ceramic glaze and precipitating TiO2 in situ at high temperature, combined with a crystallizing agent, the problem of complex and high-cost ceramic self-cleaning technology is solved, and the long-term self-cleaning and durability of the ceramic glaze is achieved, which is suitable for Industrial production.

CN117682765BActive Publication Date: 2024-10-29JINGDEZHEN CERAMIC UNIV
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202311276526.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-03
Publication Date
2024-10-29
Estimated Expiration
2043-10-03

AI Technical Summary

Technical Problem

The existing ceramic self-cleaning technology has complex processes and high costs, making it difficult to achieve large-scale production and popularization. Moreover, nano-TiO2 is easily melted by the glaze, resulting in loss of characteristics and short-lived self-cleaning properties.

Method used

The principle of phase separation is used to form a uniformly arranged nano-scale rough surface in the glaze and TiO2 is precipitated in-situ at high temperature. Combined with crystallizing agents such as zinc oxide and aluminum oxide, the nano-TiO2 self-cleaning ceramic glaze is prepared through high-temperature melt to form a super hydrophilic Glaze with strong properties and durability.

Benefits of technology

It achieves the long-term self-cleaning and durability of the ceramic glaze, reduces the preparation cost, simplifies the process, is suitable for industrial production, and improves the anti-fouling and sunlight utilization efficiency of the glaze.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117682765B_ABST
    Figure CN117682765B_ABST
Patent Text Reader

Abstract

The present invention relates to a nano-TiO2 self-cleaning ceramic glaze and a preparation method and application method thereof. The weight percentage composition of the ceramic glaze is: 9-12.1wt% kaolin, 87.9-91wt% phase-separated frit, 1-2wt% zinc oxide, 1-1.5wt% aluminum oxide, and 0-1.5% zirconium oxide. The glaze is prepared by batching, ball milling, sieving, and aging according to the ceramic glaze formula. The glaze is applied to the surface of the body, placed in a kiln in an oxidizing atmosphere after drying and heated to 1180-1210°C, and then the kiln temperature is rapidly cooled to 680-780°C after 1-2h. The nano-TiO2 self-cleaning ceramic glaze is obtained after heat preservation for 0-60 min. The present invention adopts a high-temperature in-situ one-step method to prepare the TiO2 super-hydrophilic self-cleaning ceramic glaze, and the self-cleaning effect can be achieved without a detergent, which not only saves water resources, but also protects the environment, and therefore has a wider practical application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of ceramic technology, in particular to a nano-TiO 2 Self-cleaning ceramic glaze and preparation method and application method thereof. Background Art

[0002] The surface properties of ceramic materials, especially the surface hydrophilicity, are of great significance to the application of ceramics. By utilizing the hydrophilic properties of the surfaces of various materials and changing their surface properties through physical or chemical methods, functions such as automatic cleaning and self-cleaning of liquids can be achieved. The application of self-cleaning technology in industry is mainly to achieve the purpose of self-cleaning by making the metal surface obtain a low contact angle. So far, existing research results at home and abroad have shown that the technologies that can achieve the cleaning effect of ceramic surfaces mainly include: coating super-philic thin films, constructing self-cleaning surface technology with special rough structures, nano-semiconductor photocatalysis technology, and ultra-smooth self-cleaning glaze technology. However, these technical methods have problems such as complex processes, high preparation costs, high requirements for production equipment, and complex equipment. Therefore, it is difficult to achieve large-scale production and promotion and application. This patent uses the phase separation principle to form phase separation droplets of uniform size and close arrangement in the glaze to construct a nano-scale rough surface and a micro-nano structure with an ultra-smooth plane on the macroscopic surface, and uses high temperature to in-situ precipitate TiO with hydrophilic properties. 2 The joint modification enhances the super-hydrophilicity of the glaze, so that the glaze achieves excellent self-cleaning performance. The coating process of the super-hydrophilic self-cleaning glaze in patent ZL202110859978.3 is complex and the production cost is high. The preparation of the super-hydrophilic self-cleaning glaze in patents ZL202010117271.0 and ZL202110709000.9 requires the introduction of metastable phase CaTi 2 O 5 , because it is rare in nature and needs to be artificially synthesized, the cost is relatively high; Application No. 202210568180.8 uses fused quartz to prepare SiO in situ at high temperature 2 / TiO 2 , not just TiO 2 phase of matter. Summary of the invention

[0003] The technical problem to be solved by the present invention is to provide a nano-TiO 2 Self-cleaning ceramic glaze and preparation method and application method thereof.

[0004] The technical solution of the present invention is: a nano-TiO 2The self-cleaning ceramic glaze is characterized in that the weight percentage of the ceramic glaze is: 9-12.1wt% kaolin, 87.9-91wt% phase-separated melt, 1-2wt% zinc oxide, 1-1.5wt% aluminum oxide, and 0-1.5% zirconium oxide.

[0005] The chemical composition of the phase separation melt is: K 2 O 4.81 wt%, Na 2 O 8.56 wt%, MgO 2.85 wt%, CaO12.81 wt%, B 2 O 3 6.82 wt%,Al 2 O 3 8.00 wt%, SiO 2 51.30 wt%, TiO 2 4.30 wt%, P 2 O 5 0.55 wt%; the particle size of the phase-separated melt is less than 300 μm.

[0006] The added zinc oxide, aluminum oxide and zirconium oxide are crystallizing agents.

[0007] The method for preparing the ceramic glaze is characterized in that the glaze is obtained by carrying out the steps of batching, ball milling, screening and aging according to the ceramic glaze formula.

[0008] The ball milling process is to add the raw materials: alumina ball mill: water = 1: 1.8-2: 0.45-0.6 into the ball mill according to the weight percentage of the ceramic glaze formula, and add a diluent to adjust the glaze slurry concentration; the screening process is to pass through a 250-mesh sieve; the aging process takes 6 to 12 hours.

[0009] Among the alumina ball mills, 60wt% are medium ball mills with a diameter of 6-8mm, and 40wt% are small ball mills with a diameter of 2.2-2.5mm.

[0010] The diluent is water glass or fairy water; the specific gravity of the glaze slurry is 1.69-1.73.

[0011] The application method of the glaze obtained by the above preparation method is characterized in that: the glaze is applied to the surface of the body, and after drying, it is placed in a kiln in an oxidizing atmosphere and heated to 1180-1210°C, and then the kiln temperature is rapidly cooled to 680-780°C after 1-2 hours, and the temperature is kept for 0-60 minutes to obtain nano-TiO 2 Self-cleaning ceramic glaze.

[0012] The microstructure of the ceramic glaze surface presents a nano-rough surface constructed by phase-separated droplets with a size of 5 to 10 nm, and a flat and smooth surface with a roughness of 7.25 to 11.3 nm and a wetting angle of 4.8 to 7.2. o The glaze whiteness is 83-85.4%, and the glaze hardness is 719-725Kgf∙mm -2 .

[0013] After the ceramic glaze surface is contaminated by a marker pen, the stains can be removed by adding a small amount of water to restore the clean surface.

[0014] The present invention has the following beneficial effects:

[0015] (1) The present invention precipitates nanocrystalline TiO in situ 2 Exists in the entire glaze layer and surface, overcoming the current nano-TiO 2 When introduced into the glaze, it is easily dissolved by the glaze and loses its characteristics, thereby further improving the hydrophilicity and long-term self-cleaning effectiveness of the ceramic glaze. The self-cleaning property of the obtained glaze can still be maintained after repeated use.

[0016] (2) The present invention prepares nano-TiO by a high-temperature in-situ one-step method 2 Self-cleaning ceramic glaze overcomes the current problems caused by nano-TiO 2 The introduction of powders into glazes can easily lead to agglomeration and inactivation, or the thin film / coating composites have weak mechanical strength and are easily worn. This significantly improves the long-term self-cleaning properties of the glaze, giving it a wider range of practical application prospects.

[0017] (3) Compared with common titanium dioxide super-hydrophilic ceramic glaze, the super-hydrophilic self-cleaning ceramic glaze prepared by the present invention has a simple preparation process. It only controls the formula composition, such as adding a crystallizing agent such as zirconium oxide and aluminum oxide, and uses its strong valence bond characteristics under high-temperature melt to make its high-temperature liquid phase viscosity larger, so that the phase separation droplet size is smaller, which is not conducive to the reaction of alkaline or alkaline earth ions and silicon-oxygen tetrahedron movement and rearrangement, thereby promoting the in-situ precipitation of TiO 2 The crystals are precipitated in the entire glaze layer, which further improves its durability; using its own superhydrophilic properties and the nano-rough surface constructed by the phase separation droplets, its nano-rough surface is more conducive to capturing water; and rutile TiO 2 The crystal phase significantly improves the efficiency of sunlight utilization, making it easier to maintain good super-hydrophilic and anti-fouling properties, which makes it have broad prospects in practical applications.

[0018] (4) The present invention only requires a simple adjustment of the kaolin content and the addition of a high-temperature in-situ crystallization agent to prepare TiO using a larger high-temperature viscosity. 2Super hydrophilic self-cleaning ceramic materials have simple preparation methods, low costs, good wear resistance, are easier to achieve industrial production, comply with green environmental protection concepts, and have potential application prospects in the ceramic materials and glass industries. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 The XRD pattern of the self-cleaning ceramic glaze obtained in Example 1;

[0020] Figure 2 This is a SEM photo of the self-cleaning ceramic glaze obtained in Example 1;

[0021] Figure 3 This is an AFM photo of the self-cleaning ceramic glaze obtained in Example 1;

[0022] Figure 4 This is the UV-visible diffuse reflectance spectrum of the self-cleaning ceramic glaze obtained in Example 1. DETAILED DESCRIPTION

[0023] In order to further explain the present invention and the technical means and effects adopted to achieve the predetermined invention purpose, the present invention is described in detail below in conjunction with preferred embodiments:

[0024] The chemical composition of the phase separation melt is: K 2 O 4.81 wt%, Na 2 O 8.56 wt%, MgO 2.85 wt%, CaO12.81 wt%, B 2 O 3 6.82 wt%,Al 2 O 3 8.00 wt%, SiO 2 51.30 wt%, TiO 2 4.30 wt%, P 2 O 5 0.55 wt%. Example 1

[0025] A nano-TiO 2 The self-cleaning ceramic glaze comprises: 9wt% kaolin, 91wt% phase-separated frit, 1wt% zinc oxide and 1wt% aluminum oxide.

[0026] The particle size of the phase-separated melt is less than 300 μm.

[0027] The added zinc oxide, aluminum oxide and zirconium oxide are crystallizing agents.

[0028] The preparation method of the ceramic glaze comprises the steps of batching, ball milling, sieving and aging according to the ceramic glaze formula to obtain the glaze.

[0029] The ball milling process is to add the raw materials: alumina ball mill: water = 1: 1.8:0.45 into the ball mill according to the weight percentage of the ceramic glaze formula, and add a diluent to adjust the glaze slurry concentration; the screening process is to pass through a 250 mesh sieve; the aging process time is 6 hours.

[0030] Among the alumina ball mills, 60wt% are medium ball mills with a diameter of 6-8mm, and 40wt% are small ball mills with a diameter of 2.2-2.5mm.

[0031] The diluent is water glass or fairy water; the specific gravity of the glaze slurry is 1.69.

[0032] The application method of the glaze obtained by the above preparation method is as follows: the glaze is applied to the surface of the body, and after drying, it is placed in a kiln in an oxidizing atmosphere and heated to 1180°C, and then the kiln temperature is rapidly cooled to 680°C after 1 hour, and the nano-TiO is obtained after keeping the temperature for 0 min. 2 Self-cleaning ceramic glaze.

[0033] The microstructure of the ceramic glaze surface presents a nano-rough surface constructed by phase-separated droplets with a size of 5 to 10 nm, and a flat and smooth surface with a roughness of 8.72 nm and a wetting angle of 4.8. o , glaze whiteness is 83%, glaze hardness is 719Kgf∙mm -2 .

[0034] After the ceramic glaze surface is contaminated by a marker pen, the stains can be removed by adding a small amount of water to restore the clean surface. Example 2

[0035] A nano-TiO 2 The self-cleaning ceramic glaze comprises the following weight percentages: 10wt% kaolin, 90wt% phase-separated frit, 2wt% zinc oxide, 1.5wt% aluminum oxide, and 1% zirconium oxide.

[0036] The particle size of the phase-separated melt is less than 300 μm.

[0037] The added zinc oxide, aluminum oxide and zirconium oxide are crystallizing agents.

[0038] The preparation method of the ceramic glaze comprises the steps of batching, ball milling, sieving and aging according to the ceramic glaze formula to obtain the glaze.

[0039] The ball milling process is to add the raw materials: alumina ball mill: water = 1: 2: 0.45 into the ball mill according to the weight percentage of the ceramic glaze formula, and add a diluent to adjust the glaze slurry concentration; the screening process is to pass through a 250-mesh sieve; the aging process takes 12 hours.

[0040] Among the alumina ball mills, 60wt% are medium ball mills with a diameter of 6-8mm, and 40wt% are small ball mills with a diameter of 2.2-2.5mm.

[0041] The diluent is water glass or fairy water; the specific gravity of the glaze slurry is 1.7.

[0042] The application method of the glaze obtained by the above preparation method is as follows: the glaze is applied to the surface of the body, and after drying, it is placed in a kiln in an oxidizing atmosphere and heated to 1200°C, and then the kiln temperature is rapidly cooled to 690°C after 2 hours, and the temperature is kept for 30 minutes to obtain nano-TiO 2 Self-cleaning ceramic glaze.

[0043] The microstructure of the ceramic glaze surface presents a nano-rough surface constructed by phase-separated droplets with a size of 5 to 10 nm, and a flat and smooth surface with a roughness of 7.25 nm and a wetting angle of 5.0. o , glaze whiteness is 84%, glaze hardness is 720Kgf∙mm -2 .

[0044] After the ceramic glaze surface is contaminated by a marker pen, the stains can be removed by adding a small amount of water to restore the clean surface. Example 3

[0045] A nano-TiO 2 The self-cleaning ceramic glaze comprises the following weight percentages: 11wt% kaolin, 89wt% phase-separated frit, 1.5wt% zinc oxide, 1.2wt% aluminum oxide, and 1.2% zirconium oxide.

[0046] The particle size of the phase-separated melt is less than 300 μm.

[0047] The added zinc oxide, aluminum oxide and zirconium oxide are crystallizing agents.

[0048] The preparation method of the ceramic glaze comprises the steps of batching, ball milling, sieving and aging according to the ceramic glaze formula to obtain the glaze.

[0049] The ball milling process is to add the raw materials: alumina ball mill: water = 1: 2: 0.6 into the ball mill according to the weight percentage of the ceramic glaze formula, and add a diluent to adjust the glaze slurry concentration; the screening process is to pass through a 250-mesh sieve; the aging process takes 10 hours.

[0050] Among the alumina ball mills, 60wt% are medium ball mills with a diameter of 6-8mm, and 40wt% are small ball mills with a diameter of 2.2-2.5mm.

[0051] The diluent is water glass or fairy water; the specific gravity of the glaze slurry is 1.71.

[0052] The application method of the glaze obtained by the above preparation method is as follows: the glaze is applied to the surface of the body, and after drying, it is placed in a kiln in an oxidizing atmosphere and heated to 1210°C, and then the kiln temperature is rapidly cooled to 700°C after 1.5 hours, and the temperature is kept for 60 minutes to obtain nano-TiO 2 Self-cleaning ceramic glaze.

[0053] The microstructure of the ceramic glaze surface presents a nano-rough surface constructed by phase-separated droplets with a size of 5 to 10 nm, and a flat and smooth surface with a roughness of 11.3 nm and a wetting angle of 6.2. o , glaze whiteness is 85%, glaze hardness is 725Kgf∙mm -2 .

[0054] After the ceramic glaze surface is contaminated by a marker pen, the stains can be removed by adding a small amount of water to restore the clean surface. Example 4

[0055] A nano-TiO 2 The self-cleaning ceramic glaze comprises the following weight percentages: 12wt% kaolin, 88wt% phase-separated frit, 1wt% zinc oxide, 1.3wt% aluminum oxide, and 1.3% zirconium oxide.

[0056] The particle size of the phase-separated melt is less than 300 μm.

[0057] The added zinc oxide, aluminum oxide and zirconium oxide are crystallizing agents.

[0058] The preparation method of the ceramic glaze comprises the steps of batching, ball milling, sieving and aging according to the ceramic glaze formula to obtain the glaze.

[0059] The ball milling process is to add the raw materials: alumina ball mill: water = 1: 1.85:0.6 into the ball mill according to the weight percentage of the ceramic glaze formula, and add a diluent to adjust the glaze slurry concentration; the screening process is to pass through a 250-mesh sieve; the aging process takes 9 hours.

[0060] Among the alumina ball mills, 60wt% are medium ball mills with a diameter of 6-8mm, and 40wt% are small ball mills with a diameter of 2.2-2.5mm.

[0061] The diluent is water glass or fairy water; the specific gravity of the glaze slurry is 1.72.

[0062] The application method of the glaze obtained by the above preparation method is as follows: the glaze is applied to the surface of the body, and after drying, it is placed in a kiln in an oxidizing atmosphere and heated to 1210°C, and then the kiln temperature is rapidly cooled to 750°C after 1.5 hours, and the temperature is kept for 30 minutes to obtain nano-TiO 2 Self-cleaning ceramic glaze.

[0063] The microstructure of the ceramic glaze surface presents a nano-rough surface constructed by phase-separated droplets with a size of 5 to 10 nm, and a flat and smooth surface with a roughness of 10.8 nm and a wetting angle of 6.8. o The glaze whiteness is 85.4% and the glaze hardness is 723Kgf∙mm -2 .

[0064] After the ceramic glaze surface is contaminated by a marker pen, the stains can be removed by adding a small amount of water to restore the clean surface. Example 5

[0065] A nano-TiO 2 The self-cleaning ceramic glaze comprises the following weight percentages: 9.4wt% kaolin, 90.6wt% phase-separated frit, 1.8wt% zinc oxide, 1.4wt% aluminum oxide, and 1.5% zirconium oxide.

[0066] The particle size of the phase-separated melt is less than 300 μm.

[0067] The added zinc oxide, aluminum oxide and zirconium oxide are crystallizing agents.

[0068] The preparation method of the ceramic glaze comprises the steps of batching, ball milling, sieving and aging according to the ceramic glaze formula to obtain the glaze.

[0069] The ball milling process is to add the raw materials: alumina ball mill: water = 1: 2: 0.55 into the ball mill according to the weight percentage of the ceramic glaze formula, and add a diluent to adjust the glaze slurry concentration; the screening process is to pass through a 250-mesh sieve; the aging process takes 12 hours.

[0070] Among the alumina ball mills, 60wt% are medium ball mills with a diameter of 6-8mm, and 40wt% are small ball mills with a diameter of 2.2-2.5mm.

[0071] The diluent is water glass or fairy water; the specific gravity of the glaze slurry is 1.73.

[0072] The application method of the glaze obtained by the above preparation method is as follows: the glaze is applied to the surface of the body, and after drying, it is placed in a kiln in an oxidizing atmosphere and heated to 1190°C, and then the kiln temperature is rapidly cooled to 780°C after 1.5 hours, and the nano-TiO is obtained after keeping the temperature for 0 minutes. 2 Self-cleaning ceramic glaze.

[0073] The microstructure of the ceramic glaze surface presents a nano-rough surface constructed by phase-separated droplets with a size of 5 to 10 nm, and a flat and smooth surface with a roughness of 7.95 nm and a wetting angle of 7.0. o , glaze whiteness is 84%, glaze hardness is 719Kgf∙mm-2 .

[0074] After the ceramic glaze surface is contaminated by a marker pen, the stains can be removed by adding a small amount of water to restore the clean surface. Example 6

[0075] A nano-TiO 2 The self-cleaning ceramic glaze comprises the following weight percentages: 10.2wt% kaolin, 89.8wt% phase-separated frit, 1.3wt% zinc oxide, 1wt% aluminum oxide, and 1% zirconium oxide.

[0076] The particle size of the phase-separated melt is less than 300 μm.

[0077] The added zinc oxide, aluminum oxide and zirconium oxide are crystallizing agents.

[0078] The preparation method of the ceramic glaze comprises the steps of batching, ball milling, sieving and aging according to the ceramic glaze formula to obtain the glaze.

[0079] The ball milling process is to add the raw materials: alumina ball mill: water = 1: 2: 0.6 into the ball mill according to the weight percentage of the ceramic glaze formula, and add a diluent to adjust the glaze slurry concentration; the screening process is to pass through a 250 mesh sieve; the aging process time is 12 hours.

[0080] Among the alumina ball mills, 60wt% are medium ball mills with a diameter of 6-8mm, and 40wt% are small ball mills with a diameter of 2.2-2.5mm.

[0081] The diluent is water glass or fairy water; the specific gravity of the glaze slurry is 1.7.

[0082] The application method of the glaze obtained by the above preparation method is as follows: the glaze is applied to the surface of the body, and after drying, it is placed in a kiln in an oxidizing atmosphere and heated to 1190°C, and then the kiln temperature is rapidly cooled to 720°C after 2 hours, and the temperature is kept for 30 minutes to obtain nano-TiO 2 Self-cleaning ceramic glaze.

[0083] The microstructure of the ceramic glaze surface presents a nano-rough surface constructed by phase-separated droplets with a size of 5 to 10 nm, and a flat and smooth surface with a roughness of 11.2 nm and a wetting angle of 7.2. o , glaze whiteness is 83%, glaze hardness is 725Kgf∙mm -2 .

[0084] After the ceramic glaze surface is contaminated by a marker pen, the stains can be removed by adding a small amount of water to restore the clean surface.

Claims

1. A nano-TiO2 self-cleaning ceramic glaze, characterized by: The ceramic glaze is composed of 9-12.1wt% kaolin, 87.9-91wt% phase-separated melt, 1-2wt% zinc oxide, 1-1.5wt% aluminum oxide, and 0-1.5% zirconium oxide according to the ceramic glaze formula, and the glaze is obtained by mixing, ball milling, sieving, and aging. The glaze is applied on the surface of the body, dried, placed in a kiln in an oxidizing atmosphere and heated to 1180-1210°C, then the kiln temperature is rapidly cooled to 680-780°C after 1-2 hours, and kept warm for 0-60 minutes to obtain a nano-TiO2 self-cleaning ceramic glaze; The chemical composition of the phase separation melt is: K2O 4.81 wt%, Na2O 8.56 wt%, MgO 2.85 wt%, CaO 12.81 wt%, B2O3 6.82 wt%, Al2O3 8.00 wt%, SiO2 51.30 wt%, TiO2 4.30 wt%, P2O5 0.55 wt%; the particle size of the phase-separated melt is less than 300 μm.

2. The ceramic glaze according to claim 1, characterized in that: The added zinc oxide, aluminum oxide and zirconium oxide are crystallizing agents.

3. The ceramic glaze according to claim 1, characterized in that: The ball milling process is to add the raw materials: alumina ball mill: water = 1: 1.8-2: 0.45-0.6 into the ball mill according to the weight percentage of the ceramic glaze formula, and add a diluent to adjust the glaze slurry concentration; the screening process is to pass through a 250-mesh sieve; the aging process takes 6 to 12 hours.

4. The ceramic glaze according to claim 3, characterized in that: Among the alumina ball mills, 60wt% are medium ball mills with a diameter of 6-8mm, and 40wt% are small ball mills with a diameter of 2.2-2.5mm.

5. The ceramic glaze according to claim 3, characterized in that: The diluent is water glass or fairy water; the specific gravity of the glaze slurry is 1.69-1.

73.

6. The ceramic glaze according to claim 1, characterized in that: The microstructure of the ceramic glaze surface presents a nano-rough surface constructed by phase-separated droplets with a size of 5 to 10 nm, and a flat and smooth surface with a roughness of 7.25 to 11.3 nm and a wetting angle of 4.8 to 7.

2. o The glaze whiteness is 83-85.4%, and the glaze hardness is 719-725Kgf∙mm -2 .

Citation Information

Patent Citations

  • A hydrophilic ceramic glaze prepared using CaTi2O5 surface modifier, and its preparation and application methods.

    CN111348832B

  • Self-cleaning split-phase milky white glaze and preparation method thereof

    CN113603363A

  • Coating for improving anatase TiO2 super-hydrophilic self-cleaning ceramic glaze and application method thereof

    CN113831017A

  • A superhydrophilic self-cleaning ceramic glaze with visible light response, its preparation and application methods

    CN115072999B