LED display panel and its preparation method and maintenance method

By using thermoset anti-glare coatings of epoxy resin and AG anti-glare potion on the package layer of the LED display panel, the problems of low surface consistency and high cost are solved, and a high-quality LED display panel is achieved, and in Maintain high quality after repair.

CN117747736BActive Publication Date: 2024-11-12LEDMAN OPTOELECTRONICS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311870039.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-29
Publication Date
2024-11-12
Estimated Expiration
2043-12-29

AI Technical Summary

Technical Problem

The surface consistency of the existing LED display panels is low and costly, and the inability to restore the pattern during maintenance leads to a reduced quality.

Method used

Epoxy resin is used as the encapsulation layer material, and a glossy surface layer and a thermoset anti-glare coating are provided on its outer surface. The coating material is AG anti-glare potion. A consistent surface is formed through molding and heating curing technology, reducing costs and improving quality. .

Benefits of technology

The packaging layer has high surface consistency, reduced costs, and maintained high quality after repair, avoiding the problems of different appearances in the repair area and inconsistent light output effects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117747736B_ABST
    Figure CN117747736B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of LED display technology, solves the shortcomings of low consistency and high cost of the surface of the packaging layer of the existing LED display panel, and provides an LED display panel, a preparation method thereof, and a maintenance method thereof. The LED display panel includes: a plurality of LED chips; a circuit board, at least one mounting surface of which is provided with an LED chip; a packaging layer, which is provided on the mounting surface and covers the LED chip; a glossy surface layer, which is provided on the outer surface of the packaging layer; and a thermosetting anti-glare coating, which is provided on the glossy surface layer. The LED display panel of the present invention, its preparation method, and maintenance method have the advantages of ensuring high consistency of the surface of the packaging layer of the LED display panel and reducing costs.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of LED display technology, and in particular to an LED display panel and a preparation method and a maintenance method thereof. Background Art

[0002] LED display is a flat panel display, composed of LED display panels, used to display text, images, videos and other information. LED display integrates microelectronics technology, computer technology and information processing, and has the advantages of bright colors, wide dynamic range, high brightness, long life, stable and reliable operation. LED display is widely used in commercial media, cultural performance market, sports stadiums, information dissemination, news release, securities trading, etc., and can meet the needs of different environments.

[0003] In the field of existing LED display panel packaging technology, COB (Chip On Board) packaging technology has the advantages of high brightness, high protection and efficient heat dissipation.

[0004] As for packaging technology, epoxy resin packaging materials are currently mainly used as packaging layers. Epoxy resin has the advantages of high hardness (Shore hardness D>80), a wide variety of mature curing agents and low prices. In the epoxy resin molding process, it is necessary to arrange a patterned release film on the epoxy resin surface, and transfer the pattern of the patterned release film to the epoxy resin surface through hot pressing molding by a molding machine. However, the imprinting of the patterned release film is easily affected by pressure, consistency of the pattern of the patterned release film and other factors, making it difficult to achieve complete consistency, resulting in insufficient consistency on the surface of the packaging layer. In addition, the cost of the patterned release film is high, thereby increasing the cost of the LED display panel and the LED display screen equipped with the LED display panel. In addition, since LED display panels and LED screens inevitably need maintenance to extend their use time and thus save on usage costs, during maintenance, the repair area of ​​the LED display panel cannot be restored by re-embossing, resulting in not only a relatively abrupt surface structure in the repair area, but also a large difference in the light emission effect of the repair area compared to that of areas outside the repair area, which has an adverse effect on light consistency, thereby causing a serious reduction in quality after repair.

[0005] Therefore, there is an urgent need to provide an LED display panel, a preparation method and a maintenance method thereof that can ensure high consistency of the surface of the encapsulation layer and reduce costs. Summary of the invention

[0006] The present invention aims at the shortcomings of the prior art, such as low surface consistency and high cost of the packaging layer of the existing LED display panel, and to achieve one purpose of the present invention, provides an LED display panel, including: a plurality of LED chips; a circuit board, at least one mounting surface of which is provided with the LED chip; a packaging layer, which is provided on the mounting surface and covers the LED chip; a glossy surface layer, which is provided on the outer surface of the packaging layer; and a thermosetting anti-glare coating, which is provided on the glossy surface layer.

[0007] Furthermore, the material of the encapsulation layer is epoxy resin, and the material of the thermosetting anti-glare coating is AG anti-glare solution, which includes, by weight: SiO 2 Nanoparticles: 7-12 parts, alcohol solvent: 76-86 parts, silicone additive: 7-12 parts.

[0008] Furthermore, the thermosetting anti-glare coating is set to: unit weight: 80-120 g / m 2 , thickness: 5-7μm, 60° gloss ≤10%.

[0009] To achieve another object of the present invention, a method for preparing an LED display panel is provided, which is applied to any of the above LED display panels, and includes the following steps: S11: providing a circuit board having a plurality of LED chips on at least one mounting surface thereof; S12: molding a packaging layer on the mounting surface to cover the LED chips; S13: molding the packaging layer with a smooth release film to obtain a smooth surface layer, and heating and curing the smooth surface layer; S14: performing a first heating on the smooth surface layer, and then performing a plasma treatment; S15: coating a thermosetting anti-glare coating on the smooth surface layer; S16: performing a second heating on the thermosetting anti-glare coating.

[0010] Furthermore, the first heating in step S14 includes preheating the polished surface layer at 50-100° C. for 1-4 hours.

[0011] Furthermore, the second heating in step S16 includes heating the thermosetting anti-glare coating at 160-180° C. for 20-30 min.

[0012] To achieve another object of the present invention, a maintenance method for an LED display panel is provided, which is applied to any of the above LED display panels, wherein there is at least one faulty LED chip that cannot work normally among multiple LED chips, and the maintenance method comprises: S21: digging a hole at the position where the faulty LED chip is located to obtain an opening, taking out the exposed faulty LED chip and replacing it with a new LED chip; S22: filling the opening with a packaging layer, and curing the packaging layer; S23: grinding an adjacent area of ​​the opening to remove the thermosetting anti-glare coating thereon, and grinding the packaging layer flat so that the surfaces of the packaging layer and the adjacent area from which the thermosetting anti-glare coating has been removed are flush; S24: plasma treating the packaging layer and the adjacent area from which the thermosetting anti-glare coating has been removed; S25: coating the packaging layer and the adjacent area that have been plasma treated with a thermosetting anti-glare coating; S26: heating and curing the thermosetting anti-glare coating.

[0013] Furthermore, the curing treatment in step S22 includes baking for dehumidification and preheating at 50-100° C. for 1-4 hours; and the heating curing in step S26 includes heating at 160-180° C. for 20-30 minutes.

[0014] Furthermore, the encapsulation layer in step S22 is an epoxy resin layer, and the material of the thermosetting anti-glare coating in step S25 is an AG anti-glare solution, which includes, by weight: SiO 2 Nanoparticles: 7-12 parts, alcohol solvent: 76-86 parts, silicone additive: 7-12 parts.

[0015] Furthermore, in step S21, a hole is dug by laser drilling, and the adjacent area is set as a circular area with a radius of 0.5 to 2 mm and a center of the faulty LED chip. The thermosetting anti-glare coating is sprayed, and the spraying of the thermosetting anti-glare coating is controlled to meet the following conditions: unit weight: 80 to 120 g / m 2 , thickness: 5-7μm, 60° gloss ≤10%.

[0016] The beneficial effects of the present invention are:

[0017] The LED display panel and its preparation method and maintenance method of the present invention provide a smooth surface layer and a thermosetting anti-glare coating on the outer surface of the packaging layer on the LED display panel, thereby obtaining a highly consistent surface layer on the surface of the packaging layer and reducing costs. Moreover, even if the LED display panel needs to replace its faulty LED chip later, there is no need to restore the pattern by re-embossing the maintenance area, thereby ensuring that the LED display panel has high quality even after maintenance. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] In order to more clearly illustrate the technical solution of the embodiment of the present invention, the drawings required for use in the embodiment of the present invention will be briefly introduced below. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work, and these are all within the protection scope of the present invention.

[0019] Figure 1 A schematic diagram of the layer structure of an LED display panel provided by an embodiment of the present invention;

[0020] Figure 2 A schematic flow chart of a method for preparing an LED display panel provided in an embodiment of the invention;

[0021] Figure 3 A schematic flow chart of a method for repairing an LED display panel provided by an embodiment of the invention;

[0022] Description of reference numerals:

[0023] 1-circuit board; 2-packaging layer; 3-thermosetting anti-glare coating. DETAILED DESCRIPTION

[0024] In order to make the purpose, technical solution and advantages of the embodiment of the present invention clearer, the technical solution in the embodiment of the present invention will be clearly and completely described in conjunction with the drawings in the embodiment of the present invention. It should be noted that, in this article, relational terms such as first and second are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply that there is any such actual relationship or order between these entities or operations. In the description of the present invention, it should be understood that the orientation or position relationship indicated by the terms "center", "upper", "lower", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", etc. is based on the orientation or position relationship shown in the drawings, which is only for the convenience of describing the present application and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation of the present invention. Moreover, the term "include", "comprise" or any other variant thereof is intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such a process, method, article or device. In the absence of further restrictions, the elements defined by the phrase "comprising..." do not exclude the existence of other identical elements in the process, method, article or device comprising the elements. If there is no conflict, the embodiments of the present invention and the various features in the embodiments can be combined with each other and are all within the protection scope of the present invention.

[0025] refer to Figure 1 As an object of the present invention, an LED display panel is provided, wherein the LED display panel is preferably a Micro-LED display panel or a Mini-LED display panel. The LED display panel comprises a plurality of LED chips, a circuit board 1, a packaging layer 2, a glossy surface layer and a thermosetting anti-glare coating 3, wherein an LED chip is arranged on at least one mounting surface of the circuit board 1, the packaging layer 2 is arranged on the mounting surface and covers the LED chip, the glossy surface layer is arranged on the outer surface of the packaging layer 2, i.e., a surface away from and facing away from the LED chip, the glossy surface layer can be obtained by molding the packaging layer 2 with a glossy release film (for details, please refer to the description of the preparation method of the LED display panel below), and the thermosetting anti-glare coating 3 is arranged on the glossy surface layer. Preferably, in order to make the combination of the packaging layer 2 and the circuit board 1 and the combination of the thermosetting anti-glare coating 3 and the glossy surface layer meet the combination requirements, the surface water drop angle is reduced by plasma treatment, thereby improving the wettability. In addition, if Figure 1 As shown, the surface of the thermosetting anti-glare coating 3 preferably has a regular partial top spherical surface, so the thermosetting anti-glare coating 3 can change the light direction of the LED chip by, for example, diffuse reflection, thereby achieving an anti-glare effect. In this way, since the outer surface of the encapsulation layer 2 is provided with a smooth surface layer and a thermosetting anti-glare coating 3, the adverse effects of the prior art using a patterned release film, such as susceptibility to pressure and poor pattern consistency of the patterned release film, are avoided, thereby obtaining a highly consistent surface layer on the surface of the encapsulation layer 2, and the cost is lower than that of using a patterned release film. In addition, for the subsequent maintenance of the LED display panel, there is no need to restore the pattern by re-embossing the maintenance area, thereby ensuring that the LED display panel has a high quality even after maintenance.

[0026] Specifically, the material of the encapsulation layer 2 is epoxy resin, which has the advantages of high hardness (Shore hardness D>80), a variety of mature curing agents and low price. The material of the thermosetting anti-glare coating 3 is AG anti-glare solution, which includes, by weight: SiO 2 Nanoparticles: 7-12 parts, alcohol solvents: 76-86 parts, siloxane additives: 7-12 parts. Referring to Table 1 below, the AG anti-glare solution has a lower glossiness, can reduce the specular reflection of the surface of the encapsulation layer 2, and has a strong adhesion to the encapsulation layer 2, thereby having a strong scratch resistance. Moreover, the thermosetting anti-glare coating 3 can obtain an AG texture from the AG anti-glare solution, and the AG texture can achieve diffuse reflection of light, thereby achieving an anti-glare effect.

[0027] Specifically, according to repeated experimental tests by the applicant, it is determined that the relevant parameters of the thermosetting anti-glare coating 3 made of AG anti-glare solution are set to the following specific numerical ranges: Unit weight: 80-120 g / m 2 , thickness: 5-7μm, 60° glossiness ≤10%. And referring to the following Table 1, when the thermosetting anti-glare coating 3 meets the specific numerical range of the above parameters, the LED display panel will not have flash points and can meet the quality requirements for shipment.

[0028] As another object of the present invention, in conjunction with reference Figure 2 The present invention also provides a method for preparing an LED display panel. In the absence of conflict, the preparation method described below is applied to the above LED display panel embodiments, and the relevant repeated contents are not repeated here. The preparation method comprises the following steps:

[0029] S11: providing a circuit board 1 having a plurality of LED chips disposed on at least one mounting surface thereof, and the circuit board 1 and the LED chips thereon may be prepared by a SMT process;

[0030] S12: Molding a packaging layer 2 such as epoxy resin on the mounting surface to cover the LED chip. Molding means that the packaging layer 2 is directly laminated and coated with glue;

[0031] S13: using a smooth release film to mold the encapsulation layer 2 to obtain a smooth surface layer, and heating and curing the smooth surface layer. The heating and curing may be pre-curing at 110° C. for 3 minutes and post-curing at 150° C. for 4 hours. In addition, corresponding matching and adjustment are performed according to different types of epoxy resin used in the encapsulation layer 2;

[0032] S14: first heating the smooth surface layer and then performing plasma treatment, so as to fully activate the surface groups of the smooth surface layer;

[0033] S15: coating a thermosetting anti-glare coating 3 made of, for example, AG anti-glare solution on the glossy surface;

[0034] S16: performing a second heating on the thermosetting anti-glare coating 3 .

[0035] The LED display panel of the present invention can be obtained by the method for preparing the LED display panel of the present invention, so that the LED display panel directly obtained by the preparation method also has the above-mentioned beneficial technical effects. In addition, the preparation method also has the advantages of strong operability and compact steps and processes.

[0036] Preferably, the first heating in step S14 includes preheating the glossy surface layer at 50-100° C. for 1-4 hours, so that the purpose of dehumidification is achieved by baking the glossy surface layer. Dehumidification can remove water vapor, which is beneficial to the reliable bonding of the glossy surface layer and the thermosetting anti-glare coating.

[0037] Preferably, the second heating in step S16 includes heating the thermosetting anti-glare coating 3 at 160-180°C for 20-30 minutes, so as to achieve the purpose of making the thermosetting anti-glare coating 3 have better consistency. Referring to the following Table 1, in the experimental tests divided into 7 times, and in combination with the above-mentioned numerical ranges set for the relevant parameters of the thermosetting anti-glare coating 3 using the AG anti-glare solution: Unit weight: 80-120 g / m 2 , thickness: 5-7μm, 60° gloss ≤10%. In test number 1, since its coating amount is 60g / m 2 That is less than 80g / m 2 , its glossiness is 20.5, which exceeds 10%, and thus does not meet the shipment requirements. In test number 2, the curing temperature is 130°C, which is not within the range of 160-180°C, and its adhesion is 2B, which does not meet the requirement of qualified adhesion of 5B or above, and thus does not meet the shipment requirements. In test number 3, the curing time is 15min, which is lower than the lower limit of 20-30min, and its 60° glossiness is 10.1%, which exceeds 10%, and its adhesion is 3B, which does not meet the requirement of qualified adhesion: 5B or above, and thus does not meet the shipment requirements. In test number 6, the curing temperature is 150°C, which is not within the range of 160-180°C, and its 60° glossiness is 11.2, which exceeds 10%, and thus does not meet the shipment requirements. In test number 7, since its coating amount is 150g / m 2 That is greater than 120g / m 2 And the curing temperature is 150°C, which is not within the range of 160-180°C, so that its thickness is 8μm, which is not within the range of 5-7μm, and thus does not meet the shipment requirements. If the shipment quality requirements cannot be met in the above tests, the LED display panel will have more obvious flash points. For test numbers 4 and 5 in Table 1, since the coating amount, curing temperature and thickness all meet the above-set numerical ranges, they can meet the shipment requirements. In addition, for test number 5, although the curing time is 50min, which is higher than the upper limit of 20-30min, it can meet the curing effect, but the curing efficiency is low. Therefore, the above curing time: 20-30min is the preferred time range and cannot be lower than the lower limit of 20min, but higher than 30min only affects the curing efficiency but not the curing effect.

[0038] In summary, in order to ensure the high quality of the thermosetting anti-glare coating 3 made of AG anti-glare solution, the following preparation conditions need to be met: coating amount: 80-120 g / m 2 , curing temperature: 160~180℃, curing time: 20~30min, thickness: 5-7μm.

[0039] Table 1: Comparison of different test conditions for thermosetting anti-glare coatings

[0040]

[0041]

[0042] As another object of the present invention, in conjunction with reference Figure 3 The present invention also provides a method for repairing an LED display panel. In the absence of conflicts, the repair method described below is applied to the LED display panels of the above LED display panel embodiments and the LED display panels prepared by the above preparation method embodiments. The repeated contents are not repeated here. Since it is difficult to avoid the LED display panel needing repair due to a faulty LED chip, when there is at least one faulty LED chip that cannot work properly among the multiple LED chips, the repair method includes the following steps:

[0043] S21: digging a hole at the location of the faulty LED chip to obtain an opening, taking out the exposed faulty LED chip and replacing it with a new LED chip;

[0044] Specifically, an opening is obtained by digging out the original packaging layer 2 and the original thermosetting anti-glare coating 3 covering the packaged faulty LED chip. The specific opening range is the point spacing size corresponding to the position to be repaired. For example, assuming the point spacing is P1.2, the opening range expands by 1.2mm, that is, the outer hole diameter value is 2.4mm. In this way, the opening range will not affect the adjacent normal LED chips.

[0045] In addition, if multiple adjacent LED chips are faulty and multiple faulty LED chips occupying a large area need to be repaired, sulfuric acid is first used to remove a large area of ​​the original encapsulation layer 2 and the original thermosetting anti-glare coating 3 in the corresponding area above the multiple faulty LED chips. The large area can be set as a circular hole shape and expand outward by one dot spacing as mentioned above, and then rinsed with water, and then laser finishing is used to remove the remaining encapsulation layer 2 and thermosetting anti-glare coating 3. Finally, the exposed multiple faulty LED chips are taken out and replaced with multiple new LED chips. This can improve the repair efficiency and quality of multiple faulty LED chips, and after implementing the subsequent steps, a thermosetting anti-glare coating 3 with good consistency can be obtained on the outer surface of the opening area and the adjacent area of ​​the multiple faulty LED chips.

[0046] S22: Filling the opening with the encapsulation layer 2, and curing the encapsulation layer 2. It is known that the newly filled encapsulation layer 2 is heated and cured as a new encapsulation layer like the original encapsulation layer. In addition, the following encapsulation layers can be understood as the new encapsulation layer.

[0047] S23: grinding the adjacent area of ​​the opening to remove the thermosetting anti-glare coating 3 thereon, and grinding the encapsulation layer 2 flat, that is, grinding away the redundant portion of the encapsulation layer 2, especially the portion that is higher than the surface of the adjacent area, so that the surface of the encapsulation layer 2 and the adjacent area where the thermosetting anti-glare coating 3 is removed are flush;

[0048] S24: performing plasma treatment on the encapsulation layer 2 and the adjacent area from which the thermosetting anti-glare coating 3 has been removed, so as to fully activate the surface groups of the encapsulation layer 2 and the adjacent area;

[0049] S25: coating the encapsulation layer 2 and the adjacent area after the plasma treatment with a thermosetting anti-glare coating 3, wherein the thermosetting anti-glare coating 3 can diffusely reflect light, thereby achieving an anti-glare effect;

[0050] S26: Heat and cure the thermosetting anti-glare coating 3, so as to achieve the purpose of improving the consistency of the thermosetting anti-glare coating 3.

[0051] In summary, the repair method of the LED display panel of the present invention adopts a hole-digging method to replace the faulty LED chip with a new LED chip, and then fills the encapsulation layer 2 for encapsulating the new LED chip, and adopts a grinding method to grind the encapsulation layer 2 and the thermosetting anti-glare coating 3 of the adjacent area. Since the LED chip itself is at the micron level, it is only necessary to dig a hole at a very small size where the faulty LED chip is located and then fill the encapsulation layer 2, and then grind the encapsulation layer 2 and its adjacent area. On the basis of not needing to use a smooth release film, the encapsulation layer 2 and its adjacent area can obtain a smooth surface layer and coat the thermosetting anti-glare coating 3 thereon, which can not only save maintenance time, but also the encapsulation layer 2 and its adjacent area only need to be coated with the thermosetting anti-glare coating 3 without setting the pattern obtained by the patterned release film in the prior art, and there is no need to maintain the consistency of the pattern, so that the surface structures of the two are highly consistent and there is no relatively abrupt situation, so that there is basically no difference in appearance between the repaired areas on the LED display panel, and there is no difference in the light output effects of the two, ensuring that the quality after repair is still very high, thereby extending the service life of the LED display panel and saving the use cost.

[0052] Preferably, the curing treatment in step S22 includes baking and dehumidification and preheating at 50-100°C for 1-4h; thus, this can achieve the purpose of baking and dehumidifying the encapsulation layer 2. The heating curing in step S26 includes heating at 130-170°C for 10-30min. Therefore, this can achieve the purpose of making the thermosetting anti-glare coating 3 have better consistency.

[0053] Specifically, as described above, the encapsulation layer 2 in step S22 is an epoxy resin layer, and the material of the thermosetting anti-glare coating 3 in step S25 is an AG anti-glare solution, which includes, by weight: SiO 2 Nanoparticles: 7-12 parts, alcohol solvents: 76-86 parts, siloxane additives: 7-12 parts. Referring to Table 1 above, by coating the newly filled encapsulation layer 2 with a thermosetting anti-glare coating 3 made of AG anti-glare solution, all the thermosetting anti-glare coatings 3 of the LED display panel are kept consistent, achieving the same diffuse reflectivity of light, thereby achieving a good anti-glare effect.

[0054] Preferably, laser drilling is used to dig holes in step S21. Since the LED chip is at the micron level, laser drilling has sufficient accuracy to accurately remove the packaging layer 2 above the faulty LED chip. Laser drilling can form a circular hole, so the regular shape of the opening is convenient for taking and placing the faulty LED chip and the new LED chip and filling the packaging layer 2. The adjacent area is set as a circular area with a radius of 0.5 to 2 mm with the faulty LED chip as the center. For micron-level LED chips, compared with a circular area with a radius of millimeters, the volume of the faulty LED chip is basically negligible, so it can be regarded as a point as the center of the circle. The polishing method can be laser burning polishing. The coating of the thermosetting anti-glare coating 3 is sprayed. The coating can be dipped, sprayed, slit coated, scraped, etc. The spraying method is preferably used during maintenance, which can effectively reduce the use of the thermosetting anti-glare coating 3 and is conducive to cost saving. The spraying of the thermosetting anti-glare coating 3 is controlled to meet the following requirements: Unit weight: 60 to 120 g / m 2 , thickness: 3-5μm, 60° glossiness: ≤10%. This will prevent flash points from appearing in the repair area of ​​the LED display panel, and ensure that the repaired LED display panel meets the quality requirements for shipment.

[0055] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. These modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention. Any modifications, equivalent replacements and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. An LED display panel, characterized in that: include: Multiple LED chips; A circuit board, at least one mounting surface of which is provided with the LED chip; A packaging layer, which is disposed on the mounting surface and covers the LED chip; A smooth surface layer, which is arranged on the outer surface of the encapsulation layer, and the smooth surface layer is configured to be plasma treated; A thermosetting anti-glare coating disposed on the glossy surface layer; The material of the encapsulation layer is epoxy resin, the material of the thermosetting anti-glare coating is AG anti-glare solution, and the AG anti-glare solution includes, by weight: 7 to 12 parts of SiO2 nanoparticles of different particle sizes, 76 to 86 parts of alcohol solvents, and 7 to 12 parts of siloxane additives; The thermosetting anti-glare coating is set to: unit weight: 80-120 g / m 2 , thickness: 5-7μm, 60° gloss ≤10%.

2. A method for preparing an LED display panel, applied to the LED display panel as claimed in claim 1, characterized in that: The steps include: S11: providing a circuit board having a plurality of LED chips disposed on at least one mounting surface thereof; S12: molding a packaging layer on the mounting surface to cover the LED chip; S13: using a smooth release film to mold the encapsulation layer to obtain a smooth surface layer, and heating and curing the smooth surface layer; S14: first heating the smooth surface layer, and then performing plasma treatment; S15: coating a thermosetting anti-glare coating on the glossy surface layer; S16: performing a second heating on the thermosetting anti-glare coating.

3. The method for preparing an LED display panel according to claim 2, characterized in that: The first heating in step S14 includes preheating the smooth surface layer at 50-100° C. for 1-4 hours.

4. The method for preparing an LED display panel according to claim 2, characterized in that: The second heating in the step S16 includes heating the thermosetting anti-glare coating at 160-180° C. for 20-30 minutes.

5. A method for repairing an LED display panel, applied to the LED display panel as claimed in claim 1, characterized in that: There is at least one faulty LED chip that cannot work normally among the plurality of LED chips, and the repair method comprises: S21: digging a hole at the location of the faulty LED chip to obtain an opening, taking out the exposed faulty LED chip and replacing it with a new LED chip; S22: Filling the opening with a packaging layer, and curing the packaging layer; S23: grinding the adjacent area of ​​the opening to remove the thermosetting anti-glare coating thereon, and grinding the encapsulation layer to make the surfaces of the encapsulation layer and the adjacent area where the thermosetting anti-glare coating has been removed flush; S24: performing plasma treatment on the encapsulation layer and the adjacent area from which the thermosetting anti-glare coating has been removed; S25: coating the plasma-treated encapsulation layer and the adjacent region with a thermosetting anti-glare coating; S26: heating and curing the thermosetting anti-glare coating.

6. The LED display panel maintenance method according to claim 5, characterized in that: The curing treatment in step S22 includes baking for dehumidification and preheating at 50-100° C. for 1-4 hours; the heating curing in step S26 includes heating at 160-180° C. for 20-30 minutes.

7. The LED display panel maintenance method according to claim 6, characterized in that: In the step S21, a hole is dug by laser drilling, the adjacent area is set as a circular area with the faulty LED chip as the center and a radius of 0.5 to 2 mm, the thermosetting anti-glare coating is applied by spraying, and the spraying of the thermosetting anti-glare coating is controlled to meet the following conditions: unit weight: 80 to 120 g / m 2 , thickness: 5-7μm, 60° gloss ≤10%.