A thick film long-term anticorrosion material under low surface treatment conditions

By spraying thick film long-term anticorrosion material formulas with modified epoxy resin and other components on metal substrates, the problem of pre-cleaning of existing coatings is solved, and high adhesion and corrosion resistance under low surface treatment conditions are achieved. Suitable for equipment anti-corrosion in complex environments.

CN117757332BActive Publication Date: 2024-11-12CNOOC ENERGY DEV EQUIP TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311770777.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-21
Publication Date
2024-11-12
Estimated Expiration
2043-12-21

AI Technical Summary

Technical Problem

Existing epoxy anticorrosion coatings require pre-cleaning of the substrate surface to ensure good adhesion, limiting its flexibility in field applications.

Method used

The thick film long-acting anticorrosion material formula is adopted under low surface treatment conditions, including modified epoxy resin, hydrophobic vapor phase silica, inorganic pigment, rutile titanium dioxide, propylene glycol monomethyl ether and ultrafine zinc powder, by spraying on The surface of the metal substrate is cured to form a coating with high adhesion and corrosion resistance.

Benefits of technology

Without the need for deep cleaning of the substrate surface, the coating can firmly adhere to the metal surface, providing long-term antioxidant protection, and is suitable for corrosion protection in marine, marine engineering equipment and field pipeline equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GDA0005027169440000061
    Figure GDA0005027169440000061
  • Figure GDA0005027169440000071
    Figure GDA0005027169440000071
  • Figure GDA0005027169440000072
    Figure GDA0005027169440000072
Patent Text Reader

Abstract

The invention discloses a thick film long-term anticorrosion material under low surface treatment conditions in the field of anticorrosion coatings, which is formed by mixing component A and component B, spraying on the surface of a metal substrate and curing; the component A contains modified epoxy resin, hydrophobic fumed silica, inorganic pigment, rutile titanium dioxide, propylene glycol monomethyl ether and ultrafine zinc powder; the component B contains 2,4,6-tris (dimethylaminomethyl) phenol; ethylenediamine; the balance is a mixing auxiliary agent isopropanol; the weight content of the component A and the component B is: 85-90% of the component A; 10-15% of the component B. The long-term anticorrosion material of this formula is usually used as a coating primer, has a good chemical bonding effect with the substrate, and is matched with acrylic resin and polyurethane resin topcoat to be used for the anticorrosion of ships, marine engineering equipment, and field pipeline equipment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an anti-corrosion coating, in particular to a coating with long-term anti-corrosion function. Background Art

[0002] A flexible epoxy anti-corrosion coating is disclosed in the Chinese patent database, with publication number CN101260273A and publication date 20080910. The anti-corrosion coating is composed of 20%-69% epoxy resin, 20%-69% anti-rust pigment filler, 10%-30% modified curing agent, 0.5%-3% additives, and 0%-30% diluent in a weight ratio.

[0003] The epoxy resin is one of bisphenol A diglycidyl ether, tetrabromobisphenol A diglycidyl ether, hydrogenated bisphenol A diglycidyl ether, bisphenol F diglycidyl ether, bisphenol S diglycidyl ether, or a mixture of more than one of them.

[0004] The anti-rust pigment filler is one or a mixture of mica powder, silica powder, titanium dioxide, mica iron oxide, iron red, zinc yellow, aluminum tripolyphosphate, zinc phosphate, zinc oxide, precipitated barium sulfate, talc, fumed silica, aluminum powder, and zinc powder.

[0005] The modified curing agent is a Michael adduct prepared by Michael addition reaction of aliphatic polyamine and acrylic acid oligomer, wherein the aliphatic polyamine is one of ethylenediamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine or polyethylenepolyamine or a mixture of more than one of them.

[0006] The additive is one or a mixture of several of curing accelerators, dispersants, defoamers, leveling agents and anti-settling agents.

[0007] The coating has good adhesion and anti-corrosion properties and good toughness, especially the toughness of the coating after being immersed in seawater is greatly improved compared with conventional epoxy coatings.

[0008] The disadvantage is that: the coating has certain anti-corrosion performance, but it requires the surface of the substrate to be cleaned in advance so that the coating has good adhesion. Therefore, its application is limited when implemented in the field. Summary of the invention

[0009] The purpose of the present invention is to provide a thick film long-lasting anticorrosion material under low surface treatment conditions, so that a coating with good adhesion and anticorrosion performance can be obtained under low surface treatment conditions.

[0010] The object of the present invention is achieved by: a thick film long-term anti-corrosion material under low surface treatment conditions, wherein the thick film long-term anti-corrosion material is formed by mixing component A and component B, spraying them on the surface of a metal substrate and curing them;

[0011] The component A contains modified epoxy resin, hydrophobic fumed silica, inorganic pigment, rutile titanium dioxide, propylene glycol monomethyl ether and ultrafine zinc powder.

[0012] The weight content of each ingredient is:

[0013] The modified epoxy resin is 50.8-61.2%, wherein the modified epoxy resin is low sulfonic acid modified bisphenol A diglycidyl ether; wherein the total mass of sulfonate ions and the total mass of the modified epoxy resin are in a ratio of (3-5): 100. The epoxy resin structure contains hydroxyl groups, ether groups and extremely active epoxy groups, and the hydroxyl groups and ether groups are highly polar, so that the epoxy molecules and the adjacent interfaces generate strong intermolecular forces, and the epoxy groups react with the free bonds on the metal surface to form chemical bonds, so that the epoxy resin has very high bonding strength, and after sulfonic acid modification, the hydrophilicity and dispersibility of the epoxy resin are improved.

[0014] Hydrophobic fumed silica 3-4%; fumed silica is a new ultrafine inorganic material with a very small particle size, so it has a large specific surface area, strong surface adsorption, large surface energy, high chemical purity, good dispersibility, and excellent stability, reinforcement, thickening and thixotropy. Its addition can thicken epoxy resin;

[0015] 10-15% inorganic pigment, the pigment is ferrous oxide or silver aluminum paste powder;

[0016] Rutile titanium dioxide 5.8-6.2%; the addition of rutile titanium dioxide has the advantages of high hiding power and strong tinting power, and can also enhance the mechanical strength and adhesion of the paint film, prevent cracks, prevent ultraviolet rays and moisture penetration, and extend the life of the paint film;

[0017] Propylene glycol monomethyl ether 12-14%, as an anti-instant rust additive, can also reduce the film-forming temperature and promote its condensation and film formation;

[0018] Ultrafine zinc powder 8-10%, 200-800 mesh; zinc powder can form a closed layer to strengthen the protection of the substrate. The formation of corrosion products on the surface of the metal substrate can reduce the potential difference between the coating and the substrate. After the coating is damaged, the new metal zinc layer is exposed, the potential difference increases rapidly, and a strong cathodic protection effect is produced, which greatly enhances the anti-corrosion effect of the substrate;

[0019] The weight content of each component in the B component is: 10-15% of 2,4,6-tris(dimethylaminomethyl)phenol; 5-8% of ethylenediamine; the balance is a mixing auxiliary agent, isopropyl alcohol; 2,4,6-tris(dimethylaminomethyl)phenol and ethylenediamine are both thixotropic additives, and the two work together to make the modified epoxy resin solidify, and after solidification, the anti-adhesion force is large and it is not easy to crack;

[0020] The weight contents of component A and component B are: component A 85-90%; component B 10-15%.

[0021] Compared with the prior art, the beneficial effects of the present invention are as follows: the thick-film long-term anti-corrosion material sprayed on the surface of the substrate obtained by the present invention does not require deep cleaning of the substrate surface, and can be directly sprayed when the substrate surface is not highly oxidized. The epoxy resin and the steel body can also undergo a weak chemical reaction to form a chemical bond, so that the epoxy resin can adhere firmly to the surface of the metal substrate after curing. The coating of the thick-film long-term anti-corrosion material obtained in this way has strong adhesion and good oxidation resistance, and can protect the surface of the metal substrate for a long time. The long-term anti-corrosion material of this formula is usually used as a coating primer, and has a good chemical bonding effect with the substrate. It is combined with acrylic resin and polyurethane resin topcoats and can be used for the anti-corrosion of ships, marine engineering equipment, and field pipeline equipment.

[0022] Furthermore, the metal substrate is steel, and the spraying thickness is 0.2-3 mm.

[0023] Furthermore, the curing temperature when sprayed on the surface of the metal substrate is 10-40° C., and the curing time is 2-48 hours.

[0024] Furthermore, component A is fully stirred before use, and then component B is added to component A and stirred for 5-15 minutes before spraying on the surface of the metal substrate. DETAILED DESCRIPTION

[0025] Example 1

[0026] A thick film long-term anti-corrosion material under low surface treatment conditions, wherein the thick film long-term anti-corrosion material is formed by mixing component A and component B, spraying the mixture on the surface of a metal substrate and curing the mixture;

[0027] The component A contains modified epoxy resin, hydrophobic fumed silica, inorganic pigment, rutile titanium dioxide, propylene glycol monomethyl ether and ultrafine zinc powder.

[0028] The weight content of each ingredient in component A is:

[0029] 61.2% of modified epoxy resin, wherein the modified epoxy resin is low-sulfonic acid modified bisphenol A diglycidyl ether; the low-sulfonic acid modified bisphenol A diglycidyl ether is obtained by sulfonation reaction of sodium sulfite and bisphenol A diglycidyl ether, and the amount of sodium sulfite is adjusted so that the ratio of the total mass of sulfonate ions to the total mass of the modified epoxy resin is (3-5):100, thereby forming modified bisphenol A diglycidyl ether with a low sulfonation degree; the low-sulfonic acid modified bisphenol A diglycidyl ether in which the ratio of the total mass of sulfonate ions to the total mass of the modified epoxy resin is 5:100 is used in this embodiment;

[0030] Hydrophobic fumed silica 3%;

[0031] 10% inorganic pigment, wherein the pigment is ferrous oxide;

[0032] Rutile titanium dioxide 5.8%;

[0033] Propylene glycol monomethyl ether 12%, as an anti-flash rust additive;

[0034] Ultrafine zinc powder 8%, 200 mesh-800 mesh;

[0035] The weight content of each component in the B component is: 12% of 2,4,6-tris(dimethylaminomethyl)phenol; 8% of ethylenediamine; and the balance is the mixing auxiliary agent isopropanol;

[0036] The weight content of component A and component B is: component A 85%; component B 15%;

[0037] Before using, stir component A thoroughly, then add component B to component A and continue stirring for 5-15 minutes before spraying on the surface of the metal substrate. Specifically: the metal substrate is a carbon steel plate, which is naturally stored for 60 days under 25°C and 60% constant humidity air conditions, then the surface of the carbon steel plate is simply brushed clean with a wire brush, and then a coating with a total thickness of 0.2-3mm is sprayed on the steel plate in 3-5 times; the curing temperature after spraying is 40°C, and the curing time is 24 hours, to obtain a thick film long-term anti-corrosion material coating sprayed on the surface of the carbon steel plate.

[0038] Embodiment 2-6

[0039] The following table shows the weight dosage of each substance in component A in Examples 1-6.

[0040] Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Modified epoxy resin 61.2 50.8 57 55 56.2 57.8 Hydrophobic fumed silica 3 4 4 3 4 3 Ferrous oxide 10 15 0 0 11 12 Silver aluminum paste powder 0 0 10 15 0 0 Rutile Titanium Dioxide 5.8 6.2 6 6 5.8 6.2 Propylene glycol monomethyl ether 12 14 14 12 13 13 Ultrafine zinc powder 8 10 9 9 10 8

[0041] The composition and dosage of component B corresponding to Examples 2-6 are the same as those in Example 1.

[0042] The low-sulfonic acid modified bisphenol A diglycidyl ether in Example 4-6 is obtained by sulfonation reaction of sodium sulfite and bisphenol A diglycidyl ether, and the molar ratio of sodium sulfite to bisphenol A diglycidyl ether is 1:15.

[0043] The weight amounts of component A and component B are the same as those in Example 1.

[0044] The mechanical properties of the thick film long-term anticorrosion materials of Examples 1-6 obtained in this way are as follows:

[0045] Adhesion test (Mpa) Cross-cut test, grade Example 1 ≥16Mpa 0 Example 2 ≥16Mpa 1 Example 3 ≥16Mpa 0 Example 4 ≥16Mpa 1 Example 5 ≥16Mpa 0 Example 6 ≥16Mpa 0

[0046] Example 1-6 was subjected to a cyclic immersion test, with tap water immersion and drying, 12 hours of immersion and 12 hours of drying alternately, and a grid of 10*10mm was crossed. After a period of time, the maximum size of erosion from the edge of the grid line to the center was measured. The conclusion is shown in the following table:

[0047] Time required to erode 1mm (days) Time required to erode 2mm (days) Example 1 48 82 Example 2 47 80 Example 3 52 90 Example 4 43 73 Example 5 47 78 Example 6 40 72

[0048] Examples 1-6 were subjected to salt water immersion tests to simulate the environmental conditions of seawater immersion, and the conclusions are shown in the following table:

[0049] Time required to erode 1mm (days) Time required to erode 2mm (days) Example 1 38 58 Example 2 36 67 Example 3 40 59 Example 4 32 52 Example 5 38 57 Example 6 33 54

[0050] Example 7

[0051] On the basis of Example 1, only the weight ratio of component A to component B was changed to obtain the results shown in the following table:

[0052]

[0053]

[0054] The above table shows that when the A component is 85-90% and the B component is 10-15%, the thick film long-term anti-corrosion material has a strong adhesion. As a curing agent, too much or too little of the B component will lead to a decrease in the adhesion of the thick film long-term anti-corrosion material.

[0055] Example 8

[0056] The screening of the amount of 2,4,6-tris(dimethylaminomethyl)phenol was carried out based on Example 1, and only the amount of 2,4,6-tris(dimethylaminomethyl)phenol in component B was changed to obtain the results shown in the following table:

[0057]

[0058] The results show that the preferred amount of 2,4,6-tris(dimethylaminomethyl)phenol is 10-15%.

[0059] The amount of ethylenediamine was screened. Based on Example 1, only the amount of ethylenediamine in component B was changed, and the results shown in the following table were obtained:

[0060]

[0061]

[0062] The results show that the preferred weight range of ethylenediamine is 5-8%.

[0063] Example 9

[0064] The ratio of the total mass of sulfonate ions to the total mass of the modified epoxy resin was screened, and the obtained coatings were subjected to adhesion tests and salt spray tests.

[0065] The salt spray test adopts the standard GB / T 6461-2002. The required equipment includes spray nozzle, salt water bucket, test piece holder, spray liquid collection container, salt water supply bucket, pressure bucket, compressed air supply equipment and exhaust equipment, etc. The spray horizontal area is 80cm 2 , with a diameter of about 10 cm, is placed near the sample; the amount of spray liquid is calculated in the entire hour, and the area used is 80 cm 2 The funnel collects the salt spray precipitation of continuous atomization for 8 hours, and an average of 1.6mL of solution should be collected every hour. The concentration of sodium chloride solution in the salt water bucket is maintained at 40-60g / l during the test. The pH value of the salt solution before atomization is 6.5-7.2, and the temperature is 35±2℃. After 48 hours of spraying, the sample is observed, and the percentage of defect area in the entire test area is the test content.

[0066] The test results are shown in the following table:

[0067]

[0068]

[0069] The above test results show that the reduction of sulfonate ions will significantly reduce the adhesion. When the sulfonate ions increase, the salt spray resistance of the sulfonate ions decreases due to their hydrophilicity. The preferred ratio of the total mass of sulfonate ions to the total mass of the modified epoxy resin is (3-5):100.

[0070] The present invention is not limited to the above-mentioned embodiments. On the basis of the technical solution disclosed in the present invention, technicians in this field can make some substitutions and deformations to some technical features therein according to the disclosed technical content without creative labor, and these substitutions and deformations are all within the protection scope of the present invention.

Claims

1. A thick film long-term anticorrosion material under low surface treatment conditions, characterized in that: The thick film long-term anti-corrosion material is formed by mixing component A and component B, spraying them on the surface of the metal substrate and curing them; In the A component, the weight content of each component is: 50.8-61.2% of modified epoxy resin, wherein the modified epoxy resin is low sulfonic acid modified bisphenol A diglycidyl ether; wherein the ratio of the total mass of sulfonate ions to the total mass of the modified epoxy resin is (3-5):100; the low sulfonic acid modified bisphenol A diglycidyl ether is obtained by sulfonation reaction of sodium sulfite and bisphenol A diglycidyl ether; Hydrophobic fumed silica 3-4%; 10-15% inorganic pigment, the pigment is ferrous oxide or silver aluminum paste powder; Rutile titanium dioxide 5.8-6.2%; Propylene glycol monomethyl ether 12-14%, as an anti-flash rust additive; Ultrafine zinc powder 8-10%, 200 mesh-800 mesh; The weight content of each component in the B component is: 10-15% of 2,4,6-tris(dimethylaminomethyl)phenol; 5-8% of ethylenediamine; and the balance is the mixing auxiliary agent isopropanol; The weight contents of component A and component B are as follows: component A 85-90%; component B 10-15%.

2. The thick-film long-lasting anticorrosion material under low surface treatment conditions according to claim 1, characterized in that: The metal substrate is steel, and the spraying thickness is 0.2-3 mm.

3. The thick-film long-lasting anticorrosion material under low surface treatment conditions according to claim 1, characterized in that: The curing temperature when sprayed on the surface of the metal substrate is 10-40°C and the curing time is 2-48 hours.

4. The thick-film long-term anticorrosion material under low surface treatment conditions according to claim 1, characterized in that: Before use, stir component A thoroughly, then add component B into component A and continue stirring for 5-15 minutes before spraying on the surface of the metal substrate.