A high-strength Mg-Ta composite material with good shielding performance and its preparation method and application
By designing the aluminum-coated Ta preform and the honeycomb network structure of magnesium alloy, combined with the dip-casting process and solid solution aging heat treatment, the problems of low efficiency and insufficient interface strength in the preparation of Mg-Ta composite materials were solved, and high strength was achieved Combined with good shielding properties, it is suitable for radiation-resistant materials for deep space detectors.
Patent Information
- Application Number
- CN202311824604.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-27
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-12-27
AI Technical Summary
The preparation process of existing Mg-Ta composite materials is inefficient and difficult to achieve the combination of high strength and good shielding performance. Especially under the dual challenges of radiation resistance and energy demand in deep space detectors, existing technology has not been able to effectively solve it. The problem of metallurgical connection and insufficient interface strength of Mg and Ta.
The aluminum-coated Ta preform and magnesium alloy are designed through a honeycomb network structure, combined with the dip-casting process and solid solution aging heat treatment, to form a three-dimensional interpenetrating network structure to ensure the complete filling of the magnesium liquid and the effective combination of Ta and Mg, reducing Interface cracking fails and the shielding performance is enhanced.
Achieving high strength, good shielding performance and heat resistance Mg-Ta composite materials, improving production efficiency and material stability, suitable for radiation-resistant lightweight composite materials for deep space detectors, which has important scientific significance and engineering value.
Smart Images

Figure CN117758172B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of metal matrix composite materials, and in particular relates to a high-strength Mg-Ta composite material with good shielding performance and a preparation method and application thereof. Background Art
[0002] Jupiter's moon Europa is considered to be the most likely place for life to exist. Exploring Jupiter is of great significance to the search for life outside the Earth. However, there are still two major technical difficulties in successfully exploring Jupiter. The first is Jupiter's strong surface magnetic field and the high-density high-energy particle radiation in the Jupiter orbit. The second is the energy problem caused by Jupiter's long distance. This puts forward dual requirements for the detector's instruments and equipment to resist high-energy particle radiation and be lightweight. One of the important development directions of my country's deep space exploration technology research is to upgrade and significantly reduce the weight based on the existing structural design, materials, and process technology (Optimization Design of Radiation Vault in Jupiter Orbiting Mission [J](JZ Wang, JN Ma, JW Qiu, D. Tian, AW Zhu, QX Zhang, AS Zhou. IEEE Transactions on Nuclear Science, (66) 2019, 2179-2187.)). Among them, the combination of heavy metal radiation-resistant materials such as Ta and Nb with lightweight structural metal materials such as Mg is expected to alleviate the two major technical problems of radiation and energy faced by Jupiter probes. The analysis and calculation of the radiation-resistant material system of the Jupiter probe structure show that the Mg / Ta layered composite plate can effectively reduce the weight by about 45.1% under the premise of having the same radiation-resistant effect as foreign heavy metal materials, which brings great potential for the development of my country's deep space exploration technology. However, due to the metallurgical incompatibility of Mg and Ta, the melting point of the two metals (the melting point of Ta is 2996℃, the melting point of Mg is 650℃), lattice type (Ta is BCC, Mg is HCP), linear expansion coefficient and other physical and chemical properties and metallurgical properties are very different, so Mg / Ta is difficult to connect, and there are few reports on the preparation process of Mg / Ta composites at home and abroad.
[0003] The Chinese patent with publication number CN113733685A reported a light and high-strength Mg-Al-Ta composite metal sheet and its rolling forming method. Although this method can realize the processing and preparation of Mg / Ta layered composite sheets, the process involves heat preservation treatment of Mg sheets and Ta sheets at different temperatures respectively, and then stacking and fixing the sheets. The temperature change of the stacked sheets before rolling deformation is difficult to effectively control and the production efficiency is not high; the Chinese patent with publication number CN113352708A reported a light and high-strength Mg-Ta composite metal sheet and its room temperature rolling forming method. Although this preparation method avoids medium and high temperature Rolling may cause plate oxidation and energy consumption problems, but in order to effectively reduce the residual stress between different metal plates and ensure the smooth progress of rolling deformation, it is necessary to introduce low-temperature recovery annealing and high-temperature diffusion annealing between rolling passes, and multiple rolling deformation passes are required, and its production efficiency is not high; Chinese patent publication number CN112742870A reports a method for preparing a shielded magnesium-tantalum multilayer composite plate. Although it can realize the processing and preparation of Mg / Ta layered composite plates, its process involves the use of high-temperature rolling in a vacuum to avoid the oxidation problem of the plate, which has high requirements on rolling equipment and rolling environment, and the production efficiency is not high.
[0004] It can be seen that the above patents mostly adopt a method for preparing layered composite materials by thermomechanical coupling of multi-pass medium and high temperature rolling processing and annealing heat treatment. Currently, there are few reports on the preparation of three-dimensional interpenetrating network structure Mg / Ta composite materials combining structural design and dip-casting process.
[0005] In addition, the above patents do not consider optimizing shielding performance by utilizing the distribution design of Ta in the Mg alloy in the Mg / Ta composite material. Summary of the invention
[0006] One of the purposes of the present invention is to provide a high-strength Mg-Ta composite material with good shielding performance. The Mg-Ta composite material has strong quality stability, good heat resistance, high strength and good shielding performance.
[0007] The second object of the present invention is to provide a method for preparing a high-strength Mg-Ta composite material with good shielding performance. The preparation method has a simple and mature process, low vacuum requirements, high production efficiency, and high process stability, and can be used for large-area high-strength solid-phase connection of Mg and Ta dissimilar materials.
[0008] The third object of the present invention is to provide a high-strength Mg-Ta composite material with good shielding performance as an application of radiation-resistant lightweight composite material, especially suitable for deep space detector shielding structure.
[0009] The technical solutions adopted by the present invention to achieve the above-mentioned purpose are as follows.
[0010] The high-strength Mg-Ta composite material with good shielding performance of the present invention is composed of a Ta preform with an aluminized surface and a magnesium alloy;
[0011] The Ta preform is composed of n layers of Ta wire meshes stacked in sequence, with adjacent two layers of Ta wire meshes arranged at intervals, n≥5, the Ta wire meshes are all honeycomb structures, and taking any one layer of Ta wire mesh as a reference, in the direction perpendicular to this Ta wire mesh, the hexagonal holes of this Ta wire mesh are blocked by the sides of the hexagons of the remaining n-1 layers of Ta wire meshes in space;
[0012] The magnesium alloy fills the voids of the Ta preform with an aluminized surface in space and forms a three-dimensional interpenetrating network structure with the Ta preform with an aluminized surface.
[0013] Preferably, the side width a of each hexagon of the Ta wire mesh is 0.5-1 mm, the side length b satisfies 1 mm < b ≤ 2(n-1)×a, the perpendicular distance between two parallel sides ≤ (n-1)×a, the layer spacing of the n layers of Ta wire meshes is 0.5-1 mm, and the stacking direction forms an angle θ = 90°±30° with any one side of the hexagon of the reference Ta wire mesh.
[0014] Preferably, the magnesium alloy is a Mg-Gd-Y series alloy, and more preferably, the Mg-Gd-Y series alloy is Mg-10Gd-3Y-0.5Zr (wt.%).
[0015] The preparation method of the high-strength Mg-Ta composite material with good shielding performance of the present invention includes the following steps:
[0016] S1, establish a three-dimensional model of the Ta preform;
[0017] S2, according to the three-dimensional model of the Ta preform in step S1, prepare the Ta preform by metal fiber wire braiding technology or 3D printing technology:
[0018] S3, perform surface pretreatment on the Ta preform to remove the surface oxide layer and impurities:
[0019] S4, immerse the pretreated Ta preform into the molten pure aluminum liquid for immersion plating treatment to obtain a Ta preform with an aluminized surface:
[0020] S5, proportion the components according to the content of each component in the Mg alloy, and under the protection of an inert atmosphere, perform vacuum melting to obtain molten Mg liquid:
[0021] S6, immerse the Ta preform with an aluminized surface into the molten Mg liquid, keep warm, and cool to obtain a Mg-Ta composite structure:
[0022] S7, machining the Mg-Ta composite structure to remove excess Mg alloy outside the Mg-Ta composite structure, and performing heat treatment according to the solid solution aging heat treatment process of the Mg alloy in step S5 to obtain a Mg-Ta composite material with shielding performance.
[0023] Preferably, in step S3, the Ta preform is placed in a tantalum acid cleaning solution for chemical cleaning for 0.5-2 minutes, more preferably, for 30 seconds.
[0024] Preferably, in step S4, the pretreated Ta preform is placed in molten pure aluminum for 10-20 minutes, more preferably, for 15 minutes.
[0025] Preferably, in step S5, the smelting temperature is 650-730°C.
[0026] Preferably, in step S6, the Ta preform with aluminum coating on the surface is placed in a mold, and under the protection of an inert atmosphere, molten Mg liquid is introduced into the mold, and after being kept at 650°C for 10-30min, it is naturally cooled to form a Mg-Ta composite structure; more preferably, the mold is a sand mold; more preferably, the mold is kept warm for 20min.
[0027] Preferably, in step S7, the heat treatment conditions are: first treating at 500-525° C. for 8-12 h, and then treating at 250° C. for 12 h.
[0028] The present invention also provides the use of the high-strength Mg-Ta composite material with good shielding performance or the high-strength Mg-Ta composite material with good shielding performance prepared by the above preparation method as a radiation-resistant lightweight composite material.
[0029] The principle of the present invention is as follows: the preparation method of the high-strength Mg / Ta composite material with high shielding performance of the present invention is to design a honeycomb mesh structure + a layered shell-like structure for the Ta preform. The honeycomb mesh structure ensures the complete filling of the magnesium liquid. At the same time, the cross-clamps of Mg and Ta avoid the common failure problem of insufficient interface strength of immiscible metal composites. The layered shell-like structure design realizes no gaps in a one-way view through the staggered treatment of the interlayer pores, thereby ensuring the shielding performance of the composite material and its consistency at different positions. In addition, the weight of the Ta preform is reduced by the above-mentioned structural design and adjusting the Mg / Ta mass ratio. The Ta preform is treated with aluminum liquid immersion plating, and the metallurgical bonding of the interface is achieved by setting an intermediate layer. The Ta preform with Al plated on the surface is immersed in the molten Mg liquid until the gaps are completely filled and then cooled and solidified to room temperature, thereby realizing the three-dimensional interpenetrating composite of Mg and Ta. The use of dip casting (infiltration) avoids the problem of Mg and Ta being difficult to coordinate large plastic deformation encountered in thermomechanical coupling processes such as rolling; in this process, a high-strength mechanical connection between a high-strength magnesium alloy and a Ta preform is achieved by using a three-dimensional interpenetrating network composite, avoiding the interface cracking failure problem of the layered composite; the use of a hot-dip Al layer avoids the surface oxidation of Ta on the one hand, and on the other hand, it acts as an intermediate layer to "bond" the Mg layer and the Ta layer, thereby enhancing the diffusion connection between the two immiscible systems. The Mg / Ta composite material is subjected to solid solution and aging heat treatment to eliminate the residual stress caused by the Ta bracket constraint in the casting process, and at the same time, the Ta bracket, the Al coating and the magnesium alloy body can achieve effective metallurgical bonding in the subsequent heat treatment process. In addition, the Ta preform + dip casting process used in the present invention has the characteristics of anti-shielding functionality and non-interference in the selection of Mg alloy components, and the anti-shielding performance and high-strength heat-resistant structural performance can be synergistically improved through preform design structure optimization, Mg alloy material design and heat treatment process.
[0030] Compared with the prior art, the present invention has the following beneficial effects:
[0031] The preparation method of the high-strength Mg-Ta composite material with good shielding performance of the present invention realizes the effective combination of magnesium alloy (ultra-high-strength Mg-Gd-Y alloy) and Ta by designing a structural and functional integration method of immiscible metals, based on the steps of designing Ta preform structure, pretreatment, immersion plating, alloy formulation, smelting, cooling, machining and heat treatment, thereby creating a composite material with multiple properties.
[0032] The preparation method of the high-strength Mg-Ta composite material with good shielding performance of the present invention ensures the complete filling of magnesium liquid through the honeycomb mesh structure design of the Ta preform, and at the same time avoids the problem of insufficient interface strength commonly found in immiscible metal composite materials through the honeycomb mesh structure design.
[0033] The preparation method of the high-strength Mg-Ta composite material with good shielding performance of the present invention utilizes immersion plating in molten pure aluminum liquid to enhance the bonding ability between Ta and Mg alloy and avoid the formation of an oxide layer in subsequent processes.
[0034] The method for preparing the high-strength Mg-Ta composite material with good shielding performance of the present invention realizes the metallurgical bonding of Ta-Al-Mg by utilizing the Al immersion plating layer, thereby improving the strength and stability of the composite material.
[0035] The preparation method of the high-strength Mg-Ta composite material with good shielding performance of the present invention preferably selects Mg-10Gd-3Y-0.5Zr (wt.%) alloy components, and obtains the high-strength Mg-Ta composite material through a specific solid solution aging heat treatment process, while ensuring its heat resistance.
[0036] The high-strength Mg-Ta composite material with good shielding performance of the present invention realizes no gap in one-way view by designing the layered structure of Ta wire mesh, thereby ensuring the shielding performance of the composite material and its consistency at different positions.
[0037] The high-strength Mg-Ta composite material with good shielding performance of the present invention, the yield strength of the rare earth magnesium alloy can be ≥225MPa, and after testing, the yield strength does not decrease at 250°C. It can be used to efficiently prepare radiation-resistant lightweight composite materials for deep space detector shielding structures, and has important scientific significance and engineering value. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0039] Figure 1 A schematic structural diagram of the Ta preform of the present invention.
[0040] Figure 2 A schematic structural diagram of a Ta preform in the present invention in a direction perpendicular to the reference Ta screen.
[0041] Figure 3 Schematic diagram of the key dimension parameter relationship of the Ta wire mesh of the present invention.
[0042] Figure 4 The process flow chart of the preparation method of the high-strength Mg-Ta composite material with good shielding performance in the present invention. DETAILED DESCRIPTION
[0043] To further understand the present invention, the preferred embodiments of the present invention are described below. However, it should be understood that these descriptions are only for further explaining the features and advantages of the present invention, rather than limiting the claims of the present invention.
[0044] As Figure 1 shown, the high-strength Mg-Ta composite material with good shielding performance of the present invention is composed of a Ta preform with an aluminum coating on the surface and a magnesium alloy. Among them, the Ta preform is composed of n layers of Ta wire meshes stacked in sequence, and adjacent two layers of Ta wire meshes are spaced apart. n≥5, and all Ta wire meshes are honeycomb structures. And taking any one layer of Ta wire mesh as a reference, in the direction perpendicular to this Ta wire mesh, the hexagonal holes of this Ta wire mesh are blocked by the edges of the hexagons of the remaining n-1 layers of Ta wire meshes to achieve the shielding function. For example, taking the topmost layer of Ta wire mesh as a reference, then looking in the direction perpendicular to the topmost layer of Ta wire mesh, the edges of the hexagons of the n-1 layers of Ta wire meshes below it exactly block the hexagonal holes of the topmost layer of Ta wire mesh, as Figure 2 shown; the magnesium alloy fills the voids of the Ta preform with an aluminum coating on the surface in three-dimensional space and forms a three-dimensional interpenetrating network structure with the Ta preform with an aluminum coating on the surface.
[0045] In the above technical solution, preferably, the edge width a of each hexagon of the Ta wire mesh is 0.5-1 mm, the side length b satisfies 1 mm < b ≤ 2(n-1)×a, the perpendicular distance between two parallel sides ≤ (n-1)×a, the layer spacing of the n layers of Ta wire meshes is 0.5-1 mm, and the stacking direction forms an angle θ = 90°±30° with any one side of the hexagon of the reference Ta wire mesh; as Figure 3 shown.
[0046] In the above technical solution, preferably, five layers of Ta wire meshes are used. The layer spacing of the five layers of Ta wire meshes is 0.5 mm, the thickness of the Ta preform is 4 mm, the side length of each hexagon is 2 mm, and the edge width is 0.5 mm. This structure not only meets the minimum number of layers requirements of the composite material, but also considers the structural lightweight and ensures the required shielding performance.
[0047] In the above technical solution, there is no special limitation on the Mg alloy, and it can be any kind of magnesium alloy. In this embodiment, it is preferably a Mg-Gd-Y series alloy, and particularly preferably Mg-10Gd-3Y-0.5Zr (wt.%). This alloy has the advantage of high yield strength.
[0048] As Figure 4 shown, the preparation method of the high-strength Mg-Ta composite material with good shielding performance of the present invention includes the following steps:
[0049] S1, establishing a three-dimensional model of the Ta preform;
[0050] The Ta preform can achieve complete filling of molten Mg liquid;
[0051] S2, according to the three-dimensional model of the Ta preform in step S1, a Ta preform is prepared by metal fiber filament (Ta fiber filament) weaving technology or 3D printing technology (specifically, n layers of Ta wire mesh are prepared and stacked in a mold to form a structure of the Ta preform);
[0052] Ta fiber weaving technology or 3D printing technology is an existing technology;
[0053] S3, pre-treating the surface of the Ta preform (n-layer Ta wire mesh) to remove the surface oxide layer and impurities:
[0054] Removing the oxide layer and impurities on the surface of the Ta preform (n-layer Ta wire mesh) can improve the effect of subsequent processes. Preferably, the Ta preform (n-layer Ta wire mesh) is placed in a tantalate acid cleaning solution for chemical cleaning for 0.5-2 minutes;
[0055] S4, placing the pretreated Ta preform (n-layer Ta wire mesh) into a molten pure aluminum liquid for immersion plating to obtain a Ta preform (n-layer Ta wire mesh) with aluminum plated on the surface;
[0056] The Ta preform (n-layer Ta wire mesh) is placed in molten pure aluminum for immersion plating to prevent the formation of Ta oxide layer in subsequent processes and enhance the bonding ability with Mg alloy; preferably, the pretreated Ta preform (n-layer Ta wire mesh) is placed in the molten pure aluminum for 10-20 minutes;
[0057] S5, mixing ingredients according to the content of each component in the Mg alloy, and vacuum melting under inert atmosphere protection to obtain molten Mg liquid:
[0058] The preferred melting temperature is 650°C-730°C;
[0059] S6, placing the Ta preform (n layers of Ta wire mesh) with aluminum coating on the surface in a mold (the mold may have a supporting and fixing structure corresponding to each layer of Ta wire mesh, so that n layers of Ta wire mesh are stacked to form a Ta preform), introducing molten Mg liquid into the mold under the protection of the surface inert atmosphere, keeping the temperature at 650° C. for 10-30 minutes, and then cooling naturally to form a Mg-Ta composite structure; more preferably, the mold is a sand mold;
[0060] S7, machining the Mg-Ta composite structure to remove excess Mg alloy outside the Mg-Ta composite structure, and performing heat treatment according to the solid solution aging heat treatment process of the Mg alloy in step S5 to obtain a high-strength Mg-Ta composite material with shielding performance;
[0061] Heat treatment can release the internal stress of the Mg-Ta composite material, preferably solution treatment at 500-525°C for 8-12h and aging treatment at 250°C for 12h.
[0062] In the present invention, the inert atmosphere is preferably argon.
[0063] The high-strength Mg-Ta composite material with shielding performance of the present invention can be used as a radiation-resistant lightweight composite material, especially as a radiation-resistant lightweight composite material for a shielding structure of a deep space detector.
[0064] The terms used in the present invention generally have the meanings commonly understood by those of ordinary skill in the art, unless otherwise specified.
[0065] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention will be further described in detail below in conjunction with embodiments and comparative examples.
[0066] In the following examples and comparative examples, various processes and methods not described in detail are conventional methods known in the art. The materials, reagents, devices, instruments, equipment, etc. used in the following examples and comparative examples, unless otherwise specified, can be obtained from commercial sources.
[0067] Example 1
[0068] A method for preparing a high-strength Mg-Ta composite material with good shielding performance comprises the following steps:
[0069] S1, establish Figure 1 and Figure 2 The three-dimensional model of the Ta preform shown, the Ta preform is formed by stacking five layers of Ta wire mesh, the layer spacing is 0.5 mm, the Ta wire mesh is a honeycomb structure, and the side length of each hexagon is 2 mm and the side width is 0.5 mm;
[0070] S2, based on the 3D model of the Ta preform, the Ta preform is woven by Ta fiber filaments (W0500-BA4-000: 0.500 mm (0.0197”) + / - 0.005 mm (0.0002”) – R05400 – Annealed);
[0071] S3, placing the Ta preform into a tantalum acid cleaning solution for 30 seconds to remove surface oxides and inclusions;
[0072] S4, placing the pretreated Ta preform into a molten pure aluminum liquid for immersion plating for 15 minutes to obtain a Ta preform with aluminum plated on the surface;
[0073] S5, vacuum melting Mg-10Gd-3Y-0.5Zr alloy (GW103) at 650°C under argon atmosphere protection to obtain molten Mg liquid;
[0074] S6, placing the Ta preform with aluminum coating on the surface into a sand mold with a size of 110×110×3 mm, placing the sand mold in a vacuum heat treatment furnace, and keeping it warm at 650°C. Under the protection of argon gas on the surface, introducing molten Mg liquid from outside the furnace into the sand mold, and under the protection of argon gas, the poured sand mold is further placed in a vacuum heat treatment furnace at 650°C and kept warm for 20 minutes. After the melt fully fills the Ta preform with aluminum coating on the surface, turn off the power of the vacuum heat treatment furnace, open the furnace door, and let it cool naturally to form a Mg-Ta composite structure;
[0075] S7, the Mg-Ta composite structure is subjected to a solution aging heat treatment process, first at 525°C × 12h, and then water-cooled at +250°C × 12h, to release the internal stress of the Mg-Ta composite structure;
[0076] S8, machining the Mg-Ta composite structure to remove excess Mg alloy from the outside, and obtaining a Mg / Ta interpenetrating network composite material, that is, a Mg-Ta composite material with good shielding properties.
[0077] Comparative Example 1
[0078] The preparation of a Mg / Ta interpenetrating network composite material described in this comparative example is the same as that in Example 1, with the only difference being that the aperture of the Ta mesh is larger (the side length of each hexagon of the honeycomb structure is 6 mm). Therefore, taking any layer of the Ta mesh as a reference, in a direction perpendicular to the Ta mesh, the hexagonal holes of the Ta mesh are not blocked by the side spaces of the hexagons of the remaining n-1 layers of the Ta mesh, and there are gaps.
[0079] Comparative Example 2
[0080] The preparation of a Mg / Ta interpenetrating network composite material described in this comparative example is the same as that in Example 1, the only difference being that the aperture of the Ta wire mesh is smaller (the side length of each hexagon of the honeycomb structure is 1 mm).
[0081] Comparative Example 3
[0082] The preparation method of a Mg / Ta interpenetrating network composite material described in this comparative example is the same as that in Example 1, except that step S4 is omitted, and in step S6, the pretreated Ta preform is placed in a sand mold having a size of 110×110×3 mm.
[0083] Comparative Example 4
[0084] The method for preparing a Mg / Ta interpenetrating network composite material described in this comparative example is the same as that in Example 1, except that there is no step S7, and in step S8, the Mg-Ta prepared in step S6 is machined.
[0085] The Mg / Ta interpenetrating network composite materials prepared in Example 1 and Comparative Examples 1-4 were subjected to yield strength test (GB / T228.1-2021 Metal material tensile test, the tensile direction is parallel to the layer of the Ta skeleton), field emission electron microscopy (SEM) observation and shielding radiation test. The results show that:
[0086] The Mg / Ta interpenetrating network composite material prepared in Example 1 has good surface quality, complete void filling, a yield strength of ~250 MPa, a Mg / Al / Ta interface diffusion width of ~14 μm, good interface bonding, and a neutron shielding rate of 99% when the thickness is 4 mm under irradiation environment of a californium (Cf)-252 (average energy 2.45 MeV) neutron source.
[0087] The overall quality of the Mg / Ta layered composite material prepared in Comparative Example 1 is good, but the neutron shielding efficiency is only 78%, indicating that the planar porosity of the Ta mesh is a key factor affecting the shielding effect.
[0088] In comparative example 2, when the preform was cut open, it was found that the voids in the composite material were not completely filled and there were obvious pore defects, which resulted in a poor yield strength of ~130 MPa, indicating that the use of sparse pores is a necessary condition to ensure complete filling of the molten Mg liquid.
[0089] In comparative example 3, the preform was cut open and it was found that there was no diffusion behavior at the Mg-Ta interface. SEM revealed that there were holes at the Mg / Ta interface, and the yield strength was ~200 MPa, indicating that the intermediate Al layer can effectively improve the bonding ability of Mg-Ta.
[0090] In comparative example 4, the surface and internal quality of the Mg matrix in the Mg-Ta composite material are intact, and the overall yield strength of the Mg / Ta composite material is ~150 MPa, indicating that heat treatment is a key factor in releasing the stress of the three-dimensional interpenetrating network structure and further improving its strength.
[0091] Obviously, the above embodiments are merely examples for clear explanation, and are not intended to limit the embodiments. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. The obvious changes or modifications derived from them are still within the protection scope of the invention.
Claims
1. A preparation method of a Mg-Ta composite material, characterized in that the Mg-Ta composite material is composed of a Ta preform with an aluminum coating on its surface and a Mg alloy; the Ta preform is composed of n layers of Ta wire meshes stacked in sequence, with adjacent two layers of Ta wire meshes spaced apart, n≥5, the Ta wire meshes are all honeycomb structures, and taking any one layer of Ta wire mesh as a reference, in the direction perpendicular to this Ta wire mesh, the hexagonal holes of this Ta wire mesh are blocked by the edges of the hexagons of the remaining n-1 layers of Ta wire meshes in terms of space; the Mg alloy fills the voids of the Ta preform with an aluminum coating on its surface in space, forming a three-dimensional interpenetrating network structure with the Ta preform with an aluminum coating on its surface; the edge width a of each hexagon of the Ta wire mesh is 0.5-1 mm, the side length b satisfies 1 mm < b ≤ 2(n-1)×a, the perpendicular distance between two parallel sides ≤ (n-1)×a, the layer spacing of the n layers of Ta wire meshes is 0.5-1 mm, and the stacking direction forms an angle θ = 90° ± 30° with any one side of the hexagon of the reference Ta wire mesh; The preparation method includes the following steps: S1. Establish a three-dimensional model of the Ta preform; S2. According to the three-dimensional model of the Ta preform in step S1, prepare the Ta preform by metal fiber wire weaving technology or 3D printing technology: S3. Perform surface pretreatment on the Ta preform to remove the surface oxide layer and impurities: S4. Immerse the pretreated Ta preform in molten pure aluminum liquid for immersion plating treatment to obtain a Ta preform with an aluminum coating on its surface: S5. Weigh the components according to the content of each component in the Mg alloy, and under the protection of an inert atmosphere, perform vacuum melting to obtain molten Mg liquid: S6. Immerse the Ta preform with an aluminum coating on its surface in the molten Mg liquid, keep it warm, and then cool it to obtain a Mg-Ta composite structure: S7. Perform machining treatment on the Mg-Ta composite structure to remove the excess Mg alloy outside the Mg-Ta composite structure, and perform heat treatment according to the solution aging heat treatment process of the Mg alloy in step S5 to obtain the Mg-Ta composite material.
2. The preparation method of a Mg-Ta composite material according to claim 1, characterized in that the Mg alloy is a Mg-Gd-Y series alloy.
3. The preparation method of a Mg-Ta composite material according to claim 2, characterized in that the Mg-Gd-Y series alloy is Mg-10Gd-3Y-0.5Zr.
4. The method for preparing a Mg-Ta composite material according to claim 1, characterized in that: In step S3, the Ta preform is put into tantalum acid cleaning solution for chemical cleaning for 0.5-2 min.
5. The preparation method of a Mg-Ta composite material according to claim 1, characterized in that in step S4, the pretreated Ta preform is put into molten pure aluminum liquid for 10-20 min; in step S5, the melting temperature is 650-730 °C.
6. The method for preparing a Mg-Ta composite material according to claim 1, characterized in that: In step S6, the Ta preform with an aluminum coating on its surface is placed in a mold, under the protection of an inert atmosphere, the molten Mg liquid is introduced into the mold, after keeping it warm at 650 °C for 10-30 min, it is naturally cooled to form a Mg-Ta composite structure.
7. The method for preparing a Mg-Ta composite material according to claim 1, characterized in that: In step S7, the heat treatment conditions are: firstly treating at 500-525° C. for 8-12 h, and then treating at 250° C. for 12 h.
8. Use of the Mg-Ta composite material obtained according to the preparation method according to any one of claims 1 to 7 as a radiation-resistant lightweight composite material.