A TPU supercritical foaming material and method for preparing shoe midsole
By blending polyols, isocyanates and supercritical gases in the twin-screw extruder and directly injection molding, the problems of stress and cutting waste in TPU particles were solved, and a low specific gravity, adjustable hardness and good elasticity were prepared. TPU supercritical foam shoe midsole reduces production costs and improves performance.
Patent Information
- Application Number
- CN202410088184.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-22
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-01-22
AI Technical Summary
When preparing the shoe midsole, the internal stress of TPU particles and the waste of material caused by cutting, resulting in inconsistent lateral and longitudinal magnifications of the products, low bending deformation and yield, and high production costs.
Blend and supercritical foaming using polyols, isocyanates, chain extenders and supercritical gases (such as carbon dioxide, nitrogen, and air) for direct injection molding, avoiding the preparation steps of TPU particles, and using a twin-screw extruder to complete the raw materials Mix and react, and use a variety of supercritical mixed gases to improve solubility and foaming ratio.
The prepared TPU supercritical foamed material shoes have low specific gravity, adjustable hardness, good elasticity, avoid internal stress and cutting waste, reduce production costs, and improve product yield and performance.
Smart Images

Figure CN117777404B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of foaming materials, and more specifically, to a TPU supercritical foaming material and a method for preparing a shoe midsole. Background Art
[0002] Polyurethane foam materials are usually divided into thermosetting polyurethane foam materials and thermoplastic polyurethane foam materials according to the characteristics of the raw materials and the molecular structure of the end product. Traditional thermosetting polyurethane foaming usually uses polyols and isocyanates to react chemically while introducing water into the system as a foaming agent to prepare the foam material. However, the above materials and methods often produce open-cell foam structures, such as sponges. Due to their relatively poor physical and mechanical properties, thermosetting polyurethane materials have not been widely used in the field of high-performance sports shoe midsoles.
[0003] Thermoplastic polyurethane elastomer (TPU for short) has been used in traditional sports shoe midsoles due to its good processing properties. The existing invention patent application with publication number CN105884998A discloses a method for preparing a foamed thermoplastic polyurethane elastomer material, and its technical route requires two extrusions. The product specific gravity of this method is above 0.165g / cc, and the product morphology is foamed beads, which are then molded to form a midsole. The existing invention patent application with publication number CN102276785A discloses a low-density foamed thermoplastic polyurethane elastomer and its preparation process, which uses polyols, chain extenders, isocyanates, azo foaming agents, etc. to prepare samples. The density of the samples prepared by this method is above 0.26g / cc, and a chemical foaming agent is used to realize the foaming process.
[0004] The existing supercritical foaming midsole solutions mainly include four categories: 1. Prepare TPU beads first, and then use the beads for compression molding; 2. After the raw materials are blended, they are injected / cast to obtain a small embryo, and then supercritical autoclave foaming is performed; 3. After the sheet is extruded, supercritical foaming is performed, and the desired shape is cut to make the midsole; 4. Supercritical fluid is added during the injection molding process, and the product is obtained by opening the mold. For the above solutions, when TPU particles are used for injection molding and foaming, the foamed products under the influence of oriented internal stress will show problems such as inconsistent lateral and longitudinal ratios, bending deformation, and low yield; or the cutting technical solution will produce large waste and low utilization rate. Summary of the invention
[0005] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a TPU supercritical foaming material and method for preparing shoe midsoles, which does not go through the step of preparing TPU particles, avoids the adverse effects of the internal stress of TPU particles, and does not cause waste of raw materials caused by cutting.
[0006] To achieve the above object, the present invention provides the following technical solution: a TPU supercritical foaming material for preparing a shoe midsole, the material comprising the following raw materials in parts by weight:
[0007] (1) 40-80 parts of polyol;
[0008] (2) 20-50 parts of isocyanate;
[0009] (3) 4-12 parts of chain extender;
[0010] (4) 0.1-30 parts of a modifier;
[0011] (5)Supercritical gas.
[0012] Furthermore, the polyol is a bifunctional polyol, including but not limited to a mixture of one or more of polyester polyols, polyether polyols, polycaprolactone, polycarbonate, and bio-based diols.
[0013] Furthermore, the isocyanate is a difunctional isocyanate, including but not limited to aromatic, aliphatic or alicyclic isocyanates.
[0014] Further, the isocyanate is a difunctional isocyanate, including but not limited to a mixture of one or more of diphenylmethane diisocyanate, toluene diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, dicyclohexylmethane-4,4'-diisocyanate, xylylene diisocyanate, tetramethyl metaxylylene diisocyanate, lysine diisocyanate, p-phenylene diisocyanate, and cyclohexane-1,4-diisocyanate.
[0015] Furthermore, the molar ratio of isocyanate functional group (-NCO) to alcohol hydroxyl functional group (-OH) is (0.7-1.5):1.
[0016] Furthermore, the chain extender is a difunctional alcohol, including but not limited to a mixture of one or more of ethylene glycol, 1,2-propylene glycol, 1,4-butanediol, and 1,6-hexanediol.
[0017] Furthermore, the modifier includes but is not limited to one or more of a masterbatch, a coupling agent, a toughening agent, and a filler.
[0018] Furthermore, the supercritical gas is a mixed gas of two or more of carbon dioxide, nitrogen, air and water vapor.
[0019] Furthermore, a method for preparing a TPU supercritical foaming material using the above raw materials comprises the following steps:
[0020] S1, mixing the above-mentioned polyol, isocyanate and chain extender in parts by weight and putting them into a twin-screw extruder for blending to obtain a polymer melt;
[0021] S2, preparing a supercritical gas through an air intake system, and injecting the supercritical gas and a polymer melt into a single screw extruder to prepare a molten mixture containing the supercritical gas;
[0022] S3, injecting the molten mixture into a mold, letting it stand, and opening the mold to obtain.
[0023] Furthermore, a modifier may be added in step S1, and the modifier includes but is not limited to one or more of a masterbatch, a coupling agent, a toughening agent, and a filler.
[0024] Furthermore, the mold working parameters of step S3 are pressure 5-20 MPa, standing at 30-150° C. for 30 s-2 h.
[0025] In summary, the present invention has the following beneficial effects:
[0026] Due to the method of the present invention, the steps do not include the preparation of TPU particles. The raw materials of the components and weight parts of the present invention are blended and reacted in a twin-screw extruder, and a polymer with a predetermined hardness and resilience is obtained by bulk polymerization, thereby avoiding the internal stress of TPU particles. The present invention adopts two or more supercritical mixed gases to avoid the defects of limited solubility and diffusivity of a single supercritical fluid in a polymer. The use of supercritical mixed gases can increase the solubility of the supercritical fluid in the polymer, and the foaming ratio of the prepared product is increased, and the specific gravity is lower. The shoe midsole of the TPU supercritical foaming material prepared by the present invention has a specific gravity of 0.06-0.2g / cc and a hardness range of 10-50Asker C. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 1 is a graph showing the relationship between torque and time of the TPU of each embodiment of the present invention and the comparative example during kneading in a Haake rheometer. In the graph, the blue curve is Example 1; the green curve is Example 2; and the red curve is
[0028] Embodiment 3;
[0029] Figure 2 1 and 2 are SEM images of the foamed midsoles of the embodiments and comparative examples of the present invention, wherein a: embodiment 1; b: embodiment 2; c: embodiment 3; d: comparative example 1; and e: comparative example 2. DETAILED DESCRIPTION
[0030] The present invention is further described in detail below with reference to the embodiments.
[0031] Embodiment 1:
[0032] 60 parts of polytetramethylene ether glycol, 6 parts of 1,4-butanediol, 32 parts of MDI-100, hard segment content 38%, NCO coefficient 1.01; after mixing the above raw materials, put them into a twin-screw extruder, blend them at 180°C to obtain a polymer melt; the air intake system is set to CO2:N2 at 10:90, and supercritical gas and polymer melt are injected into a single-screw extruder to prepare a molten mixture containing supercritical gas; then it is injected into a mold at 40°C, and after maintaining the pressure for 30 minutes, the mold is opened to release the pressure to obtain a midsole product.
[0033] Embodiment 2:
[0034] 60 parts of polytetramethylene ether glycol, 8 parts of 1,4-butanediol, 38 parts of MDI-100, hard segment content 43%, NCO coefficient 1.01; after mixing the above raw materials, put them into a twin-screw extruder, blend them at 190°C to obtain a polymer melt; the air intake system is set to CO2:N2 at 10:90, and supercritical gas and polymer melt are injected into a single-screw extruder to prepare a molten mixture containing supercritical gas; then it is injected into a mold at 40°C, and after maintaining the pressure for 25 minutes, the mold is opened to release the pressure to obtain a midsole product.
[0035] Embodiment 3:
[0036] 60 parts of polytetramethylene ether glycol, 10 parts of 1,4-butanediol, 44 parts of MDI-100, hard segment content 47%, NCO coefficient 1.01; after mixing the above raw materials, put them into a twin-screw extruder, blend them at 200°C to obtain a polymer melt; the air intake system is set to CO2:N2 at 10:90, and supercritical gas and polymer melt are injected into a single-screw extruder to prepare a molten mixture containing supercritical gas; then it is injected into a mold at 40°C, and after maintaining the pressure for 20 minutes, the mold is opened to release the pressure to obtain a midsole product.
[0037] Comparative Example 1: A TPU two-step autoclave foaming midsole according to the invention patent application publication number CN 108081652 A.
[0038] Comparative Example 2: A midsole is obtained by cutting, grinding and secondary molding of the TPU sheet foam material according to the invention patent application publication number CN110524781A.
[0039] Performance testing
[0040] The hardness, rebound and specific gravity of the embodiments of the present invention and the comparative examples were tested in the following manner:
[0041] Hardness: Tested according to ASTM D2240;
[0042] Rebound: Tested according to DIN 53512;
[0043] Specific gravity: tested according to ISO 845-2006;
[0044] The test results are shown in Table 1.
[0045] Table 1 Performance test results of various embodiments and comparative examples
[0046] name Hardness (Asker C) Rebound(%) Specific gravity (g / cc) Example 1 29 74 0.08 Example 2 36 75 0.10 Example 3 45 70 0.12 Comparative Example 1 35 70 0.13 Comparative Example 2 40 70 0.15
[0047] As can be seen from Table 1, the hardness of the shoe midsole prepared in the embodiment of the present invention is adjustable, the hardness ranges from 20 to 50 Asker C, the specific gravity is low, the specific gravity does not exceed 0.12 g / cc, and it has good resilience; while the shoe midsoles of Comparative Examples 1 and 2 have a large specific gravity and poor resilience.
[0048] The intermediate polymer melt of each embodiment of the present invention was tested using a Haake rheometer. The Haake rheometer was set to have the temperatures of zone 1, zone 2, and zone 3 at 120°C, 120°C, and 120°C, respectively, and a rotation speed of 60 rpm. The results are shown in FIG. Figure 1 . Figure 1 The different torque peaks represent the different hardness of the material, and the different times of torque reduction represent the melting rate of the material, which in turn reflects the different melting points of the material. Figure 1 It can be seen that: the raw materials of Examples 1-3 are added with MDI hard segment components with increasing contents, and the hardness of the intermediate products obtained after the reaction increases successively; it is precisely because of the increase in the hard segment content that the energy required to melt the material is higher, so the melting point of the material is also increased successively; by adjusting the MDI hard segment content of the raw material, the hardness of the product can be flexibly adjusted to expand the application range of the product; the sample of Example 1 reflects a lower torque and the lowest hardness at the initial stage; the samples of Examples 2 and 3 have similar initial torques, but the inflection point of Example 2 comes earlier and the melting temperature is lower than that of Example 3. It can be analyzed that the hardness and melting point of the samples of Examples 1, 2, and 3 increase successively, which is consistent with the expectation of adjusting the hardness by the MDI hard segment content of the raw material.
[0049] Depend on Figure 2 It can be seen that the TPU supercritical foaming material of the present invention is used to prepare the shoe midsole, and the pore structure is uniform and dense, which is significantly better than the TPU midsole prepared by the two-step method in comparative example 1, and comparable to the sheet foaming and cutting midsole in comparative example 2; although the sheet foaming and cutting midsole can reduce the problem of oriented internal stress, the production steps require first making the foamed sheet, and then cutting the sheet into the required sole shape, and performing secondary molding, and the sheet cutting greatly increases the production cost, wastes cutting scraps, and has high cutting machinery costs; the shoe midsole of the present invention has similar product performance to that of comparative document 2, avoids material waste caused by cutting, does not require cutting equipment, and greatly reduces production costs.
[0050] The steps of the present invention do not include the preparation of TPU particles. The raw materials of the components and weight parts of the present invention are blended and reacted in a twin-screw extruder, and a polymer with a predetermined hardness and resilience is obtained by bulk polymerization, thereby avoiding the internal stress of the TPU particles, thereby reducing the deformation of the prepared shoe midsole and improving the yield rate of the product. The present invention adopts two or more supercritical mixed gases to avoid the defects of limited solubility and diffusivity of a single supercritical fluid in a polymer. The use of the supercritical mixed gas can increase the solubility of the supercritical fluid in the polymer, and the foaming ratio of the prepared product is increased, and the specific gravity is lower. The shoe midsole of the TPU supercritical foaming material prepared by the present invention has a specific gravity of 0.06-0.2, a hardness range of 10-50, good resilience, excellent performance, and does not require cutting with conventional technology, thereby reducing waste and saving costs.
[0051] This specific embodiment is merely an explanation of the present invention and is not a limitation of the present invention. After reading this specification, those skilled in the art may make non-creative modifications to the present embodiment as needed. However, as long as they are within the scope of the claims of the present invention, they are protected by the patent law.
Claims
1. A TPU supercritical foaming material for preparing a shoe midsole, characterized in that: The material comprises the following raw materials in parts by weight: (1) 40-80 parts of polyol; (2) 20-50 parts of isocyanate; (3) 4-12 parts of chain extender; (4) 0.1-30 parts of modifier; (5) Supercritical gas; The supercritical gas is a mixed gas of two or more of carbon dioxide, nitrogen, air and water vapor; The preparation method comprises the following steps: S1, mixing polyol, isocyanate and chain extender according to weight parts and putting them into a twin-screw extruder for blending to obtain a polymer melt; S2, preparing a supercritical gas through an air intake system, and injecting the supercritical gas and a polymer melt into a single screw extruder to prepare a molten mixture containing the supercritical gas; S3, injecting the molten mixture into a mold, letting it stand, and opening the mold to obtain.
2. The TPU supercritical foaming material for preparing a shoe midsole according to claim 1, characterized in that: The polyol is a difunctional polyol, including but not limited to a mixture of one or more of polyester polyol, polyether polyol and bio-based diol.
3. The TPU supercritical foaming material for preparing a shoe midsole according to claim 2, characterized in that: The isocyanate is a difunctional isocyanate, including but not limited to aromatic, aliphatic or alicyclic isocyanates.
4. The TPU supercritical foaming material for preparing a shoe midsole according to claim 1, characterized in that: The isocyanate is a difunctional isocyanate, including but not limited to a mixture of one or more of diphenylmethane diisocyanate, toluene diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, dicyclohexylmethane-4,4'-diisocyanate, xylylene diisocyanate, tetramethyl metaxylylene diisocyanate, lysine diisocyanate, p-phenylene diisocyanate, and cyclohexane-1,4-diisocyanate.
5. The TPU supercritical foaming material for preparing shoe midsoles according to claim 3, characterized in that: The molar ratio of isocyanate functional group -NCO to alcohol hydroxyl functional group -OH is (0.7-1.5):
1.
6. The TPU supercritical foaming material for preparing a shoe midsole according to claim 1, characterized in that: The chain extender is a difunctional alcohol, including but not limited to a mixture of one or more of ethylene glycol, 1,2-propylene glycol, 1,4-butanediol, and 1,6-hexanediol.
7. The TPU supercritical foaming material for preparing a shoe midsole according to claim 1, characterized in that: The modifier includes but is not limited to one or more of a masterbatch, a coupling agent, a toughening agent, and a filler.
8. The TPU supercritical foaming material for preparing shoe midsoles according to claim 1, characterized in that: The mold working parameters in step S3 are pressure 5-20 MPa and standing at 30-150° C. for 30 seconds to 2 hours.
Citation Information
Patent Citations
Low-density foamed thermoplastic polyurethane elastomer and its preparation process
CN102276785A
Foamed type TPU (thermoplastic polyurethane elastomer) material and preparation method thereof
CN105884998A
Preparation process of supercritical foaming sole
CN108081652A
TPU sheet foaming process
CN110524781A
E-TPU elastomer material and preparation method thereof
CN113307942A