A method for preparing oxygen-free copper rod

By adjusting the smelting furnace structure and nitrogen delivery method during the preparation process of the oxygen-free copper rod, combined with the covering layer treatment in the holding furnace, the oxygen content of the oxygen-free copper rod was successfully reduced, the electrical conductivity and tensile strength were improved, and the problem was solved The problem of high oxygen content in the existing technology meets the high performance needs of special fields.

CN117816917BActive Publication Date: 2024-10-01JIANG SU DONG HENG PHOTOELECTRICITY CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202311855323.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-29
Publication Date
2024-10-01
Estimated Expiration
2043-12-29

AI Technical Summary

Technical Problem

The existing oxygen-free copper rods have high oxygen content, resulting in low electrical conductivity and reduced tensile strength, and cannot meet the needs for low oxygen content and high performance in special fields.

Method used

By adjusting the structure of the smelting furnace, increasing the distribution of ventilation pipes and nitrogen delivery methods, and using chestnut charcoal and flake graphite coverings in the holding furnace to remove oxygen from the copper liquid, combined with the adjustment of process parameters, the content of the oxygen-free copper rods was controlled. The oxygen content is below 1ppm, which improves the conductivity and tensile strength.

Benefits of technology

The oxygen content of the oxygen-free copper rod is controlled in a low range, with high conductivity, high tensile strength and good stability. It meets the high requirements of special fields and is easy to promote and apply.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004642062400000091
    Figure BDA0004642062400000091
  • Figure BDA0004642062400000101
    Figure BDA0004642062400000101
Patent Text Reader

Abstract

The invention relates to the field of preparation of oxygen-free copper rods, and specifically provides a method for preparing the oxygen-free copper rod. The main steps include baking, smelting, heat preservation and condensation of electrolytic copper plate raw materials into solids, and upper copper rods. The invention specifically adjusts the structure of a smelting furnace, and a plurality of ventilation pipes are evenly distributed at intervals on the bottom and peripheral walls of the smelting furnace. During the smelting process, the plurality of ventilation pipes at the bottom of the smelting furnace extend into the copper liquid, and nitrogen is continuously introduced into the copper liquid. After the smelting is completed, the ventilation pipes arranged on the bottom and peripheral walls of the smelting furnace are opened at the same time to transport nitrogen into the copper liquid. In this way, oxygen in the copper liquid can be well removed. Then, a layer of chestnut charcoal is first covered on the top surface of the copper liquid in the heat preservation furnace. Studies have found that the chestnut charcoal can well eliminate oxygen in the copper liquid. The oxygen content of the oxygen-free copper rod of the invention can be controlled to be below 1 ppm, and the oxygen-free copper rod has high electrical conductivity, high tensile strength and good stability, meets higher requirements in special fields, and is convenient for popularization and application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the preparation of an oxygen-free copper rod, in particular to a method for preparing the oxygen-free copper rod, and in particular to an oxygen-free copper rod and a preparation method and application thereof. Background Art

[0002] Oxygen-free copper rod is a copper material that does not contain oxygen or any deoxidizer residue. According to the standard, the oxygen content is not more than 0.02%, the total impurity content is not more than 0.05%, and the copper purity is greater than 99.95%. Due to its good electrical conductivity, thermal conductivity and corrosion resistance, it is widely used in wind power wires, nuclear power wires, automotive wires or aerospace fields.

[0003] The oxygen content in oxygen-free copper rod is a key factor affecting its quality. When the oxygen content is too high, the process performance of oxygen-free copper rod deteriorates, which is manifested as a significant increase in the rate of broken rods and wires during casting and stretching. This is because oxygen can react with copper to form a brittle phase of cuprous oxide, forming a copper-cuprous oxide eutectic, which is distributed on the surface in a network structure. This brittle phase has high hardness and will separate from the copper body during cold deformation, resulting in a decrease in the mechanical properties of the copper rod, which is prone to breakage in subsequent processing. In addition, high oxygen content can also lead to a decrease in the conductivity and tensile strength of the oxygen-free copper rod. At present, the content standard of domestic oxygen-free copper rod products will be controlled below 10ppm, but with the continuous improvement of industrial technology, the domestic requirements for oxygen-free copper rods are constantly increasing. In some special fields, there is a demand for oxygen-free copper rods with an oxygen content lower than 1ppm. The conventional oxygen-free copper rods in the existing technology have a high oxygen content and cannot meet this requirement. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing an oxygen-free copper rod in view of the problem that the oxygen-free copper in the prior art has a high oxygen content and a low electrical conductivity. The method improves the structure of a smelting furnace, adjusts the nitrogen delivery method, adjusts the copper liquid covering layer material in a holding furnace and adjusts other process parameter ranges, so that the oxygen content of the prepared oxygen-free copper rod is controlled within a low range, the electrical conductivity is high, the tensile strength is high, the stability is good, and it is easy to promote and apply.

[0005] In order to achieve the above object, the technical solution adopted by the present invention is:

[0006] A method for preparing an oxygen-free copper rod comprises the following steps:

[0007] Step 1, heating the smelting furnace to above 1160°C for standby use;

[0008] Step 2: Hang the electrolytic copper plate raw material above the red charcoal at the furnace mouth for baking and drying;

[0009] Step 3, quickly transport the dried electrolytic copper plate to the smelting furnace, and keep the smelting furnace in a vacuum state for smelting; a plurality of vent pipes are evenly spaced on the bottom and the surrounding wall of the smelting furnace; during the smelting process, the plurality of vent pipes at the bottom of the smelting furnace extend into the copper liquid, and nitrogen is continuously introduced into the copper liquid, and at the same time, the gas is extracted from the top of the smelting furnace until the smelting is completed;

[0010] Step 4: After the smelting is completed, the vent pipes arranged at the bottom and the surrounding wall of the smelting furnace are opened at the same time to deliver nitrogen to the copper liquid, and at the same time, the gas is discharged from the top of the smelting furnace;

[0011] Step 5, transporting the copper liquid obtained in step 4 to a holding furnace through a melting ditch, wherein the top surface of the copper liquid is sequentially covered with chestnut charcoal having a thickness of more than 12 cm and flake graphite having a thickness of more than 2.5 cm from bottom to top;

[0012] Step 6, insert the hollow crystallizer into the copper liquid in the holding furnace, and the copper liquid enters the central control crystallizer and is condensed into a solid using circulating water; the solid is led to the copper rod by the traction device;

[0013] Step 7: The wire is coiled on a winding machine via a wire dividing rod to prepare an oxygen-free copper rod.

[0014] The present invention provides a method for preparing oxygen-free copper rods, the main steps of which include baking, smelting, heat preservation and condensation of electrolytic copper plate raw materials into solids, and upper copper rods. The present invention specifically adjusts the structure of the smelting furnace, and a plurality of ventilation pipes are evenly distributed at intervals on the bottom and the peripheral wall of the smelting furnace; during the smelting process, the plurality of ventilation pipes at the bottom of the smelting furnace extend into the copper liquid, and nitrogen is continuously introduced into the copper liquid. The gas is extracted from the top of the smelting furnace. After the smelting is completed, the ventilation pipes arranged on the bottom and the peripheral wall of the smelting furnace are opened at the same time to transport nitrogen to the copper liquid. Nitrogen, at the same time, the gas is discharged from the top of the smelting furnace. In this way, the oxygen in the copper liquid can be well removed. Then, the top surface of the copper liquid in the insulation furnace is covered with a layer of chestnut charcoal. Studies have found that chestnut charcoal can better eliminate the oxygen in the copper liquid. Then, a layer of flake graphite is covered to block the air. By adjusting the range of other process parameters, the oxygen content of the prepared oxygen-free copper rod is controlled below 1ppm, with high electrical conductivity, high tensile strength and good stability, which meets the higher requirements of special fields and is easy to promote and apply.

[0015] Furthermore, in step 1, the temperature of the smelting furnace is maintained at 1160°C to 1250°C.

[0016] Furthermore, in step 2, the electrolytic copper plate raw material is baked for 3-5 minutes. The electrolytic copper plate is dried before smelting, especially in a humid and rainy environment, as the dried raw material can prevent oxidation during the production process.

[0017] Furthermore, in step 3, the bottom and surrounding walls of the smelting furnace are covered with the ventilation pipes, and the interval between adjacent ventilation pipes is 10 to 20 cm.

[0018] Furthermore, in step 3 and / or step 4, the length of the vent pipe at the bottom of the smelting furnace extending into the molten copper accounts for 5% to 15% of the height of the molten copper; the length of the vent pipe on the peripheral wall of the smelting furnace extending into the molten copper accounts for 5% to 15% of the distribution width of the molten copper; and the pressure of the nitrogen in the vent pipe is 2.5 bar to 4.5 bar.

[0019] Furthermore, in step 4, nitrogen is delivered for 25 to 40 minutes.

[0020] Through experimental research, it was found that the deoxidation effect is closely related to factors such as the distribution and spacing of the vent pipes in the smelting furnace, and the method of passing nitrogen twice during and after smelting. Changing the layout of the vent pipes in the furnace and the method of passing nitrogen will increase the oxygen content in the oxygen-free copper rod, reduce the tensile strength, and reduce the stability.

[0021] Furthermore, in step 5, the top surface of the copper liquid is covered with chestnut charcoal with a thickness of 12 to 15 cm and flake graphite with a thickness of 2.5 to 4 cm from bottom to top.

[0022] The study found that compared with conventional charcoal on the market, chestnut charcoal can better eliminate oxygen in the copper liquid, and the oxygen-free copper rod prepared has a lower oxygen content.

[0023] Furthermore, the particle size of the chestnut charcoal and the particle size of the flake graphite are 320 mesh to 350 mesh.

[0024] Furthermore, in step 5, the insulation temperature is 1185°C to 1220°C; in step 6, the inlet temperature of the circulating cooling water in the hollow crystallizer is 25 to 28°C, and the temperature difference between the inlet and outlet cooling water is 5 to 8°C; in step 6, the pulling speed is 25 to 120 mm / min, and the diameter of the prepared oxygen-free copper rod is 8 to 15 mm.

[0025] The insulation temperature, the temperature of the cooling water in the hollow crystallizer, the temperature difference between the cooling inlet and outlet water, and the pulling speed are all key factors affecting the quality of oxygen-free copper rods. If the process parameters are not adjusted properly, there may be a risk of coarse crystals, loose structure, and even broken rods.

[0026] Another object of the present invention is to provide a product prepared by the above oxygen-free copper rod preparation method.

[0027] An oxygen-free copper rod prepared by the above method for preparing an oxygen-free copper rod.

[0028] The oxygen-free copper rod prepared by the invention has an oxygen content controlled within a relatively low range, has high electrical conductivity, good stability, and is easy to promote and apply.

[0029] Another object of the present invention is to provide application of the oxygen-free copper rod.

[0030] As mentioned above, oxygen-free copper rods are used in wind power lines, nuclear power lines and automotive lines.

[0031] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are:

[0032] 1. The present invention provides a method for preparing an oxygen-free copper rod, the main steps of which include baking, smelting, heat preservation, condensation of electrolytic copper plate raw materials into solids, and upper copper rods. The present application specifically adjusts the structure of the smelting furnace, and a plurality of vents are evenly spaced at the bottom and the surrounding wall of the smelting furnace; during the smelting process, the plurality of vents at the bottom of the smelting furnace extend into the copper liquid, and nitrogen is continuously introduced into the copper liquid, and the gas is extracted from the top of the smelting furnace. After the smelting is completed, the vents arranged on the bottom and the surrounding wall of the smelting furnace are opened at the same time to transport nitrogen to the copper liquid, and at the same time, the gas is discharged from the top of the smelting furnace. In this way, the oxygen in the copper liquid can be well removed, and then the top surface of the copper liquid in the heat preservation furnace is first covered with a layer of chestnut charcoal. Studies have found that chestnut charcoal can better eliminate oxygen in the copper liquid, and then a layer of flake graphite is covered to block the air, and then the oxygen content of the prepared oxygen-free copper rod is controlled below 1ppm by adjusting the range of other process parameters.

[0033] 2. The oxygen content of the oxygen-free copper rod prepared by the present invention is controlled in a relatively low range, and the electrical conductivity is high, the tensile strength is high, the stability is good, and it is easy to promote and apply.

[0034] 3. The present invention provides the application of oxygen-free copper rods in wind power lines, nuclear power lines and automotive lines. DETAILED DESCRIPTION

[0035] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0036] The following examples and comparative examples use electrolytic copper plate raw materials from the same batch with the same specifications, a purity of 99.95% and an oxygen content of 300 ppm.

[0037] Example 1

[0038] Preparation of oxygen-free copper rod

[0039] Step 1, heat the smelting furnace to 1200±5℃ and set aside;

[0040] Step 2: Hang the electrolytic copper plate raw material above the red charcoal at the furnace mouth and bake it for 4 minutes to dry;

[0041] Step 3, quickly transport the dried electrolytic copper plate to the smelting furnace, and keep the smelting furnace in a vacuum state for smelting; a plurality of vent pipes are evenly spaced on the bottom and the surrounding wall of the smelting furnace, and the interval between adjacent vent pipes is 15 cm; during the smelting process, the plurality of vent pipes at the bottom of the smelting furnace extend into the molten copper, and nitrogen is continuously introduced into the molten copper. The length of the vent pipe at the bottom of the smelting furnace extending into the molten copper accounts for 10% of the height of the molten copper, the pressure of the nitrogen is 3 bar, and the flow rate of the nitrogen is adjusted to 2.5 Nm 3 / h, and at the same time, the gas is extracted from the top of the smelting furnace until the smelting is completed;

[0042] Step 4: After smelting is completed, the bottom and the ventilation pipes arranged on the peripheral wall of the smelting furnace are opened at the same time to transport nitrogen to the copper liquid for 30 minutes. At the same time, the gas is discharged from the top of the smelting furnace; wherein, the length of the ventilation pipe on the peripheral wall of the smelting furnace extending into the copper liquid accounts for 10% of the distribution width of the copper liquid, and the nitrogen transportation in the ventilation pipe at the bottom of the smelting furnace is consistent with step 3, the pressure of nitrogen in the ventilation pipe on the peripheral wall of the smelting furnace is 2.8 bar, and the flow rate of nitrogen is adjusted to 2Nm 3 / h, subject to ensuring that nitrogen can be discharged stably.

[0043] Step 5, the copper liquid obtained in step 4 is transported to a holding furnace through a melting ditch, the holding temperature is 1200° C., and the top surface of the copper liquid is covered with 13 cm thick chestnut charcoal and 3 cm thick flake graphite from bottom to top;

[0044] Step 6, extend the hollow crystallizer into the copper liquid in the insulation furnace, the copper liquid enters the central control crystallizer and is condensed into a solid using circulating water, the inlet temperature of the circulating cooling water in the hollow crystallizer is 27°C, and the temperature difference between the cooling inlet and outlet water is 6°C; the solid is led to a copper rod through a traction device, the traction speed is 80mm / min, and the diameter of the prepared oxygen-free copper rod is 10mm.

[0045] Example 2

[0046] Preparation of oxygen-free copper rod

[0047] Step 1, heating the smelting furnace to 1160°C for standby use;

[0048] Step 2: Hang the electrolytic copper plate raw material above the red charcoal at the furnace mouth and bake it for 3 minutes to dry;

[0049] Step 3, quickly transport the dried electrolytic copper plate to the smelting furnace, and keep the smelting furnace in a vacuum state for smelting; a plurality of vent pipes are evenly spaced on the bottom and surrounding wall of the smelting furnace, and the interval between adjacent vent pipes is 10 cm; during the smelting process, the plurality of vent pipes at the bottom of the smelting furnace extend into the molten copper, and nitrogen is continuously introduced into the molten copper. The length of the vent pipe at the bottom of the smelting furnace extending into the molten copper accounts for 5% of the height of the molten copper, the pressure of the nitrogen is 4 bar, and the flow rate of the nitrogen is adjusted to 3 Nm 3 / h, and at the same time, the gas is extracted from the top of the smelting furnace until the smelting is completed;

[0050] Step 4: After smelting is completed, the bottom and the ventilation pipes arranged on the peripheral wall of the smelting furnace are opened at the same time to transport nitrogen to the copper liquid for 40 minutes. At the same time, the gas is discharged from the top of the smelting furnace; wherein, the length of the ventilation pipe on the peripheral wall of the smelting furnace extending into the copper liquid accounts for 5% of the distribution width of the copper liquid, and the nitrogen transportation situation in the ventilation pipe at the bottom of the smelting furnace is consistent with step 3, the pressure of nitrogen in the ventilation pipe on the peripheral wall of the smelting furnace is 4.5 bar, and the flow rate of nitrogen is adjusted to 2.5 Nm 3 / h, subject to ensuring that nitrogen can be discharged stably.

[0051] Step 5, conveying the copper liquid obtained in step 4 to a holding furnace through a melting ditch, the holding temperature being 1185° C., and the top surface of the copper liquid is sequentially covered with chestnut charcoal with a thickness of 12 cm and flake graphite with a thickness of 4 cm from bottom to top;

[0052] Step 6, extend the hollow crystallizer into the copper liquid in the insulation furnace, the copper liquid enters the central control crystallizer and is condensed into a solid using circulating water, the inlet temperature of the circulating cooling water in the hollow crystallizer is 25°C, and the temperature difference between the cooling inlet and outlet water is 5°C; the solid is led to a copper rod through a traction device, the traction speed is 120mm / min, and the diameter of the prepared oxygen-free copper rod is 15mm.

[0053] Example 3

[0054] Preparation of oxygen-free copper rod

[0055] Step 1, heating the smelting furnace to 1250°C for standby use;

[0056] Step 2: Hang the electrolytic copper plate raw material above the red charcoal at the furnace mouth and bake it for 5 minutes to dry;

[0057] Step 3, quickly transport the dried electrolytic copper plate to the smelting furnace, and keep the smelting furnace in a vacuum state for smelting; a plurality of vent pipes are evenly spaced on the bottom and surrounding wall of the smelting furnace, and the interval between adjacent vent pipes is 20 cm; during the smelting process, the plurality of vent pipes at the bottom of the smelting furnace extend into the molten copper, and nitrogen is continuously introduced into the molten copper. The length of the vent pipe at the bottom of the smelting furnace extending into the molten copper accounts for 15% of the height of the molten copper, the pressure of the nitrogen is 2.5 bar, and the flow rate of the nitrogen is adjusted to 1.8 Nm 3 / h, and at the same time, the gas is extracted from the top of the smelting furnace until the smelting is completed;

[0058] Step 4: After smelting is completed, the bottom and the ventilation pipes arranged on the peripheral wall of the smelting furnace are opened at the same time to transport nitrogen to the copper liquid for 25 minutes. At the same time, the gas is discharged from the top of the smelting furnace; wherein, the length of the ventilation pipe on the peripheral wall of the smelting furnace extending into the copper liquid accounts for 15% of the distribution width of the copper liquid, and the nitrogen transportation in the ventilation pipe at the bottom of the smelting furnace is consistent with step 3, the pressure of nitrogen in the ventilation pipe on the peripheral wall of the smelting furnace is 2.5 bar, and the flow rate of nitrogen is adjusted to 2.2 Nm 3 / h, subject to ensuring that nitrogen can be discharged stably.

[0059] Step 5, conveying the copper liquid obtained in step 4 to a holding furnace through a melting ditch, the holding temperature being 1220° C., and the top surface of the copper liquid is sequentially covered with chestnut charcoal with a thickness of 15 cm and flake graphite with a thickness of 2.5 cm from bottom to top;

[0060] Step 6, extend the hollow crystallizer into the copper liquid in the insulation furnace, the copper liquid enters the central control crystallizer and is condensed into a solid using circulating water, the inlet temperature of the circulating cooling water in the hollow crystallizer is 28°C, and the temperature difference between the cooling inlet and outlet water is 8°C; the solid is led to a copper rod through a traction device, the traction speed is 25mm / min, and the diameter of the prepared oxygen-free copper rod is 8mm.

[0061] Comparative Example 1

[0062] Comparative Example 1 Compared with the process of preparing the oxygen-free copper rod in Example 1, no nitrogen treatment was performed, and the specific operation process was as follows:

[0063] Preparation of oxygen-free copper rod

[0064] Step 1, heat the smelting furnace to 1200±5℃ and set aside;

[0065] Step 2: Hang the electrolytic copper plate raw material above the red charcoal at the furnace mouth and bake it for 4 minutes to dry;

[0066] Step 3, quickly transporting the dried electrolytic copper plate to a smelting furnace, and keeping the smelting furnace in a vacuum state, smelting to obtain copper liquid;

[0067] Step 4, the copper liquid obtained in step 3 is transported to a holding furnace through a melting ditch, the holding temperature is 1200° C., and the top surface of the copper liquid is covered with 13 cm thick chestnut charcoal and 3 cm thick flake graphite from bottom to top;

[0068] Step 5, extend the hollow crystallizer into the copper liquid in the insulation furnace, the copper liquid enters the central control crystallizer and is condensed into a solid using circulating water, the inlet temperature of the circulating cooling water in the hollow crystallizer is 27°C, and the temperature difference between the cooling inlet and outlet water is 6°C; the solid is led to a copper rod through a traction device, the traction speed is 80mm / min, and the diameter of the prepared oxygen-free copper rod is 10mm.

[0069] Comparative Example 2

[0070] Comparative Example 2 Compared with the process of preparing the oxygen-free copper rod in Example 1, the nitrogen treatment in step 3 was not performed, and the specific operation process was as follows:

[0071] Preparation of oxygen-free copper rod

[0072] Step 1, heat the smelting furnace to 1200±5℃ and set aside;

[0073] Step 2: Hang the electrolytic copper plate raw material above the red charcoal at the furnace mouth and bake it for 4 minutes to dry;

[0074] Step 3, quickly transporting the dried electrolytic copper plate to a smelting furnace, and keeping the smelting furnace in a vacuum state, smelting to obtain copper liquid;

[0075] Step 4: After smelting is completed, the bottom and the ventilation pipes arranged on the peripheral wall of the smelting furnace are opened at the same time to transport nitrogen to the copper liquid for 30 minutes, and at the same time, the gas is discharged from the top of the smelting furnace; wherein, the length of the ventilation pipe on the peripheral wall of the smelting furnace extending into the copper liquid accounts for 10% of the distribution width of the copper liquid, and the nitrogen transportation in the ventilation pipe at the bottom of the smelting furnace is consistent with step 3 in Example 1, the pressure of nitrogen in the ventilation pipe on the peripheral wall of the smelting furnace is 2.8 bar, and the flow rate of nitrogen is adjusted to 2Nm 3 / h, subject to ensuring that nitrogen can be discharged stably.

[0076] Step 5, the copper liquid obtained in step 4 is transported to a holding furnace through a melting ditch, the holding temperature is 1200° C., and the top surface of the copper liquid is covered with 13 cm thick chestnut charcoal and 3 cm thick flake graphite from bottom to top;

[0077] Step 6, extend the hollow crystallizer into the copper liquid in the insulation furnace, the copper liquid enters the central control crystallizer and is condensed into a solid using circulating water, the inlet temperature of the circulating cooling water in the hollow crystallizer is 27°C, and the temperature difference between the cooling inlet and outlet water is 6°C; the solid is led to a copper rod through a traction device, the traction speed is 80mm / min, and the diameter of the prepared oxygen-free copper rod is 10mm.

[0078] Comparative Example 3

[0079] Compared with the process of preparing the oxygen-free copper rod in Example 1, the operation of step 4 was not performed in Comparative Example 3. The specific operation process is as follows:

[0080] Preparation of oxygen-free copper rod

[0081] Step 1, heat the smelting furnace to 1200±5℃ and set aside;

[0082] Step 2: Hang the electrolytic copper plate raw material above the red charcoal at the furnace mouth and bake it for 4 minutes to dry;

[0083] Step 3, quickly transport the dried electrolytic copper plate to the smelting furnace, and keep the smelting furnace in a vacuum state for smelting; a plurality of vent pipes are evenly spaced on the bottom and the surrounding wall of the smelting furnace, and the interval between adjacent vent pipes is 15 cm; during the smelting process, the plurality of vent pipes at the bottom of the smelting furnace extend into the molten copper, and nitrogen is continuously introduced into the molten copper. The length of the vent pipe at the bottom of the smelting furnace extending into the molten copper accounts for 10% of the height of the molten copper, the pressure of the nitrogen is 3 bar, and the flow rate of the nitrogen is adjusted to 2.5 Nm 3 / h, and at the same time, the gas is extracted from the top of the smelting furnace until the smelting is completed;

[0084] Step 4, the copper liquid obtained in step 3 is transported to a holding furnace through a melting ditch, the holding temperature is 1200° C., and the top surface of the copper liquid is covered with 13 cm thick chestnut charcoal and 3 cm thick flake graphite from bottom to top;

[0085] Step 5, extend the hollow crystallizer into the copper liquid in the insulation furnace, the copper liquid enters the central control crystallizer and is condensed into a solid using circulating water, the inlet temperature of the circulating cooling water in the hollow crystallizer is 27°C, and the temperature difference between the cooling inlet and outlet water is 6°C; the solid is led to a copper rod through a traction device, the traction speed is 80mm / min, and the diameter of the prepared oxygen-free copper rod is 10mm.

[0086] Comparative Example 4

[0087] In the process of preparing the oxygen-free copper rod in Comparative Example 4, compared with Example 1, the arrangement of the ventilation pipe in the smelting furnace was changed, and the specific operation process was as follows:

[0088] Preparation of oxygen-free copper rod

[0089] Step 1, heat the smelting furnace to 1200±5℃ and set aside;

[0090] Step 2: Hang the electrolytic copper plate raw material above the red charcoal at the furnace mouth and bake it for 4 minutes to dry;

[0091] Step 3, quickly transport the dried electrolytic copper plate to the smelting furnace, and keep the smelting furnace in a vacuum state for smelting; a vent pipe is provided at the bottom of the smelting furnace, and during the smelting process, the vent pipe at the bottom of the smelting furnace extends into the copper liquid, and nitrogen is continuously introduced into the copper liquid. At the same time, the gas is extracted from the top of the smelting furnace until the smelting is completed;

[0092] Step 4: After smelting is completed, the vent pipe at the bottom of the smelting furnace is continued to transport nitrogen to the copper liquid for 30 minutes, and at the same time, the gas is discharged from the top of the smelting furnace.

[0093] Step 5, the copper liquid obtained in step 4 is transported to a holding furnace through a melting ditch, the holding temperature is 1200° C., and the top surface of the copper liquid is covered with 13 cm thick chestnut charcoal and 3 cm thick flake graphite from bottom to top;

[0094] Step 6, extend the hollow crystallizer into the copper liquid in the insulation furnace, the copper liquid enters the central control crystallizer and is condensed into a solid using circulating water, the inlet temperature of the circulating cooling water in the hollow crystallizer is 27°C, and the temperature difference between the cooling inlet and outlet water is 6°C; the solid is led to a copper rod through a traction device, the traction speed is 80mm / min, and the diameter of the prepared oxygen-free copper rod is 10mm.

[0095] Comparative Example 5

[0096] In the process of preparing oxygen-free copper rod in Comparative Example 5, compared with Example 1, the ventilation mode of the smelting furnace is changed, and the specific operation process is as follows:

[0097] Step 1, heat the smelting furnace to 1200±5℃ and set aside;

[0098] Step 2: Hang the electrolytic copper plate raw material above the red charcoal at the furnace mouth and bake it for 4 minutes to dry;

[0099] Step 3, quickly transport the dried electrolytic copper plate to the smelting furnace, and keep the smelting furnace in a vacuum state for smelting; a vent pipe is provided at the bottom of the smelting furnace, and during the smelting process, the vent pipe at the bottom of the smelting furnace extends into the copper liquid, and nitrogen is continuously introduced into the copper liquid. The smelting furnace is also provided with a stirring device, which can stir the nitrogen into tiny bubbles. At the same time, the top of the smelting furnace extracts the gas until the smelting is completed;

[0100] Step 4: After smelting is completed, the vent pipe at the bottom of the smelting furnace is continued, and bubble stirring is performed to transport nitrogen to the copper liquid for 30 minutes. At the same time, the gas is discharged from the top of the smelting furnace.

[0101] Step 5, the copper liquid obtained in step 4 is transported to a holding furnace through a melting ditch, the holding temperature is 1200° C., and the top surface of the copper liquid is covered with 13 cm thick chestnut charcoal and 3 cm thick flake graphite from bottom to top;

[0102] Step 6, extend the hollow crystallizer into the copper liquid in the insulation furnace, the copper liquid enters the central control crystallizer and is condensed into a solid using circulating water, the inlet temperature of the circulating cooling water in the hollow crystallizer is 27°C, and the temperature difference between the cooling inlet and outlet water is 6°C; the solid is led to a copper rod through a traction device, the traction speed is 80mm / min, and the diameter of the prepared oxygen-free copper rod is 10mm.

[0103] Comparative Example 6

[0104] Comparative Example 6 Compared with Example 1, the chestnut charcoal in Example 1 was replaced with conventional commercial charcoal, and the other preparation processes were the same as those in Example 1.

[0105] test:

[0106] The oxygen content, electrical conductivity and tensile strength of the oxygen-free copper rods prepared in Examples 1-3 and Comparative Examples 1-6 were tested respectively.

[0107] The oxygen content was tested in accordance with the YS / T922 standard, and the conductivity was tested in accordance with the method specified in the GB / T3048.2 standard. The test results are shown in Table 1.

[0108] Table 1 Performance test results of copper rods prepared in the embodiments and comparative examples

[0109]

[0110]

[0111] The present invention provides a method for preparing oxygen-free copper rods, the main steps of which include baking, smelting, heat preservation and condensation of electrolytic copper plate raw materials into solids, and upper copper rods. The present invention specifically adjusts the structure of the smelting furnace, and a plurality of ventilation pipes are evenly distributed at intervals on the bottom and the peripheral wall of the smelting furnace; during the smelting process, the plurality of ventilation pipes at the bottom of the smelting furnace extend into the copper liquid, and nitrogen is continuously introduced into the copper liquid. The gas is extracted from the top of the smelting furnace. After the smelting is completed, the ventilation pipes arranged on the bottom and the peripheral wall of the smelting furnace are opened at the same time to transport nitrogen to the copper liquid. Nitrogen, at the same time, the gas is discharged from the top of the smelting furnace. In this way, the oxygen in the copper liquid can be well removed. Then, the top surface of the copper liquid in the insulation furnace is covered with a layer of chestnut charcoal. Studies have found that chestnut charcoal can better eliminate the oxygen in the copper liquid. Then, a layer of flake graphite is covered to block the air. By adjusting the range of other process parameters, the oxygen content of the prepared oxygen-free copper rod is controlled below 1ppm, with high electrical conductivity, high tensile strength and good stability, which meets the higher requirements of special fields and is easy to promote and apply.

[0112] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing an oxygen-free copper rod, characterized in that: The following steps are involved: Step 1, heat the smelting furnace to 1200±5℃ and set aside; Step 2: Hang the electrolytic copper plate raw material above the red charcoal at the furnace mouth and bake it for 4 minutes to dry; Step 3, quickly transport the dried electrolytic copper plate to the smelting furnace, and keep the smelting furnace in a vacuum state for smelting; a plurality of vent pipes are evenly spaced on the bottom and the surrounding wall of the smelting furnace, and the interval between adjacent vent pipes is 15 cm; during the smelting process, the plurality of vent pipes at the bottom of the smelting furnace extend into the molten copper, and nitrogen is continuously introduced into the molten copper. The length of the vent pipe at the bottom of the smelting furnace extending into the molten copper accounts for 10% of the height of the molten copper, the pressure of the nitrogen is 3 bar, and the flow rate of the nitrogen is adjusted to 2.5 Nm 3 / h, and at the same time, the gas is extracted from the top of the smelting furnace until the smelting is completed; Step 4: After smelting is completed, the vent pipes arranged at the bottom and the peripheral wall of the smelting furnace are opened at the same time to deliver nitrogen to the copper liquid for 30 minutes. At the same time, the gas is discharged from the top of the smelting furnace, wherein the length of the vent pipe on the peripheral wall of the smelting furnace extending into the copper liquid accounts for 10% of the distribution width of the copper liquid, and the nitrogen delivery in the vent pipe at the bottom of the smelting furnace is consistent with step 3. The pressure of nitrogen in the vent pipe on the peripheral wall of the smelting furnace is 2.8 bar, and the flow rate of nitrogen is adjusted to 2Nm 3 / h; Step 5, the copper liquid obtained in step 4 is transported to a holding furnace through a melting ditch, the holding temperature is 1200° C., and the top surface of the copper liquid is covered with 13 cm thick chestnut charcoal and 3 cm thick flake graphite from bottom to top; Step 6, extending the hollow crystallizer into the copper liquid in the holding furnace, the copper liquid enters the central control crystallizer and is condensed into a solid using circulating water, the inlet temperature of the circulating cooling water in the hollow crystallizer is 27°C, and the temperature difference between the cooling inlet and outlet water is 6°C; the solid is led to a copper rod through a traction device, the traction speed is 80mm / min, and the diameter of the prepared oxygen-free copper rod is 10mm; Step 7, winding the wire on a winding machine through a wire dividing rod to obtain an oxygen-free copper rod; The oxygen-free copper rod has an oxygen content of 0.46 ppm, an electrical conductivity of 103.5% IACS, and a tensile strength of 230 MPa.

2. An oxygen-free copper rod prepared by the method for preparing an oxygen-free copper rod as claimed in claim 1.

3. Application of the oxygen-free copper rod as claimed in claim 2 in wind power lines, nuclear power lines and automotive lines.

Citation Information

Cited By

  • Low-oxygen high-purity phosphorus copper rod continuous casting process based on scrap copper

    CN120967158A

  • A continuous casting process of low-oxygen high-purity phosphor copper rod based on scrap copper

    CN120967158B