An organic ferroelectric liquid crystal thin film material and its preparation method and application

By using specific combinations of components and preparation methods in organic ferroelectric liquid crystal materials, the problem of insufficient stability and ferroelectric properties at high temperatures is solved, and the preparation of organic ferroelectric liquid crystal thin film materials with excellent performance at high temperatures is realized. , suitable for dielectric energy storage capacitors.

CN117820775BActive Publication Date: 2024-12-06WUHAN INSTITUTES OF ADVANCED TECHNOLOGY CHINESE ACADEMY OF SCIENCES
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202311821883.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-27
Publication Date
2024-12-06
Estimated Expiration
2043-12-27

AI Technical Summary

Technical Problem

Existing organic ferroelectric liquid crystal materials have poor stability at high temperatures and are not excellent in ferroelectric performance, making it difficult to effectively apply in the field of information storage devices.

Method used

Using a main matrix, 4,4',4"'-(porphyrin-5,10,15,20-tetrayl)tetrakis(N-hexadecylbenzamide), dopants and interfaces The combination of active agents forms an organic ferroelectric liquid crystal thin film material through the preparation method, and uses the compatibility and characteristics of these components to adjust their ferroelectric properties and dielectric constants to improve high temperature stability and ferroelectric properties.

Benefits of technology

The prepared organic ferroelectric liquid crystal film material has excellent stability and good ferroelectric properties at high temperatures. It is suitable for use in the field of dielectric energy storage capacitors. The preparation method is simple and easy to operate, and is suitable for industrial-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117820775B_ABST
    Figure CN117820775B_ABST
Patent Text Reader

Abstract

The present application relates to the field of information storage devices, and in particular to an organic ferroelectric liquid crystal film material and its preparation method and application. The present invention uses 4,4',4",4"'-(porphyrin-5,10,15,20-tetrayl)tetrakis(N-hexadecylbenzamide) with a special structure and a polymer main matrix, a dopant and other components to prepare an organic ferroelectric liquid crystal film material. Since the added components have good compatibility, the prepared modified film has good consistency and stability; in addition, due to the addition of 4,4',4",4"'-(porphyrin-5,10,15,20-tetrayl)tetrakis(N-hexadecylbenzamide), the prepared organic liquid crystal film material has good stability at high temperature and can be converted into a liquid crystal phase, so that the organic liquid crystal film material has good dielectric properties and has good prospects in the field of dielectric energy storage capacitors; the method of the present invention is also simple and easy to operate, suitable for industrial-scale production, and is conducive to the commercial utilization of organic ferroelectric liquid crystal films.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of information storage devices, and in particular to an organic ferroelectric liquid crystal thin film material and a preparation method and application thereof. Background Art

[0002] Ferroelectric liquid crystal materials are mesocrystal materials with special hysteresis loops and spontaneous polarization characteristics, which are widely used in display devices, optoelectronic devices, sensors and other fields. However, traditional ferroelectric liquid crystal materials have some limitations in performance and application, such as low stability, low response speed and limited operating temperature range. Therefore, it is of great significance to study and develop new ferroelectric liquid crystal materials.

[0003] In order to further improve the performance of ferroelectric liquid crystal materials, researchers have tried to prepare organic ferroelectric liquid crystal thin film materials and add organic molecules with special structures, such as Chinese patent application CN1214073A (invalid) discloses a ferroelectric liquid crystal mixture and Chinese patent CN85104134B (invalid) discloses a ferroelectric liquid crystal composition. In recent years, porphyrin compounds have received extensive attention due to their unique photoelectric properties and biocompatibility. In addition, their molecular structure has a high degree of stability and adjustability, and their physical and chemical properties can be changed by regulating the molecular structure, and it has ferroelectric properties. Therefore, adding porphyrin with a certain structure in the process of preparing organic liquid crystal ferroelectric materials has the potential to be used as a ferroelectric liquid crystal material.

[0004] At present, there are many studies on organic ferroelectric liquid crystal materials with special structures being conducted. However, there are very few types of such organic ferroelectric liquid crystal materials, and there are problems such as difficulty in preparation and complicated preparation process. In addition, the organic ferroelectric materials with special structures prepared by existing methods still have the problem of poor stability at high temperatures, and the ferroelectric performance is not excellent enough, and still cannot be well applied in the field of information storage devices. Therefore, the purpose of the present invention is to provide an organic ferroelectric liquid crystal film material with good high temperature resistance and good stability, and a preparation method and application thereof. Summary of the invention

[0005] The embodiments of the present application provide an organic ferroelectric liquid crystal thin film material and a preparation method and application thereof, so as to solve the problems of the existing organic ferroelectric liquid crystal thin film materials having insufficient ferroelectric properties and poor high temperature resistance.

[0006] In a first aspect, the present invention provides an organic ferroelectric liquid crystal thin film material, comprising the following components in parts by weight:

[0007] 25-40 copies of main matrix;

[0008] 4,4',4",4"'-(porphyrin-5,10,15,20-tetrayl)tetrakis(N-hexadecylbenzamide) 50-65 parts;

[0009] 2 to 7 parts of dopant;

[0010] 1 to 4 parts of surfactant;

[0011] The structural formula of the 4,4',4",4"'-(porphyrin-5,10,15,20-tetrayl)tetrakis(N-hexadecylbenzamide) is:

[0012]

[0013] Specifically, the main matrix is ​​selected from at least one of polystyrene (PS) or polymethyl methacrylate (PMMA); these polymers have good thermal stability and good compatibility with 4,4',4",4"'-(porphyrin-5,10,15,20-tetrayl)tetrakis(N-hexadecylbenzamide);

[0014] Specifically, the dopant is titanium oxide or zirconium oxide; adding an appropriate amount of the dopant can adjust the dielectric constant, refractive index, and charge transport performance of the organic ferroelectric liquid crystal film material through the interaction with the main matrix and 4,4',4",4"'-(porphyrin-5,10,15,20-tetrayl)tetra(N-hexadecylbenzamide), and can further improve the ferroelectric properties of the organic ferroelectric liquid crystal film material;

[0015] Specifically, the size of the dopant is less than 500 nm;

[0016] Specifically, the surfactant is selected from sodium dodecyl sulfate (SDS) or sodium dodecylbenzene sulfonate (SDBS); adding a proper amount of the surfactant can maintain the stability and orientation of the prepared 4,4',4",4"'-(porphyrin-5,10,15,20-tetrayl)tetrakis(N-hexadecylbenzamide) in the system;

[0017] In a second aspect, the present invention provides a method for preparing the above-mentioned organic ferroelectric liquid crystal thin film material, comprising the following steps:

[0018] Step 1: dissolving the main matrix in a solvent to obtain a polymer solution, adding 4,4',4",4"'-(porphyrin-5,10,15,20-tetrayl)tetrakis(N-hexadecylbenzamide) and a dopant to the polymer solution and stirring them thoroughly, adding an appropriate amount of a surfactant and continuing to stir evenly to obtain a mixture;

[0019] Step 2: coating the mixture on a substrate to obtain a thin film, and then drying the thin film to obtain the organic ferroelectric liquid crystal thin film material;

[0020] Specifically, the solvent in step 1 is selected from at least one of chloroform, dichloromethane or tetrahydrofuran;

[0021] Specifically, the substrate in step 2 is glass or silicon wafer;

[0022] Specifically, the coating in step 2 is spin coating or dipping;

[0023] Specifically, the drying method in step 2 is spin drying.

[0024] Specifically, the preparation method of the 4,4',4",4"'-(porphyrin-5,10,15,20-tetrayl)tetrakis(N-hexadecylbenzamide) comprises:

[0025] Step 1. Under an inert atmosphere, a toluene solution containing iodobenzene is added to 5,10,15,20-tetrakis(4-bromophenyl)porphyrin, and then palladium acetate, bis(2-diphenylphosphinophenyl)ether and cesium hydroxide monohydrate are added thereto, and then hexadecylamine, chloroform and water are added to react;

[0026] Step 2. Cool the reaction solution obtained in step 1 to room temperature, remove palladium acetate and the organic phase in the reaction solution, then collect and wash the precipitate, and then recrystallize to obtain the organic liquid crystal ferroelectric material.

[0027] Specifically, the molar ratio of the 5,10,15,20-tetrakis(4-bromophenyl)porphyrin, iodobenzene, bis(2-diphenylphosphophenyl)ether, cesium hydroxide monohydrate and hexadecylamine added in step 1 is 1:2-2.5:0.10-0.11:10-11:1-1.2.

[0028] Specifically, the inert atmosphere in step 1 is a nitrogen atmosphere or an argon atmosphere.

[0029] Specifically, the molar ratio of the palladium acetate added in step 1 to the 5,10,15,20-tetrakis(4-bromophenyl)porphyrin is 1:40-45, and the volume ratio of the added iodobenzene-containing toluene solution to the added chloroform is 6:5.

[0030] Specifically, the reaction in step 1 is carried out under condensation reflux conditions, the reaction temperature is 75 to 90° C., and the reaction time is 16 to 24 hours.

[0031] Specifically, the molar concentration of iodobenzene in the toluene solution containing iodobenzene in step 1 is 0.15-0.2M.

[0032] Specifically, the washing solvent in step 2 is ethyl acetate.

[0033] Specifically, the process of removing the organic phase in step 2 is to spin-dry the organic phase after liquid separation, and the organic phase includes toluene and chloroform.

[0034] Specifically, the preparation method of 5,10,15,20-tetrakis(4-bromophenyl)porphyrin in step 1 comprises:

[0035] Step 1), adding propionic acid to bromobenzaldehyde under an inert atmosphere, then stirring and adding pyrrole to react to obtain a solid product;

[0036] Step 2), repeatedly washing the solid product, separating and purifying it, and then recrystallizing it to obtain 5,10,15,20-tetrakis(4-bromophenyl)porphyrin.

[0037] More specifically, the structure of the prepared 5,10,15,20-tetrakis(4-bromophenyl)porphyrin is as follows:

[0038]

[0039] More specifically, in step 1), the molar ratio of bromobenzaldehyde to pyrrole is 1:1-1.02, and the volume ratio of propionic acid to pyrrole is 100:3.

[0040] More specifically, the reaction in step 1) is carried out under condensation reflux conditions, the reaction temperature is 120-140° C., and the reaction time is 12-16 hours.

[0041] More specifically, the inert atmosphere in step 1) is a nitrogen atmosphere or an argon atmosphere.

[0042] More specifically, the washing reagent in step 2) is dichloromethane.

[0043] More specifically, the separation and purification process in step 2) is as follows: dispersing the solid product obtained after washing in dichloromethane to obtain a dark red liquid, and then drying the dark red liquid by spin drying and then subjecting it to column chromatography.

[0044] In a third aspect, the present invention provides an application of the above-mentioned organic ferroelectric liquid crystal thin film material in the field of dielectric energy storage capacitors.

[0045] The beneficial effects of the technical solution provided by this application include:

[0046] 1. The present invention uses 4,4',4",4"'-(porphyrin-5,10,15,20-tetrayl)tetrakis(N-hexadecylbenzamide) with a special structure, a polymer main matrix, a dopant and other components as raw materials to prepare an organic ferroelectric liquid crystal film. Since the added components have good compatibility, the prepared film has good consistency and stability. In addition, since 4,4',4",4"'-(porphyrin-5,10,15,20-tetrayl)tetrakis(N-hexadecylbenzamide) has good stability at high temperature and can be converted into a liquid crystal phase, and has good ferroelectric properties and dielectric properties, the prepared organic liquid crystal film has good ferroelectric properties and dielectric properties, and has good prospects in the field of dielectric energy storage capacitors.

[0047] 2. The method for preparing the organic liquid crystal film provided by the method of the present invention is simple and easy to operate, suitable for industrial-scale production, and is conducive to the commercial utilization of the organic ferroelectric liquid crystal film. BRIEF DESCRIPTION OF THE DRAWINGS

[0048] Figure 1 The phase change diagram of the organic ferroelectric liquid crystal thin film material prepared in Example 2;

[0049] Figure 2 The dielectric properties test diagram of the organic ferroelectric liquid crystal thin film material prepared in Example 2;

[0050] Figure 3 This is the polarization-electric field hysteresis curve of the organic ferroelectric liquid crystal thin film material prepared in Example 2. DETAILED DESCRIPTION

[0051] The technical solution of the present application will be clearly and completely described below in conjunction with the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present application.

[0052] The preparation method of 5,10,15,20-tetrakis(4-bromophenyl)porphyrin according to the embodiment of the present invention is as follows:

[0053] Step 1) Add 16.2 mmol of bromobenzaldehyde into a 250 mL three-necked flask, evacuate the air and fill with nitrogen, use a dropping funnel to add 150 mL of propionic acid to the reaction flask, adjust the temperature to 130°C, stir and add 16.2 mmol of pyrrole, and filter to obtain a solid product;

[0054] Step 2) Wash the solid product 4 times with dichloromethane, then rinse the filter cake with dichloromethane to obtain a dark red liquid, spin-dry the filtrate, separate and purify by column chromatography, and then recrystallize to obtain 5,10,15,20-tetrakis(4-bromophenyl)porphyrin. The structure of the synthesized 5,10,15,20-tetrakis(4-bromophenyl)porphyrin is as follows:

[0055]

[0056] Example 1

[0057] Preparation of 4,4',4",4"'-(porphyrin-5,10,15,20-tetrayl)tetrakis(N-hexadecylbenzamide) described in the examples of the present invention:

[0058] Step 1. Take 1.0 mmol of 5,10,15,20-tetrakis(4-bromophenyl)porphyrin, add 12 mL of toluene solution containing iodobenzene (0.17 M iodobenzene, 2.0 mmol) under an inert atmosphere, then add 25 μmol of palladium acetate solution, 0.10 mmol of bis(2-diphenylphosphinophenyl)ether solution, and 10 mmol of cesium hydroxide monohydrate. Then add 1.2 mmol of hexadecylamine and 10 mL of chloroform. Add water (1 mL) and stir the reactants at 80°C for 24 hours;

[0059] Step 2. The reaction solution obtained in step 1 is cooled to room temperature, the catalyst is filtered off, the organic phase is spin-dried after separation, the toluene and chloroform solutions in the system are removed, the precipitate is collected and washed with ethyl acetate, and then recrystallized twice to obtain the 4,4',4",4"'-(porphyrin-5,10,15,20-tetrayl)tetrakis(N-hexadecylbenzamide).

[0060] Example 2

[0061] Preparation of organic ferroelectric liquid crystal thin film materials:

[0062] Step 1, dissolving 37 parts by mass of PS in 25 parts by mass of chloroform to obtain a polymer solution, adding 57 parts by mass of 4,4',4",4"'-(porphyrin-5,10,15,20-tetrayl)tetrakis(N-hexadecylbenzamide) prepared in Example 1 and 4 parts by mass of titanium oxide (300 nm) to the polymer solution and stirring well, adding 3 parts by mass of SDS and continuing to stir evenly to obtain a mixture;

[0063] Step 2: coating the mixture on a glass substrate to obtain a thin film, and then spin-drying the thin film to obtain the organic ferroelectric liquid crystal thin film material.

[0064] The organic ferroelectric liquid crystal thin film material was heated to 660K for thermogravimetric testing, and its weight loss rate was measured to be 0%, which indicates that the organic ferroelectric liquid crystal thin film material has excellent thermal stability at a temperature as high as 660K.

[0065] Example 3

[0066] Preparation of organic ferroelectric liquid crystal thin film materials:

[0067] Step 1, dissolving 25 parts by mass of PS in 15 parts by mass of dichloromethane to obtain a polymer solution, adding 50 parts by mass of 4,4',4",4"'-(porphyrin-5,10,15,20-tetrayl)tetrakis(N-hexadecylbenzamide) prepared in Example 1 and 2 parts by mass of zirconium oxide (500 nm) to the polymer solution and stirring well, adding 1 part by mass of SDBS and continuing to stir evenly to obtain a mixture;

[0068] Step 2: coating the mixture on a silicon wafer to obtain a thin film, and then spin-drying the thin film to obtain the organic ferroelectric liquid crystal thin film material.

[0069] The organic ferroelectric liquid crystal thin film material was heated to 660K for thermogravimetric testing, and its weight loss rate was measured to be 0%, which indicates that the organic ferroelectric liquid crystal thin film material has excellent thermal stability at a temperature as high as 660K.

[0070] Example 4

[0071] Preparation of organic ferroelectric liquid crystal thin film materials:

[0072] Step 1, dissolving 40 parts by mass of PS in 40 parts by mass of tetrahydrofuran to obtain a polymer solution, adding 65 parts by mass of 4,4',4",4"'-(porphyrin-5,10,15,20-tetrayl)tetrakis(N-hexadecylbenzamide) prepared in Example 1 and 7 parts by mass of zirconium oxide (500 nm) to the polymer solution and stirring well, adding 4 parts by mass of SDBS and continuing to stir evenly to obtain a mixture;

[0073] Step 2: coating the mixture on a glass substrate to obtain a thin film, and then spin-drying the thin film to obtain the organic ferroelectric liquid crystal thin film material.

[0074] The organic ferroelectric liquid crystal thin film material was heated to 660K for thermogravimetric testing, and its weight loss rate was measured to be 0%, which indicates that the organic ferroelectric liquid crystal thin film material has excellent thermal stability at a temperature as high as 660K.

[0075] Example 5

[0076] Preparation of organic ferroelectric liquid crystal thin film materials:

[0077] Step 1, dissolving 35 parts by mass of PMMA in 40 parts by mass of tetrahydrofuran to obtain a polymer solution, adding 55 parts by mass of 4,4',4",4"'-(porphyrin-5,10,15,20-tetrayl)tetrakis(N-hexadecylbenzamide) prepared in Example 1 and 4 parts by mass of zirconium oxide (100 nm) to the polymer solution and stirring well, adding 2 parts by mass of SDBS and continuing to stir evenly to obtain a mixture;

[0078] Step 2: coating the mixture on a glass substrate to obtain a thin film, and then spin-drying the thin film to obtain the organic ferroelectric liquid crystal thin film material.

[0079] The organic ferroelectric liquid crystal thin film material was heated to 600K for thermogravimetric testing, and its weight loss rate was measured to be 0%, which indicates that the organic ferroelectric liquid crystal thin film material has good thermal stability at a temperature as high as 600K.

[0080] Example 6

[0081] Preparation of organic ferroelectric liquid crystal thin film materials:

[0082] Step 1, dissolving 35 parts by mass of PS in 15 parts by mass of tetrahydrofuran to obtain a polymer solution, adding 60 parts by mass of 4,4',4",4"'-(porphyrin-5,10,15,20-tetrayl)tetrakis(N-hexadecylbenzamide) prepared in Example 1 and 6 parts by mass of zirconium oxide (300 nm) to the polymer solution and stirring well, adding 3 parts by mass of SDBS and continuing to stir evenly to obtain a mixture;

[0083] Step 2: coating the mixture on a glass substrate to obtain a thin film, and then spin-drying the thin film to obtain the organic ferroelectric liquid crystal thin film material.

[0084] The organic ferroelectric liquid crystal thin film material was heated to 650K for thermogravimetric testing, and its weight loss rate was measured to be 0%, which indicates that the organic ferroelectric liquid crystal thin film material has good thermal stability at a temperature as high as 650K.

[0085] Performance Testing

[0086] The performance of the organic ferroelectric liquid crystal thin film material prepared in this embodiment was tested, and the test results are shown in Figures 1 to 3 .

[0087] Figure 1 is the phase change diagram of the organic ferroelectric liquid crystal thin film material prepared in Example 2, Figure 1It can be seen that the organic ferroelectric liquid crystal thin film material shows a reversible and continuous phase transition from solid phase 1 to solid phase 2 at 336K, solid phase 2 to intermediate phase at 440K, and intermediate phase to isotropic liquid at 560K, and the relatively viscous behavior of the intermediate phase corresponds to the formation of a higher-order liquid crystal phase;

[0088] Figure 2 The dielectric properties test diagram of the organic ferroelectric liquid crystal thin film material prepared in Example 2, the specific test method is:

[0089] Take two pieces of indium tin oxide (ITO) glass with a conductive area of ​​1 cm2 in the middle, heat the organic ferroelectric liquid crystal film material prepared in Example 1 to the liquid crystal state, sandwich it between the corresponding ITO glasses, and connect them in series with gold foil to form a dielectric measurement unit with an average electrode gap of 2 um. The dielectric constants at 1, 10, 100, and 1000 kHz were measured at a voltage of 0.5 V in the temperature range of 320 to 560 K.

[0090] Figure 3 This is a graph showing the test results of the ferroelectric properties of the organic ferroelectric liquid crystal thin film material prepared in Example 2. The specific test method is as follows:

[0091] Take two pieces of indium tin oxide (ITO) glass with a conductive area of ​​1 cm2 in the middle, heat the organic ferroelectric liquid crystal film material prepared in Example 1 to the liquid crystal state, sandwich it between the corresponding ITO glasses, and connect them in series with gold foil to form a dielectric measurement unit with an average electrode gap of 2 um. Measure the ferroelectric response behavior at 0.1, 0.2, 0.5, and 1 Hz at 510K.

[0092] The test results show that the organic ferroelectric liquid crystal film material exhibits polarization-electric field hysteresis behavior within the range of 0.1 to 1.0 Hz, and the current response at a frequency of 1 Hz is much higher than the current response at a frequency of 0.5 Hz. This indicates that at this high temperature (510 K), the components of the organic ferroelectric liquid crystal film material can cause ferroelectric response and have good ferroelectric properties.

[0093] The above test results show that the organic ferroelectric liquid crystal film material prepared by the method of the present invention has good high temperature stability under high temperature conditions, can be transformed into a liquid crystal phase at high temperature, and also has good dielectric properties, and has good application prospects in the field of dielectric energy storage capacitors.

Claims

1. An organic ferroelectric liquid crystal thin film material, characterized in that: By weight, it includes the following ingredients: 25-40 copies of main matrix; 4,4',4"',4"'-(porphyrin-5,10,15,20-tetrayl)tetrakis(N-hexadecylbenzamide) 50-65 parts; 2 to 7 parts of dopant; 1 to 4 parts of surfactant; The structural formula of the 4,4',4",4"'-(porphyrin-5,10,15,20-tetrayl)tetrakis(N-hexadecylbenzamide) is: Wherein, the preparation method of the 4,4',4",4"'-(porphyrin-5,10,15,20-tetrayl)tetrakis(N-hexadecylbenzamide) comprises: Step 1. Under an inert atmosphere, a toluene solution containing iodobenzene is added to 5,10,15,20-tetrakis(4-bromophenyl)porphyrin, and then palladium acetate, bis(2-diphenylphosphinophenyl)ether and cesium hydroxide monohydrate are added thereto, and then hexadecylamine, chloroform and water are added to react; Step 2. Cool the reaction solution obtained in step 1 to room temperature, remove palladium acetate and the organic phase in the reaction solution, then collect and wash the precipitate, and then recrystallize to obtain; The main matrix is ​​selected from at least one of polystyrene and polymethyl methacrylate.

2. The organic ferroelectric liquid crystal thin film material according to claim 1, characterized in that: The dopant is titanium oxide or zirconium oxide.

3. The organic ferroelectric liquid crystal thin film material according to claim 2, characterized in that: The size of the dopant is less than 500 nm.

4. The organic ferroelectric liquid crystal thin film material according to claim 1, characterized in that: The surfactant is selected from sodium dodecyl sulfate or sodium dodecylbenzene sulfonate.

5. The method for preparing an organic ferroelectric liquid crystal thin film material according to claim 1, characterized in that: The following steps are involved: Step 1: dissolving the main matrix in a solvent to obtain a polymer solution, adding 4,4',4",4"'-(porphyrin-5,10,15,20-tetrayl)tetrakis(N-hexadecylbenzamide) and a dopant to the polymer solution and stirring them thoroughly, adding an appropriate amount of a surfactant and continuing to stir evenly to obtain a mixture; Step 2: coating the mixture on a substrate to obtain a thin film, and then drying the thin film to obtain the organic ferroelectric liquid crystal thin film material.

6. The method for preparing the organic ferroelectric liquid crystal thin film material according to claim 5, characterized in that: The solvent in step 1 is selected from at least one of chloroform, dichloromethane or tetrahydrofuran.

7. The method for preparing an organic ferroelectric liquid crystal thin film material according to claim 5, characterized in that: The molar ratio of the 5,10,15,20-tetrakis(4-bromophenyl)porphyrin, iodobenzene, bis(2-diphenylphosphophenyl)ether, cesium hydroxide monohydrate and hexadecylamine added in the step 1 is 1:2-2.5:0.10-0.11:10-11:1-1.

2.

8. Use of the organic ferroelectric liquid crystal thin film material according to any one of claims 1 to 4 in the field of dielectric energy storage capacitors.

Citation Information

Patent Citations

  • Ferroelectric liquid crystal mixture

    CN1214073A

  • Ferroelectric liquid crystal composites

    CN85104134A

  • Amide porphyrin derivative and preparation method thereof

    CN103374004A

  • Water-soluble porphyrin conjugated polymer as well as preparation method and application thereof

    CN103755928A

  • Polystyrene-porphyrin derivative nano vertical array thin film as well as preparation method and application thereof

    CN111548683A