A kind of water-based high-gloss industrial paint emulsion and preparation method thereof
By using tris(2-hydroxyethyl)isocyanurate triacrylate and α-methylstyrene dimer in water-based industrial paints, combined with hard core and soft shell processes and reactive emulsifiers, the paint film problem was solved Poor flexibility and resistance issues, achieving high hardness, gloss and environmentally friendly water-based industrial coating performance.
Patent Information
- Application Number
- CN202311854307.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-29
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-12-29
AI Technical Summary
Existing high-gloss water-based industrial paints have poor flexibility during the film-forming process and are prone to cracking or delamination. Although phosphate emulsifiers improve salt spray resistance, they affect water resistance, and thiol molecular weight regulators have an odor. And toxic, difficult to volatilize, affecting the environment and human health.
Tris(2-hydroxyethyl)isocyanurate triacrylate is used as the internal cross-linking agent and α-methylstyrene dimer is used as the molecular weight regulator. Through the core-shell process design of hard core and soft shell, the paint quality is improved. Cross-linking density and gloss of the film, and improved adhesion and salt spray resistance through reactive emulsifiers and phosphate ester emulsifiers.
Improves the impact resistance, adhesion, water resistance, salt spray resistance and hardness of the paint film, while enhancing the flexibility and film-forming properties of the paint film, reducing water retention, increasing the drying speed, and obtaining high hardness and gloss And environmentally friendly water-based industrial coatings.
Smart Images

Figure GDA0004956623880000031 
Figure GDA0004956623880000041 
Figure GDA0004956623880000071
Abstract
Description
Technical Field
[0001] The invention mainly relates to the technical field of coatings, and specifically relates to a water-based high-gloss industrial paint emulsion and a preparation method thereof. Background Art
[0002] In recent years, the problem of atmospheric pollution in my country has become increasingly prominent. Traditional solvent-based industrial coatings contain a large amount of organic solvents, and organic solvents are often used for dilution during the construction process. These organic solvents evaporate into the atmosphere, which is harmful to the health of construction and user personnel, causing environmental pollution and fire hazards. The organic compounds that evaporate into the atmosphere react photochemically with nitrogen oxides in the presence of ultraviolet rays (sunlight) to form smog, which pollutes the environment, damages human health, leads to reduced crop yields, accelerated material aging and destruction of the ecological system, which has seriously affected the normal production and living order and endangered people's physical and mental health.
[0003] With the improvement of social environmental protection requirements and the strengthening of supervision, VOC (volatile organic compound) emissions of industrial paints (industrial coatings) have become a key area of air pollution control. It is an inevitable trend to develop low-VOC emission, green and environmentally friendly industrial paints and realize the green transformation and upgrading of industrial paints. Water-based industrial paints have become a hot spot in industrial paint research and application due to their low VOC, high flash point, storage and transportation safety, etc. Among water-based industrial paints, high-gloss water-based industrial paints are widely used in engineering machinery, special vehicles, bicycles, tricycles, equipment and facilities, steel structures and other industrial fields.
[0004] At present, high-gloss water-based industrial paints are mainly achieved through two-component hydroxyl dispersions, two-component acrylic emulsions and one-component water-based acrylic emulsions. Although two-component hydroxyl dispersions and two-component water-based acrylic emulsions are better than one-component water-based acrylic emulsions in terms of performance, when two-component hydroxyl dispersions and two-component water-based acrylic emulsions are used in industrial paints, the coating construction is complicated, the cost is high, and they contain a certain amount of solvents, especially the hydroxyl dispersions have a higher solvent content. These factors will cause water-based industrial paints to release a large amount of VOCs during the coating process, which will have a certain impact on the environment and the health of construction workers. When one-component acrylic emulsions are used in water-based industrial coatings, the coating construction is simple, the cost is low, and the VOC emissions are extremely low, which will hardly affect the environment and human health. However, one-component water-based acrylic emulsions have low hardness, poor resistance, poor adhesion, poor gloss, and poor salt spray. These factors have greatly affected the wide application of one-component water-based acrylic emulsions in water-based industrial coatings.
[0005] Patent 113429522A disclosed in the prior art uses a core-shell structure design with a soft core and a hard shell to ensure a low amount of film-forming aid added while having good adhesion, hardness and anti-sticking properties. It introduces a phosphate emulsifier to improve the salt spray resistance of the emulsion, and uses a thiol molecular weight regulator to adjust the polymer particle size distribution, which can improve the gloss of the synthetic product.
[0006] On the one hand, the above-mentioned prior art can make the emulsion have good adhesion, hardness and anti-sticking properties through the structural design of soft core and hard shell, but the structure of soft core and hard shell will make the emulsion form a harder outer layer of paint film during the film forming process, which will cause the outer layer of the paint film to be brittle, thereby making it less flexible and less impact-resistant after the emulsion is formed. Therefore, the coating is very likely to crack or even delaminate at the corners and curved positions, and when bumps occur during transportation or handling, the coating is also very likely to crack or even delaminate. On the other hand, although the introduction of phosphate emulsifiers can improve salt spray resistance, it will affect the water resistance of the emulsion, and the improvement of salt spray resistance also has certain limitations; although the use of mercaptan molecular weight regulators can significantly improve the gloss of the emulsion, mercaptan compounds contain sulfur, have a special odor, are difficult to volatilize, pollute the environment, and are toxic. And they are all hazardous chemicals, and special treatment is required during transportation, storage, and use, which is not only troublesome, but also expensive, and its residue will affect sensory evaluation. Summary of the invention
[0007] In order to solve the above problems, the present invention provides a water-based high-gloss industrial paint emulsion and a preparation method thereof.
[0008] In a first aspect of the present invention, a water-based high-gloss industrial paint emulsion is provided. The raw materials for preparing the water-based high-gloss industrial paint emulsion include the following components in parts by weight:
[0009]
[0010]
[0011] Furthermore, the internal cross-linking agent is tris(2-hydroxyethyl)isocyanurate triacrylate.
[0012] Furthermore, the molecular weight regulator is α-methylstyrene dimer.
[0013] Furthermore, the phosphate emulsifier is one or any two of RS-610, RE-610, and RS-710.
[0014] In a second aspect of the present invention, a method for preparing a water-based high-gloss industrial paint emulsion is also provided, comprising the following steps:
[0015] (a) adding 200-400 parts of deionized water, 2-4 parts of reactive emulsifier and 2-4 parts of phosphate emulsifier into a reactor, stirring and mixing to obtain a bottom solution;
[0016] (b) adding 100-200 parts of deionized water, 1-2 parts of reactive emulsifier and 1-2 parts of phosphate emulsifier to a pre-emulsification tank, stirring and mixing, and then adding 220-440 parts of styrene, 40-80 parts of methyl methacrylate, 5-10 parts of methacrylic acid, 5-10 parts of acrylic acid, 0-50 parts of butyl acrylate, 1-3 parts of internal crosslinking agent tris(2-hydroxyethyl)isocyanurate triacrylate, 1-2 parts of molecular weight regulator α-methylstyrene dimer and 0.4-1 parts of initiator, and continuing stirring for 20-60 minutes to obtain a core monomer pre-emulsion;
[0017] (c) heating the reactor in step (a) to 85-90° C., adding 2-5 parts of the core monomer pre-emulsion obtained in step (b) to the reactor, and adding 0.4-1 parts of initiator, and keeping the temperature for 10-30 minutes;
[0018] (d) adding the remaining core monomer pre-emulsion to the reactor dropwise at 85° C.-90° C. for 90-180 min, and then keeping the temperature at 85-90° C. for 30-60 min.
[0019] (e) adding 100-200 parts of deionized water, 1-2 parts of reactive emulsifier and 1-2 parts of phosphate emulsifier to another pre-emulsification tank, stirring and mixing, and then adding 40-80 parts of methyl methacrylate, 150-300 parts of isooctyl acrylate, 5-10 parts of methacrylic acid, 4-7 parts of internal crosslinking agent tris(2-hydroxyethyl)isocyanurate triacrylate, 1-2 parts of molecular weight regulator α-methylstyrene dimer and 0.4-1 parts of initiator, and continuing stirring for 20-60 minutes to obtain a shell monomer pre-emulsion;
[0020] (f) After the core monomer emulsion is added dropwise and the insulation is completed, the prepared shell monomer pre-emulsion is added dropwise to the reactor at 85° C.-90° C. for 90-180 min. After completion, the mixture is kept at 85-90° C. for 60-120 min.
[0021] (g) After the insulation in step (f), the temperature is lowered to 65-75°C, an oxidant is added and the temperature is maintained for 20-30 minutes, and then a reducing agent is added and the temperature is maintained for 30-60 minutes;
[0022] (h) After the heat preservation in step (g) is completed, the temperature is lowered to below 50° C., 10-15 parts of a pH regulator, 1.5-2.5 parts of a defoaming agent and 5-10 parts of a fungicide are added, the temperature is kept and stirred for 10-20 minutes to obtain a hard-core soft-shell water-based high-gloss industrial paint emulsion.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] 1. A kind of water-based high-gloss industrial paint emulsion provided by the present invention, the trifunctional internal crosslinking agent tris (2-hydroxyethyl) isocyanuric acid triacrylate (THEICTA) is introduced, on the one hand THEICTA contains a long flexible chain, which can give the polymer molecule good flexibility, improve the impact resistance and adhesion of the emulsion; on the one hand, during the emulsion polymerization process, THEICTA is an internal crosslinking agent containing three double-bond functional groups, which can react and crosslink with methyl methacrylate and styrene, so that the emulsion is changed from a linear structure to a more dense network structure, increasing the crosslinking density of the emulsion, thereby improving the water resistance, salt spray resistance and hardness of the emulsion. On the other hand, the structural unit containing a certain amount of N in the THEICTA structure can better form more hydrogen bonds, and more hydrogen bonds can increase more binding points of the network polymer, further improve the crosslinking density of the emulsion, and increase the cohesion of the emulsion, thereby improving the water resistance, salt spray resistance and hardness of the emulsion.
[0025] 2. The water-based high-gloss industrial paint emulsion provided by the present invention also introduces a molecular weight regulator α-methylstyrene dimer (AMDS), which is an environmentally friendly, safe and odorless molecular weight regulator and chain transfer agent. In the first aspect, the addition of AMDS can effectively adjust the molecular weight of the acrylic emulsion, making the molecular weight of the acrylic emulsion smaller, the molecular weight distribution is uniform and narrow, and the leveling property is good, thereby significantly improving the gloss of the emulsion; in the second aspect, AMDS itself has a strong hydrophobicity, which can also improve the water resistance and salt spray resistance of the emulsion. In the third aspect, AMDS is a benzene ring containing a conjugated structure, which has a strong electron-withdrawing ability, resulting in it having a certain electrophilicity, and the carbon-centered alkyl radical formed during the polymerization of acrylic emulsion has a certain nucleophilicity, so the chain transfer efficiency of AMDS is higher, and the transfer efficiency of AMDS is higher, and it is easier to terminate the reaction after the polymer is polymerized to a certain extent, which is beneficial to control the polymer molecular weight within a certain range, so it is more conducive to forming a network structure with a uniform molecular weight distribution.
[0026] 3. The present invention provides a method for preparing a water-based high-gloss industrial paint emulsion. In the emulsion synthesis process, a hard-core and soft-shell core-shell process is adopted, and the core monomer Tg is set at 70-90°C, and the shell monomer Tg is set at -30-10°C. The core monomer is designed at 70-90°C so that the paint film has a certain hardness, and the shell layer is designed at -30-10°C so that the paint film has a certain toughness and the emulsion has good film-forming properties. The hard-core and soft-shell design can reduce the water retention of the emulsion and increase the drying speed of the emulsion during the film-forming process. Therefore, through such a structural Tg design, the emulsion has a certain hardness while having good film-forming properties and flexibility, so that a water-based industrial coating with high hardness, good film-forming properties, fast drying speed and certain flexibility can be obtained. DETAILED DESCRIPTION
[0027] To facilitate understanding of the present invention, the present invention will be described below in conjunction with specific implementation methods. However, the present invention can be implemented in different forms and is not limited to the embodiments described in the text. On the contrary, these embodiments are provided to make the content disclosed in the present invention more thorough and comprehensive.
[0028] The present invention provides a water-based high-gloss industrial paint emulsion, and the raw materials for preparation thereof include the following components in parts by weight:
[0029]
[0030]
[0031] The reactive emulsifier is one of SR-10, AR-10 and LR-10 or a mixture of any of them.
[0032] Conventional emulsifiers are physically adsorbed on the surface of latex particles to keep the latex particles stable. However, this effect is often destroyed when the emulsion forms a film, causing the emulsifier molecules to precipitate, greatly reducing the water resistance of the emulsion film. The emulsifier selected in the present invention is a reactive emulsifier, which contains a reactive functional group carbon-carbon double bond and can be combined with the polymer matrix through free radical reaction. The emulsifier will not migrate to the surface of the paint film and affect the water resistance and other resistances of the paint film.
[0033] The above-mentioned phosphate emulsifier is one or any two of RS-610, RE-610, RS-710. The phosphate ester in the phosphate emulsifier can chelate with the iron on the metal surface, thereby improving the adhesion of the emulsion on the metal substrate and the salt spray resistance.
[0034] Among them, the internal crosslinking agent is tris(2-hydroxyethyl)isocyanuric acid triacrylate (THEICTA). Tris(2-hydroxyethyl)isocyanuric acid triacrylate is a trifunctional internal crosslinking agent with three carbon-carbon double bond reaction points. It can be well polymerized with methyl methacrylate and styrene to change the synthesized polymer from a linear structure to a network structure, thereby enhancing the density of the paint film. In addition, the N-containing structural unit further increases the crosslinking density of the emulsion through hydrogen bonding, increases the cohesion of the paint film, and thus improves the water resistance, salt spray resistance and hardness of the emulsion.
[0035] The molecular weight regulator in the present invention is alpha-methylstyrene dimer (AMDS), which is a green, environmentally friendly and odorless molecular weight regulator that can effectively regulate the molecular weight of acrylic emulsion, thereby significantly improving the gloss of the emulsion; the alpha-methylstyrene dimer itself has strong hydrophobicity, and can improve the water resistance and salt spray resistance of the emulsion.
[0036] The initiator in the present invention is one of potassium persulfate, sodium persulfate, and ammonium persulfate, or a mixture of any of them.
[0037] The oxidant in the present invention is one of tert-butyl hydroperoxide and tert-butyl cumene peroxide or a mixture of the two.
[0038] The reducing agent in the present invention is any one of sodium bisulfite and ascorbic acid or a combination of the two.
[0039] The pH in the present invention is adjusted to 25% concentration of ammonia water, which has high neutralization efficiency and low price.
[0040] The defoamer in the present invention is a mineral oil defoamer.
[0041] The bactericide in the present invention is kasone and / or BIT.
[0042] In combination with the water-based high-gloss industrial paint emulsion composed of the above components, by setting the core monomer Tg to 70-90°C and the shell monomer Tg to -30-10°C, a hard core and soft shell core-shell process is adopted, the core monomer is designed at 70-90°C to make the paint film have a certain hardness, and the shell layer is designed at -30-10°C, so that the paint film has a certain toughness, and the emulsion has good film-forming properties, and the hard core and soft shell design can reduce the water retention of the emulsion and increase the drying speed of the emulsion in the film-forming process. Therefore, through such a structural Tg design, the emulsion has a certain hardness and good film-forming properties and flexibility. Thus, a water-based industrial coating with high hardness, good film-forming properties, fast drying speed, and certain flexibility can be obtained.
[0043] And by introducing the internal cross-linking agent tris(2-hydroxyethyl)isocyanuric acid triacrylate (THEICTA), on the one hand, the introduction of ethyl acrylate flexible chain segments can further improve the flexibility of the emulsion, thereby improving the impact resistance and adhesion of the emulsion. On the other hand, tris(2-hydroxyethyl)isocyanuric acid triacrylate is a carbon-carbon double bond containing three functional groups, which can be well polymerized with monomers such as methyl methacrylate and styrene, so that the synthesized polymer changes from a linear structure to a network structure, enhancing the density of the paint film, thereby improving the water resistance, salt spray resistance and hardness of the emulsion. At the same time, by adding the green, environmentally friendly and odorless molecular weight regulator α-methylstyrene dimer (AMDS), on the one hand, the molecular weight of the acrylic emulsion is effectively adjusted to improve the gloss of the emulsion. On the other hand, it has strong hydrophobicity, which will also improve the water resistance and salt spray resistance of the emulsion.
[0044] Example 1
[0045] (a) Preparation of the bottom solution: Add 200 parts of deionized water, 2 parts of AR-10 and 2 parts of RS-610 into a reactor and stir to obtain a bottom solution.
[0046] (b) Preparation of core monomer pre-emulsion: Add 100 parts of deionized water, 1 part of AR-10 and 1 part of RS-610 to a pre-emulsification tank, stir and mix well, then add 220 parts of styrene, 60 parts of methyl methacrylate, 5 parts of methacrylic acid, 5 parts of acrylic acid, 2 parts of THEICTA, 1 part of AMDS and 0.4 parts of KPS, continue stirring for 20-60 minutes to obtain a core monomer pre-emulsion.
[0047] (c) heating the reactor in step (a) to 85-90° C., adding 2 parts of the core monomer pre-emulsion obtained in step (b) to the reactor, and adding 0.4 parts of KPS, and keeping the temperature for 10-30 minutes;
[0048] (d) The remaining core monomer pre-emulsion is added dropwise to the reactor at 85°C-90°C for 90-180 min. After completion, the mixture is kept at 85-90°C for 30-60 min.
[0049] (e) Preparation of shell monomer pre-emulsion: Add 100 parts of deionized water, 1 part of AR-10 and 1 part of RS-610 to a pre-emulsification tank, stir and mix well, then add 40 parts of methyl methacrylate, 150 parts of isooctyl acrylate, 7 parts of methacrylic acid, 3 parts of THEICTA, 1 part of AMDS and 0.4 parts of KPS, continue stirring for 20-60 minutes to obtain a shell pre-emulsion.
[0050] (f) After the core monomer emulsion is added and the insulation is completed, the prepared shell monomer pre-emulsion is added dropwise to the reactor at 85°C-90°C for 90-180 minutes. After completion, the reactor is kept at 85-90°C for 60-120 minutes.
[0051] (g) Post-treatment: After the insulation is completed, the temperature is lowered to 65°C, TBHP is added first, and the temperature is kept for 20 min, and then NaHSO3 is added and the temperature is kept for 30 min.
[0052] (h) Post-addition: After the insulation is completed, the temperature is lowered to 30°C, and 10 parts of ammonia water, then 1.5 parts of WBA and 5 parts of Kathon are added, and stirred for 10 minutes to obtain a water-based high-gloss industrial paint emulsion.
[0053] Example 2
[0054] (a) Preparation of the bottom solution: Add 300 parts of deionized water, 3 parts of SR-10 and 3 parts of RS-610 into a reactor and stir to obtain a bottom solution.
[0055] (b) Preparation of core monomer pre-emulsion: 150 parts of deionized water, 1.5 parts of SR-10 and 1.5 parts of RS-610 were added to a pre-emulsification tank, and stirred well. Then, 330 parts of styrene, 80 parts of methyl methacrylate, 7 parts of methacrylic acid, 7 parts of acrylic acid, 25 parts of butyl acrylate, 3 parts of THEICTA, 1 part of AMDS and 0.7 parts of NPS were added, and stirring was continued for 20-60 minutes to obtain a core monomer pre-emulsion.
[0056] (c) The reactor in step (a) is heated to 85-90° C., 2 parts of the core monomer pre-emulsion obtained in step (b) are added to the reactor, and 0.7 parts of NPS are added, and the temperature is kept for 10-30 minutes.
[0057] (d) The remaining core monomer pre-emulsion is added dropwise to the reactor at 85°C-90°C for 90-180 min. After completion, the mixture is kept at 85-90°C for 30-60 min.
[0058] (e) Preparation of shell monomer pre-emulsion: Add 150 parts of deionized water, 1.5 parts of SR-10 and 1.5 parts of RS-610 to a pre-emulsification tank, stir and mix well, then add 40 parts of methyl methacrylate, 200 parts of isooctyl acrylate, 11 parts of methacrylic acid, 5 parts of THEICTA, 2 parts of AMDS and 0.7 parts of NPS, continue stirring for 20-60 minutes to obtain a shell pre-emulsion.
[0059] (f) After the core monomer emulsion is added and the insulation is completed, the prepared shell monomer pre-emulsion is added dropwise to the reactor at 85°C-90°C for 90-180 minutes. After completion, the reactor is kept at 85-90°C for 60-120 minutes.
[0060] (g) Post-treatment: After the insulation is completed, the temperature is lowered to 65°C, 0.6 parts of TBHP are added, and the temperature is kept for 20 minutes. Then, 0.6 parts of NaHSO3 are added and the temperature is kept for 30 minutes.
[0061] (h) Post-addition: After the insulation is completed, the temperature is lowered to 30° C., 10 parts of aqueous ammonia are added, and then 2 parts of NXZ and 6 parts of BIT are added and stirred for 10 minutes to obtain a water-based high-gloss industrial paint emulsion.
[0062] Example 3
[0063] (a) Preparation of bottom solution: Add 400 parts of deionized water, 4 parts of LR-10 and 4 parts of RS-610 into a reactor and stir to obtain a bottom solution.
[0064] (b) Preparation of core monomer pre-emulsion: Add 200 parts of deionized water, 2 parts of LR-10 and 2 parts of RS-610 into a pre-emulsification tank, stir and mix well, then add 440 parts of styrene, 100 parts of methyl methacrylate, 10 parts of methacrylic acid, 10 parts of acrylic acid, 50 parts of butyl acrylate, 4 parts of THEICTA, 2 parts of AMDS and 1 part of APS, continue stirring for 20-60 minutes to obtain a core monomer pre-emulsion.
[0065] (c) The reactor in step (a) is heated to 85-90° C., 5 parts of the core monomer pre-emulsion obtained in step (b) are added to the reactor, and 1 part of APS is added, and the temperature is kept for 10-30 minutes.
[0066] (d) The remaining core monomer pre-emulsion is added dropwise to the reactor at 85°C-90°C for 90-180 min. After completion, the mixture is kept at 85-90°C for 30-60 min.
[0067] (e) Preparation of shell monomer pre-emulsion: Add 200 parts of deionized water, 2 parts of LR-10 and 2 parts of RS-610 into a pre-emulsification tank, stir and mix well, then add 60 parts of methyl methacrylate, 300 parts of isooctyl acrylate, 10 parts of methacrylic acid, 6 parts of THEICTA, 2 parts of AMDS and 1 part of APS, continue stirring for 20-60 minutes to obtain a shell pre-emulsion.
[0068] (f) After the core monomer emulsion is added and the insulation is completed, the prepared shell monomer pre-emulsion is added dropwise to the reactor at 85°C-90°C for 90-180 minutes. After completion, the reactor is kept at 85-90°C for 60-120 minutes.
[0069] (g) Post-treatment: After the heat preservation was completed, the temperature was lowered to 65°C, 0.8 parts of LQ-TBCP was added, and the mixture was kept warm for 20 min, and then 0.8 parts of VC was added and the mixture was kept warm for 30 min.
[0070] (h) Post-addition: After the insulation is completed, the temperature is lowered to 30°C, and 15 parts of ammonia water, then 2.5 parts of NXZ and 10 parts of Kathon are added, and stirred for 10 minutes to obtain a water-based high-gloss industrial paint emulsion.
[0071] Example 4
[0072] (a) Preparation of bottom solution: Add 400 parts of deionized water, 4 parts of SR-10 and 4 parts of RE-610 into a reactor and stir to obtain a bottom solution.
[0073] (b) Preparation of core monomer pre-emulsion: Add 200 parts of deionized water, 2 parts of SR-10 and 2 parts of RE-610 into a pre-emulsification tank, stir and mix well, then add 440 parts of styrene, 100 parts of methyl methacrylate, 10 parts of methacrylic acid, 10 parts of acrylic acid, 50 parts of butyl acrylate, 4 parts of THEICTA, 2 parts of AMDS and 1 part of APS, continue stirring for 20-60 minutes to obtain a core monomer pre-emulsion.
[0074] (c) The reactor in step (a) is heated to 85-90° C., 2 parts of the core monomer pre-emulsion obtained in step (b) are added to the reactor, and 1 part of APS is added, and the temperature is kept for 10-30 minutes.
[0075] (d) The remaining core monomer pre-emulsion is added dropwise to the reactor at 85°C-90°C for 90-180 min. After completion, the mixture is kept at 85-90°C for 30-60 min.
[0076] (e) Preparation of shell monomer pre-emulsion: Add 200 parts of deionized water, 2 parts of SR-10 and 2 parts of RE-610 into a pre-emulsification tank, stir and mix well, then add 60 parts of methyl methacrylate, 300 parts of isooctyl acrylate, 10 parts of methacrylic acid, 6 parts of THEICTA, 2 parts of AMDS and 1 part of APS, continue stirring for 20-60 minutes to obtain a shell pre-emulsion.
[0077] (f) After the core monomer emulsion is added and the insulation is completed, the prepared shell monomer pre-emulsion is added dropwise to the reactor at 85°C-90°C for 90-180 minutes. After completion, the reactor is kept at 85-90°C for 60-120 minutes.
[0078] (g) Post-treatment: After the heat preservation was completed, the temperature was lowered to 65°C, 0.8 parts of LQ-TBCP was added, and the mixture was kept warm for 20 min, and then 0.8 parts of VC was added and the mixture was kept warm for 30 min.
[0079] (h) Post-addition: After the heat preservation is completed, the temperature is lowered to 30° C., 15 parts of aqueous ammonia, then 2.5 parts of WBA and 7.5 parts of BIT are added, and the mixture is stirred for 10 minutes to obtain a water-based high-gloss industrial paint emulsion.
[0080] Example 5
[0081] (a) Preparation of the bottom solution: Add 200 parts of deionized water, 2 parts of SR-10 and 2 parts of RS-710 into the reactor and stir to obtain the bottom solution.
[0082] (b) Preparation of core monomer pre-emulsion: Add 100 parts of deionized water, 1 part of SR-10 and 1 part of RS-710 to a pre-emulsification tank, stir and mix well, then add 330 parts of styrene, 90 parts of methyl methacrylate, 8 parts of methacrylic acid, 8 parts of acrylic acid, 25 parts of butyl acrylate, 2 parts of THEICTA, 1 part of AMDS and 0.4 parts of APS, continue stirring for 20-60 minutes to obtain a core monomer pre-emulsion;
[0083] (c) heating the reactor in step (a) to 85-90° C., adding 2 parts of the core monomer pre-emulsion obtained in step (b) to the reactor, and adding 0.4 parts of APS, and keeping the temperature for 10-30 minutes;
[0084] (d) The remaining core monomer pre-emulsion is added dropwise to the reactor at 85°C-90°C for 90-180 min. After completion, the mixture is kept at 85-90°C for 30-60 min.
[0085] (e) Preparation of shell monomer pre-emulsion: Add 100 parts of deionized water, 1 part of SR-10 and 1 part of RS-710 to a pre-emulsification tank, stir and mix well, then add 40 parts of methyl methacrylate, 225 parts of isooctyl acrylate, 6 parts of methacrylic acid, 3 parts of THEICTA, 1 part of AMDS and 0.4 parts of APS, continue stirring for 20-60 minutes to obtain a shell pre-emulsion.
[0086] (f) After the core monomer emulsion is added and the insulation is completed, the prepared shell monomer pre-emulsion is added dropwise to the reactor at 85°C-90°C for 90-180 minutes. After completion, the reactor is kept at 85-90°C for 60-120 minutes.
[0087] (g) Post-treatment: After the insulation is completed, the temperature is lowered to 65°C, 0.51 parts of LQ-TBCP are added, and the temperature is kept for 20 minutes. Then, 0.5 parts of NaHSO3 are added and the temperature is kept for 30 minutes.
[0088] (h) Post-addition: After the insulation is completed, the temperature is lowered to 30°C, and 10 parts of ammonia water, then 1.5 parts of WBA and 5 parts of Kathon are added, and stirred for 10 minutes to obtain a water-based high-gloss industrial paint emulsion.
[0089]
[0090]
[0091]
[0092] SR-10: vinyl polyoxyethylene alkyl sulfide ammonium acid, manufacturer Aidico;
[0093] AR-10: Allyloxy aromatic alcohol oxyethylene ether ammonium sulfate, manufactured by Japan Daiichi Pharmaceutical; LR-10: Fatty alcohol reactive emulsifier, manufactured by Nanjing Qicheng;
[0094] ST: Styrene, manufacturer Shanghai Huayi;
[0095] MMA: methyl methacrylate, manufactured by Shanghai Huayi;
[0096] MAA: methacrylic acid, manufacturer Wanhua Chemical;
[0097] AA: Acrylic acid, manufacturer Wanhua Chemical
[0098] BA: Butyl acrylate, manufacturer: Wanhua Chemical;
[0099] EHA: Isooctyl acrylate, manufactured by Shanghai Huayi;
[0100] KPS: Potassium persulfate, manufacturer Fujian Minglin;
[0101] APS: ammonium persulfate, manufacturer Fujian Minglin;
[0102] NPS: sodium persulfate, manufacturer Fujian Minglin;
[0103] TMP3EOTA: tris(2-hydroxyethyl)isocyanurate triacrylate, manufactured by Sartomer;
[0104] AMDS: α-methylstyrene dimer, manufacturer: Yiyuan New Materials Technology Co., Ltd.;
[0105] TBHP: tert-butyl hydroperoxide, manufacturer: Peixing Chemical Co., Ltd.;
[0106] LQ-TBCP: tert-butyl cumene peroxide, manufacturer: Hand in Hand Chemical Technology Co., Ltd.
[0107] NaHSO3: sodium bisulfite, manufacturer: Zhentai Chemical;
[0108] VC: L-ascorbic acid, manufacturer: Jinfuyuan Biotechnology Co., Ltd.;
[0109] Kason: 1.5 content, manufacturer Hoffman;
[0110] BIT: 5% content, manufacturer Hofmann;
[0111] WBA: mineral oil defoamer, manufacturer BASF;
[0112] NXZ: mineral oil defoamer, manufacturer Nopco;
[0113] Comparative Example 1
[0114] The only difference between Comparative Example 1 and Example 1 is that the raw materials for preparing the aqueous emulsion do not include an internal crosslinking agent, and other conditions are the same as those in Example 1.
[0115] Comparative Example 2
[0116] The difference between this comparative example and Example 1 is that the raw materials for preparing the aqueous emulsion do not include a molecular weight regulating monomer, and other conditions are the same as those in Example 1.
[0117] Comparative Example 3
[0118] A water-based high-gloss industrial paint emulsion prepared according to patent publication CN113429522 A.
[0119] The water-based industrial paint prepared in the embodiment and the comparative example was tested for performance. The gloss was tested according to the method specified in GBT 9754-2007; the adhesion was tested according to the method specified in GB / T 1720-1979, and the score was 0-5. The higher the score, the better the adhesion; the water resistance was tested according to the method specified in GB / T1733-1993; the salt water resistance was tested according to the method specified in GB / T 1763-1979; the salt spray resistance was tested according to the method specified in GB / T 1771-2007; the flexibility was tested according to the method of GB / T 1731-1993, and the score was 1-5. The higher the score, the better the flexibility; the pencil hardness was tested according to the method of GB 6739-86. The test results are shown in Table 1 below:
[0120] Table 1: Test results of embodiments and comparative examples
[0121]
[0122]
[0123] According to Table 1, the water-based industrial paint emulsion provided by the present invention is applied to water-based industrial paint coatings, and the paint film has high hardness, good adhesion to the substrate, good flexibility, good water resistance, salt water resistance and salt spray resistance, and high gloss. The flexibility of the embodiment is significantly improved compared with the comparative example, among which the comprehensive performance of embodiment 3 is the best, the paint film hardness can reach H, the adhesion to the substrate is level 5, the water resistance can reach 360 hours, the salt water resistance and salt spray resistance can reach 180 hours, the 60° gloss can reach 96°, and the flexibility is also good.
[0124] The flexibility of Comparative Examples 1 and 2 is worse than that of the embodiment, but better than that of Comparative Example 3. The hardness, water resistance, salt water resistance and salt spray resistance of Comparative Example 1 are worse than those of the embodiment and Comparative Example 3, and the gloss of Comparative Example 2 is worse than that of the embodiment and Comparative Example 1.
[0125] The above is an exemplary description of the present invention. Obviously, the specific implementation of the present invention is not limited to the above-mentioned method. As long as such non-substantial improvements are made by adopting the method concept and technical solution of the present invention, or the concept and technical solution of the present invention are directly applied to other occasions without improvement, they are all within the protection scope of the present invention.
Claims
1. A method for preparing a water-based high-gloss industrial paint emulsion, characterized in that: The steps include: (a) adding 200-400 parts of deionized water, 2-4 parts of reactive emulsifier and 2-4 parts of phosphate emulsifier into a reactor, stirring and mixing to obtain a bottom solution; (b) adding 100-200 parts of deionized water, 1-2 parts of reactive emulsifier and 1-2 parts of phosphate emulsifier to a pre-emulsification tank, stirring and mixing, and then adding 220-440 parts of styrene, 40-80 parts of methyl methacrylate, 5-10 parts of methacrylic acid, 5-10 parts of acrylic acid, 0-50 parts of butyl acrylate, 1-3 parts of internal crosslinking agent tris(2-hydroxyethyl)isocyanurate triacrylate, 1-2 parts of molecular weight regulator α-methylstyrene dimer and 0.4-1 parts of initiator, and continuing stirring for 20-60 minutes to obtain a core monomer pre-emulsion; (c) heating the reactor in step (a) to 85-90° C., adding 2-5 parts of the core monomer pre-emulsion obtained in step (b) to the reactor, and adding 0.4-1 parts of initiator, and keeping the temperature for 10-30 minutes; (d) adding the remaining core monomer pre-emulsion to the reactor dropwise at 85° C.-90° C. for 90-180 min, and then keeping the temperature at 85-90° C. for 30-60 min. (e) adding 100-200 parts of deionized water, 1-2 parts of reactive emulsifier and 1-2 parts of phosphate emulsifier to another pre-emulsification tank, stirring and mixing, and then adding 40-80 parts of methyl methacrylate, 150-300 parts of isooctyl acrylate, 5-10 parts of methacrylic acid, 4-7 parts of internal crosslinking agent tris(2-hydroxyethyl)isocyanurate triacrylate, 1-2 parts of molecular weight regulator α-methylstyrene dimer and 0.4-1 parts of initiator, and continuing stirring for 20-60 minutes to obtain a shell monomer pre-emulsion; (f) After the core monomer emulsion is added dropwise and the insulation is completed, the prepared shell monomer pre-emulsion is added dropwise to the reactor at 85° C.-90° C. for 90-180 min. After completion, the mixture is kept at 85-90° C. for 60-120 min. (g) After the insulation in step (f), the temperature is lowered to 65-75°C, an oxidant is added and the temperature is maintained for 20-30 minutes, and then a reducing agent is added and the temperature is maintained for 30-60 minutes; (h) After the heat preservation in step (g) is completed, the temperature is lowered to below 50° C., 10-15 parts of a pH regulator, 1.5-2.5 parts of a defoaming agent and 5-10 parts of a fungicide are added, the temperature is kept and stirred for 10-20 minutes to obtain a hard-core soft-shell water-based high-gloss industrial paint emulsion.
2. The method for preparing a water-based high-gloss industrial paint emulsion according to claim 1, characterized in that: The phosphate emulsifier is one or any two of RS-610, RE-610 and RS-710.