A conjugated coordination polymer aerogel material and its preparation method and application
By preparing conjugated coordination polymer aerogel materials with a porous structure, the problem of easy accumulation and agglomeration of conjugated coordination polymer materials is solved, its conductivity and catalytic performance are improved, and its applications in catalysis, adsorption and other fields are expanded. application.
Patent Information
- Application Number
- CN202410030174.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-09
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-01-09
AI Technical Summary
Existing conjugated coordination polymer materials have large particle sizes and are prone to accumulation and agglomeration, resulting in a reduction in the number of active sites, which limits their performance improvement and application expansion.
Using an aerogel material constructed of conjugated organic ligands and metal single atoms, a porous structure of conjugated coordination polymer aerogel is prepared through solvothermal method and solvent exchange method, and carbon dioxide supercritical drying is used to form a large specific surface area. Aerogel materials, improve agglomeration and increase exposure of active sites.
It effectively improves the conductivity and catalytic performance of the conjugated coordination polymer aerogel material, increases the number of active sites and the local concentration of reactants, and improves its application performance in catalysis, adsorption and other fields.
Smart Images

Figure CN117866274B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of conjugated coordination polymer materials, and in particular relates to a conjugated coordination polymer aerogel material and a preparation method and application thereof. Background Art
[0002] As a new type of single-atom catalyst, conjugated coordination polymers have good electronic conductivity and stability. It is a type of material formed by hybridizing the π orbital of a conjugated organic ligand with the d electron orbital of a transition metal. Conjugated coordination polymers have a strong conjugation effect, and their π-d electron coupling promotes the delocalization of their charges, which significantly improves the conductivity of the material. Conjugated coordination polymers have become an important type of functional material due to their advantages such as high atomic utilization and strong atomic structure designability. However, the particle size of the currently developed conjugated coordination polymer materials is large and they tend to agglomerate with each other, which greatly reduces the number of exposed active sites and limits the accessibility of the active sites. Therefore, how to rationally design and accurately synthesize conjugated coordination polymer materials to improve the agglomeration phenomenon and increase the number of exposed active sites is the key to improving their performance.
[0003] Aerogel materials have become a hot topic of research due to their extremely low apparent density, high porosity, and large specific surface area. They exhibit extremely low thermal conductivity and good barrier, adsorption, and catalytic properties in practical applications such as thermal insulation, flame retardancy, sound insulation, and adsorption. Therefore, it is of great significance to realize the preparation of conjugated coordination polymer aerogel materials, which can improve the problem of easy accumulation and agglomeration of currently developed conjugated coordination polymer materials, thereby achieving performance improvement and application expansion. Summary of the invention
[0004] In view of the problems and shortcomings of the prior art, the present invention provides a conjugated coordination polymer aerogel material and a preparation method and application thereof. The preparation conditions are mild and a porous aerogel structure with a large specific surface area can be formed, which effectively improves the problem of easy accumulation and agglomeration of the currently developed conjugated coordination polymer materials. The conjugated coordination polymer aerogel material can fully expose the metal site and use the pore enrichment effect to increase the local reactant concentration on the surface of the metal site, increase the residence time of the reaction intermediate on the surface of the metal site, and thus improve the catalytic performance.
[0005] The first aspect of the present invention is to provide a conjugated coordination polymer aerogel material, which is constructed from metal single atoms and conjugated organic ligands, wherein the metal single atoms include at least one of iron, cobalt, nickel, copper, and zinc, and the conjugated organic ligands include 2,3,6,7,10,11-hexahydroxytriphenyl.
[0006] In one embodiment, the metal single atom content in the conjugated coordination polymer aerogel material is 13.0 wt% to 18.0 wt%.
[0007] In one embodiment, the specific surface area of the conjugated coordination polymer aerogel material is greater than 80 m 2 g -1 .
[0008] The second aspect of the present invention is to provide a method for preparing a conjugated coordination polymer aerogel material, the method comprising the following steps:
[0009] (1) Dissolve the precursor metal salt in water to obtain a concentration of not less than 0.3 mol·L -1 The conjugated organic ligand is dissolved in an organic solvent to obtain a concentration of not less than 0.2 mol·L -1 A conjugated organic ligand solution is prepared, and the metal salt solution and the conjugated organic ligand solution are mixed and heated to prepare a gelled conjugated coordination polymer;
[0010] (2) adding an exchange solvent to the gelled conjugated coordination polymer to perform solvent exchange to obtain a wet gel of the conjugated coordination polymer;
[0011] (3) The conjugated coordination polymer wet gel is subjected to a carbon dioxide supercritical drying treatment to prepare a conjugated coordination polymer aerogel material.
[0012] In one embodiment, the method for preparing the conjugated coordination polymer aerogel material comprises the following steps:
[0013] (1) Dissolve the precursor metal salt in deionized water to obtain a concentration of not less than 0.3 mol·L -1 The precursor metal salt solution is prepared by dissolving the conjugated organic ligand in an organic solvent to obtain a concentration of not less than 0.2 mol·L -1 The precursor metal salt solution and the conjugated organic ligand dispersion are mixed after being fully dissolved, and placed in a blast oven to heat up to prepare a gelled conjugated coordination polymer;
[0014] (2) adding acetone to the gelled conjugated coordination polymer to perform solvent exchange to obtain a conjugated coordination polymer wet gel;
[0015] (3) subjecting the conjugated coordination polymer wet gel to a carbon dioxide supercritical drying treatment to finally prepare a conjugated coordination polymer aerogel material.
[0016] In one implementation case, the molar ratio of the precursor metal salt to the conjugated organic ligand in step (1) is 1 to 2:1, preferably 1.5:1.
[0017] In one embodiment, the metal type of the precursor metal salt in step (1) includes at least one of iron, cobalt, nickel, copper and zinc.
[0018] In one embodiment, the precursor metal salt in step (1) includes at least one of acetate, chloride, sulfate, and nitrate, preferably acetate.
[0019] In one implementation case, the conjugated organic ligand in step (1) is 2,3,6,7,10,11-hexahydroxytriphenyl.
[0020] In one implementation case, the organic solvent in step (1) includes at least one of dimethyl sulfoxide and N,N-dimethylformamide, preferably dimethyl sulfoxide.
[0021] In one implementation case, the temperature of the blast oven in step (1) is 65-80°C, preferably 75°C.
[0022] In one implementation case, the metal salt solution and the conjugated organic ligand solution in step (1) are subjected to ultrasonic dispersion treatment independently, and the ultrasonic dispersion treatment time is 0.5 to 2 hours, preferably 1 hour.
[0023] In one embodiment, the concentration of the precursor metal salt solution in step (1) is 0.3 to 1.2 mol·L -1 .
[0024] In one embodiment, the concentration of the precursor metal salt solution in step (1) is 0.5 to 1.0 mol·L -1 , preferably 0.75 mol·L -1 .
[0025] In one embodiment, the concentration of the conjugated organic ligand dispersion in step (1) is 0.2 to 0.8 mol·L -1 .
[0026] In one embodiment, the concentration of the conjugated organic ligand dispersion in step (1) is 0.3 to 0.6 mol·L -1 , preferably 0.5 mol·L -1 .
[0027] In one implementation case, the heating treatment in step (1) includes a temperature treatment in a blast oven, and the reaction time in the blast oven is 24 to 48 hours, preferably 24 hours.
[0028] In one embodiment, the metal element of the gelled conjugated coordination polymer in step (2) includes at least one of iron, cobalt, nickel, copper and zinc.
[0029] In one embodiment, in step (2), the exchange solvent includes at least one of ethanol, acetone, and isopropanol, preferably acetone.
[0030] In one implementation case, the number of solvent exchanges using the exchange solvent in step (2) is 12 to 20 times, preferably 20 times.
[0031] In one implementation case, the time for solvent exchange using the exchange solvent in step (2) is 3 to 5 days, preferably 4 days.
[0032] In one implementation case, the supercritical drying treatment time of carbon dioxide in step (3) is 8 to 24 hours, preferably 12 hours.
[0033] On the other hand, the present invention provides a conjugated coordination polymer aerogel material prepared by the above method.
[0034] In one implementation case, the metal single atom content in the conjugated coordination polymer aerogel material is 13.0 wt% to 18.0 wt%, and the advantage of the structural designability of the conjugated coordination polymer is retained.
[0035] The inventive principle of the present invention is: the hydroxyl groups of the conjugated organic ligands react with metal ions to obtain conjugated coordination polymer nanoparticles, and at the same time, an induced cross-linking effect is achieved through a high-concentration raw material synthesis strategy to promote sol-gel transition, so that the conjugated coordination polymer nanoparticles are connected to form a wet gel state through non-covalent interactions, and finally a conjugated coordination polymer aerogel material is obtained through supercritical carbon dioxide drying treatment.
[0036] On the other hand, the present invention also provides an application of the above-mentioned preparation method or an application of a conjugated coordination polymer aerogel material, including applications in catalysis, adsorption, sensing, electrochemical energy storage, electromagnetic shielding and wave absorption.
[0037] Compared with the prior art, the present invention has the following beneficial effects:
[0038] 1. The conjugated coordination polymer aerogel material prepared by the present invention can fully utilize the π-d electronic coupling of the conjugated coordination polymer to promote the delocalization of charges, and the conjugated coordination polymer aerogel material finally prepared has good electrical conductivity.
[0039] 2. The conjugated coordination polymer aerogel material synthesized by the present invention has the advantages of large specific surface area and a large number of exposed active sites, which effectively improves the shortcomings of the current conjugated coordination polymer material that is easy to accumulate and agglomerate. This design can achieve the performance improvement of the material. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 These are scanning electron microscope photos of the nickel-based conjugated coordination polymer aerogel material of Example 1 and the nickel-based conjugated coordination polymer material of Comparative Example 1.
[0041] Figure 2 It is the X-ray diffraction pattern of the nickel-based conjugated coordination polymer aerogel material in Example 1 and the structural formula of the nickel-based conjugated coordination polymer aerogel material in Example 1.
[0042] Figure 3 The graphs are nitrogen isothermal adsorption-desorption curves of the nickel-based conjugated coordination polymer aerogel material of Example 1 and the nickel-based conjugated coordination polymer material of Comparative Example 1.
[0043] Figure 4 This is the X-ray photoelectron spectrum of the nickel-based conjugated coordination polymer aerogel material of Example 1.
[0044] Figure 5 This is the X-ray absorption spectrum of the nickel-based conjugated coordination polymer aerogel material of Example 1.
[0045] Figure 6 The linear sweep voltammetry curves of the nickel-based conjugated coordination polymer aerogel material of Example 1 and the nickel-based conjugated coordination polymer material of Comparative Example 1 are shown. DETAILED DESCRIPTION
[0046] The present invention provides a conjugated coordination polymer aerogel material and a preparation method and application thereof. First, a precursor metal salt and a conjugated organic ligand are prepared by a solvothermal method and a solvent exchange method to obtain a conjugated coordination polymer wet gel, and then the wet gel is dried by supercritical carbon dioxide to obtain a conjugated coordination polymer aerogel material. The conjugated coordination polymer aerogel material prepared by the present invention has the advantages of a wide source of synthetic raw materials, high metal single atom density, strong molecular structure designability, high specific surface area, etc. In addition, the preparation process is simple and easy to operate, and the obtained conjugated coordination polymer aerogel material has good performance and an extremely wide range of applications.
[0047] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0048] Unless otherwise specified, the sources of the reagents used in the embodiments of the present invention can be purchased from the market.
[0049] The present invention provides a characterization test result diagram of Example 1, and other embodiments all adopt the same characterization test method. Those skilled in the art can directly and unambiguously determine the content of the embodiments of the present invention through the characterization test method provided by the present invention.
[0050] Example 1: Preparation of nickel-based conjugated coordination polymer aerogel material
[0051] (1) Using a balance, 187 mg (0.75 mmol) of nickel acetate tetrahydrate was weighed and dissolved in 1.0 mL of deionized water. 162 mg (0.50 mmol) of conjugated organic ligand 2,3,6,7,10,11-hexahydroxytriphenyl was weighed and dissolved in 1.0 mL of dimethyl sulfoxide. The mixture was dispersed by ultrasonic for 1 h. After being fully dissolved, the mixture was mixed in a glass bottle and placed in a 75° C. forced air oven for 24 h to obtain a gelled nickel-based conjugated coordination polymer.
[0052] (2) Add 4 mL of acetone to the obtained gelled nickel-based conjugated coordination polymer, remove the upper clear liquid after 4 hours, and repeat the above solvent exchange step 20 times to obtain a nickel-based conjugated coordination polymer wet gel.
[0053] (3) The nickel-based conjugated coordination polymer wet gel is subjected to a carbon dioxide supercritical drying treatment for 12 hours, and the final product is a nickel-based conjugated coordination polymer aerogel material.
[0054] Example 2: Preparation of iron-based conjugated coordination polymer aerogel material
[0055] (1) Using a balance, 143 mg (0.75 mmol) of ferric acetate was weighed and dissolved in 1.0 mL of deionized water. 162 mg (0.50 mmol) of conjugated organic ligand 2,3,6,7,10,11-hexahydroxytriphenyl was weighed and dissolved in 1.0 mL of dimethyl sulfoxide. The mixture was dispersed by ultrasonic for 1 h. After being fully dissolved, the mixture was mixed in a glass bottle and placed in a 75° C. forced air oven for 24 h to obtain a gelled iron-based conjugated coordination polymer.
[0056] (2) Add 4 mL of acetone to the obtained gelled iron-based conjugated coordination polymer, remove the upper clear liquid after 4 hours, and repeat the above solvent exchange step 20 times to obtain an iron-based conjugated coordination polymer wet gel.
[0057] (3) The iron-based conjugated coordination polymer wet gel is subjected to a carbon dioxide supercritical drying treatment for 12 hours, and the final product is an iron-based conjugated coordination polymer aerogel material.
[0058] Example 3: Preparation of cobalt-based conjugated coordination polymer aerogel material
[0059] (1) Using a balance, 187 mg (0.75 mmol) of cobalt acetate tetrahydrate was weighed and dissolved in 1.0 mL of deionized water. 162 mg (0.50 mmol) of conjugated organic ligand 2,3,6,7,10,11-hexahydroxytriphenyl was weighed and dissolved in 1.0 mL of dimethyl sulfoxide. The mixture was dispersed by ultrasonic for 1 h. After being fully dissolved, the mixture was mixed in a glass bottle and placed in a 75° C. forced air oven for 24 h to obtain a gelled cobalt-based conjugated coordination polymer.
[0060] (2) Add 4 mL of acetone to the obtained gelled cobalt-based conjugated coordination polymer, remove the upper clear liquid after 4 hours, and repeat the above solvent exchange step 20 times to obtain a cobalt-based conjugated coordination polymer wet gel.
[0061] (3) The cobalt-based conjugated coordination polymer wet gel is subjected to a carbon dioxide supercritical drying treatment for 12 hours, and the final product is a cobalt-based conjugated coordination polymer aerogel material.
[0062] Comparative Example 1: Preparation of nickel-based conjugated coordination polymer materials
[0063] (1) Using a balance, 15 mg (0.06 mmol) of nickel acetate tetrahydrate was weighed and dissolved in 2.0 mL of deionized water. 13 mg (0.04 mmol) of conjugated organic ligand 2,3,6,7,10,11-hexahydroxytriphenyl was weighed and dissolved in 2.0 mL of dimethyl sulfoxide. The mixture was dispersed by ultrasonic for 1 h. After being fully dissolved, the mixture was mixed in a glass bottle and placed in a 75° C. forced air oven for 24 h to obtain a nickel-based conjugated coordination polymer.
[0064] (2) Add 4 mL of acetone to the obtained nickel-based conjugated coordination polymer, remove the upper clear liquid after 4 hours, and repeat the above solvent exchange step 20 times.
[0065] (3) The material after solvent exchange is subjected to carbon dioxide supercritical drying treatment for 12 hours, and the final product is a nickel-based conjugated coordination polymer material.
[0066] Test example: Performance test of nickel-based conjugated coordination polymer aerogel materials
[0067] This test example conducts relevant performance tests on the nickel-based conjugated coordination polymer aerogel material prepared by high-concentration raw materials in Example 1 and the nickel-based conjugated coordination polymer material prepared by low-concentration raw materials in Comparative Example 1, mainly including scanning electron microscope test, X-ray diffraction spectrum test, nitrogen isothermal adsorption and desorption test, X-ray photoelectron energy spectrum test, X-ray absorption spectrum test and electrocatalytic oxygen evolution performance test, and the results are as follows:
[0068] like Figure 1Shown are scanning electron microscope photographs of the nickel-based conjugated coordination polymer aerogel material of Example 1 and the nickel-based conjugated coordination polymer material of Comparative Example 1. It can be observed that the agglomeration phenomenon of the nickel-based conjugated coordination polymer material of Comparative Example 1 is more obvious. In contrast, the nickel-based conjugated coordination polymer aerogel material of Example 1 is basically free of agglomeration, and the nickel-based conjugated coordination polymer aerogel material has a porous morphology as a whole.
[0069] like Figure 2 a shows the X-ray diffraction spectrum of the nickel-based conjugated coordination polymer aerogel material of Example 1. The spectrum has characteristic peaks at 2θ=4.7°, 9.3°, 14.1°16.3° and 27.1°, corresponding to the (010), (020), (030), (220) and (002) crystal planes, respectively. Through these characteristic peaks, it can be determined that the nickel-based conjugated coordination polymer aerogel material of Example 1 was successfully synthesized. Its compound structure is as follows Figure 2 b. However, the nickel-based conjugated coordination polymer material prepared by using low-concentration raw materials in Comparative Example 1 did not have such a result. Combined with the above-mentioned scanning electron microscope results, it is shown that only under high-concentration conditions can a conjugated coordination polymer aerogel material with a porous structure be formed, which improves the problems of the currently developed conjugated coordination polymer materials, such as large particle size, mutual accumulation and agglomeration, and a small number of exposed metal sites.
[0070] like Figure 3 The graphs show the nitrogen isothermal adsorption and desorption curves of the nickel-based conjugated coordination polymer aerogel material of Example 1 and the nickel-based conjugated coordination polymer material of Comparative Example 1. The specific surface area of the nickel-based conjugated coordination polymer aerogel material of Example 1 is 118.9 m 2 g -1 The specific surface area of the nickel-based conjugated coordination polymer material in Comparative Example 1 is 60.8 m 2 g -1 This indicates that the nickel-based conjugated coordination polymer aerogel material of Example 1 can expose more active sites than the nickel-based conjugated coordination polymer material of Comparative Example 1.
[0071] like Figure 4 The figure shows the X-ray photoelectron spectrum of the nickel-based conjugated coordination polymer aerogel material of Example 1, and it can be seen that the nickel-based conjugated coordination polymer aerogel material contains oxygen and nickel elements.
[0072] like Figure 5The X-ray absorption spectrum of the nickel-based conjugated coordination polymer aerogel material of Example 1 is shown. An obvious nickel-oxygen peak can be observed, and no nickel-nickel peak is observed, confirming that the metal components in the prepared nickel-based conjugated coordination polymer aerogel material are all nickel single atoms. In addition, as shown in Table 1, the test results of the inductively coupled plasma emission spectrometer for the nickel-based conjugated coordination polymer aerogel material show that the nickel single atom content is about 13.9%.
[0073] Table 1. Test results of inductively coupled plasma emission spectrometer for nickel-based conjugated coordination polymer aerogel materials
[0074]
[0075] like Figure 6 The figure shows the linear sweep voltammetry curves of the nickel-based conjugated coordination polymer aerogel material of Example 1 and the nickel-based conjugated coordination polymer material of Comparative Example 1 in 1M KOH electrolyte. It can be seen from the figure that the nickel-based conjugated coordination polymer aerogel material of Example 1 has a linear sweep voltammetry curve in 100mA cm -2 The overpotential at the current density is 432 mV, while the nickel-based conjugated coordination polymer material of comparative example 1 is -2 The overpotential at the current density is 552 mV. This shows that the electrocatalytic oxygen evolution performance of the nickel-based conjugated coordination polymer aerogel material of Example 1 is better than that of the nickel-based conjugated coordination polymer material of Comparative Example 1.
[0076] The above-mentioned embodiments only express several implementation methods of the present invention, and the description is relatively specific and detailed, but it cannot be understood as limiting the scope of the invention patent. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention.
Claims
1. A conjugated coordination polymer aerogel material, characterized in that: The conjugated coordination polymer aerogel material is constructed of metal single atoms and conjugated organic ligands, wherein the metal single atoms include at least one of iron, cobalt, nickel, copper and zinc, and the content of the metal single atoms is 13.0wt% to 18.0wt%; the conjugated organic ligands include 2,3,6,7,10,11-hexahydroxytriphenyl; The preparation method of the conjugated coordination polymer aerogel material comprises the following steps: (1) Dissolve the precursor metal salt in water to a concentration of 0.3~1.2 mol·L -1 The conjugated organic ligand is dissolved in an organic solvent to a concentration of 0.2~0.8 mol·L -1 The conjugated organic ligand solution is prepared by mixing the metal salt solution and the conjugated organic ligand solution, wherein the molar ratio of the precursor metal salt to the conjugated organic ligand is 1 to 2:1, and heating the mixture to obtain a gelled conjugated coordination polymer; (2) adding an exchange solvent to the gelled conjugated coordination polymer to perform solvent exchange to obtain a wet gel of the conjugated coordination polymer; (3) The conjugated coordination polymer wet gel is subjected to a carbon dioxide supercritical drying treatment to prepare a conjugated coordination polymer aerogel material.
2. The conjugated coordination polymer aerogel material according to claim 1, characterized in that: The specific surface area of the conjugated coordination polymer aerogel material is greater than 80 m 2 g -1 .
3. The conjugated coordination polymer aerogel material according to claim 1, characterized in that: In the step (1), the molar ratio of the precursor metal salt to the conjugated organic ligand is 1.5:
1.
4. The conjugated coordination polymer aerogel material according to claim 1, characterized in that: The precursor metal salt in step (1) includes at least one of acetate, chloride, sulfate and nitrate.
5. The conjugated coordination polymer aerogel material according to claim 1, characterized in that: The conjugated organic ligand in step (1) is 2,3,6,7,10,11-hexahydroxytriphenyl.
6. The conjugated coordination polymer aerogel material according to claim 1, characterized in that: The organic solvent in step (1) includes at least one of dimethyl sulfoxide and N,N-dimethylformamide.
7. The conjugated coordination polymer aerogel material according to claim 1, characterized in that: In the step (1), the metal salt solution and the conjugated organic ligand solution are subjected to ultrasonic dispersion treatment for 0.5 to 2 h respectively.
8. The conjugated coordination polymer aerogel material according to claim 7, characterized in that: In the step (1), the metal salt solution and the conjugated organic ligand solution are subjected to ultrasonic dispersion treatment for 1 h respectively.
9. The conjugated coordination polymer aerogel material according to claim 1, characterized in that: The heating treatment in step (1) includes a blast oven heating treatment at a temperature of 65-80°C and a reaction time of 24-48 hours.
10. The conjugated coordination polymer aerogel material according to claim 1, characterized in that: In step (1), the concentration of the precursor metal salt solution is 0.5-1.0 mol·L -1 .
11. The conjugated coordination polymer aerogel material according to claim 10, characterized in that: In step (1), the concentration of the precursor metal salt solution is 0.75 mol·L -1 .
12. The conjugated coordination polymer aerogel material according to claim 1, characterized in that: In the step (1), the concentration of the conjugated organic ligand dispersion is 0.3-0.6 mol·L -1 .
13. The conjugated coordination polymer aerogel material according to claim 12, characterized in that: In the step (1), the concentration of the conjugated organic ligand dispersion is 0.5 mol·L -1 .
14. The conjugated coordination polymer aerogel material according to claim 1, characterized in that: In the step (2), the exchange solvent includes at least one of ethanol, acetone, and isopropanol.
15. The conjugated coordination polymer aerogel material according to claim 1, characterized in that: In the step (2), the number of times of solvent exchange using acetone is 12 to 20 times.
16. The conjugated coordination polymer aerogel material according to claim 1, characterized in that: The supercritical carbon dioxide drying treatment time in step (3) is 8 to 24 hours.
17. Use of the conjugated coordination polymer aerogel material according to any one of claims 1 to 16, including applications in catalysis, adsorption, sensing, electrochemical energy storage, electromagnetic shielding and wave absorption.